Hydrogen sulfide removal adsorbent and preparation method thereof

By anchoring the combined materials of metal oxide nanoparticles in the MFI molecular sieve, the problems of low utilization rate and sintering of zinc oxide adsorbents are solved, and efficient hydrogen sulfide removal and high-temperature regeneration resistance are achieved.

CN116440856BActive Publication Date: 2024-11-22TSINGHUA UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310097664.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-19
Publication Date
2024-11-22
Estimated Expiration
2043-01-19

AI Technical Summary

Technical Problem

The existing zinc oxide adsorbents are low in the industry and are difficult to regenerate, and are prone to sintering during high-temperature regeneration, resulting in a desulfurization performance.

Method used

Using a combination of MFI molecular sieve and metal oxide nanoparticles, metal oxide nanoparticles are anchored in the pores of MFI molecular sieve through van der Waals force and electrostatic interaction to avoid aggregation and sintering, and at the same time, the nanoparticles are isolated by using a multi-channel structure. Maintain high desulfurization activity.

Benefits of technology

The high dispersion of metal oxide nanoparticles is achieved, high desulfurization activity at low temperatures, and sintering is avoided during the low temperature regeneration process, which improves the recycling rate and stability of the adsorbent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116440856B_ABST
    Figure CN116440856B_ABST
Patent Text Reader

Abstract

The invention discloses a hydrogen sulfide removal adsorbent and a preparation method thereof. The hydrogen sulfide removal adsorbent comprises an MFI type molecular sieve and metal oxide nanoparticles, wherein the metal oxide nanoparticles are distributed in the pores of the MFI type molecular sieve. The metal oxide nanoparticles of the hydrogen sulfide removal adsorbent are highly dispersed, the diffusion resistance of hydrogen sulfide in the metal oxide nanoparticle crystal is small, the desulfurization activity is still high under low temperature and low concentration difference driving force, and the sintering of the metal oxide nanoparticles during high temperature regeneration can be effectively avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrogen sulfide removal, and particularly relates to a hydrogen sulfide removal adsorbent and a preparation method thereof. Background Art

[0002] Hydrogen sulfide is a highly toxic, flammable, corrosive, weakly acidic gas. The emission of hydrogen sulfide not only damages the environment, but also causes great harm to the human body. In industry, the presence of hydrogen sulfide can lead to problems such as equipment corrosion and catalyst poisoning. Therefore, the removal of hydrogen sulfide is one of the main problems faced by industries such as natural gas and petrochemicals. With the development of society, industrial processes have put forward higher and higher requirements for the removal of hydrogen sulfide. For example, the concentration of hydrogen sulfide in the process of synthetic ammonia should be lower than 1ppm, the concentration of hydrogen sulfide in processes such as methanol synthesis and Fischer-Tropsch synthesis should be lower than 0.1ppm, and the concentration of hydrogen sulfide in fuel cells should be as low as 0.004ppm. Therefore, it is of great significance to develop efficient and deep removal technology for hydrogen sulfide. Among different desulfurization technologies, metal oxide adsorption desulfurization has attracted much attention due to its high desulfurization selectivity and simple process flow.

[0003] Among different types of metal oxides, zinc oxide is widely used in industrial desulfurization due to its advantages such as high desulfurization accuracy, stable sulfide, and large equilibrium constant. However, problems such as low utilization rate and difficult regeneration of zinc oxide are the main bottlenecks restricting the further promotion of the desulfurization adsorbent process. This is because the adsorbents used in industry are mostly large-grained zinc oxide. Due to the existence of intracrystalline diffusion resistance and the formation of a dense layer of zinc sulfide, the utilization rate of zinc oxide particles is low. In addition, the regeneration of the adsorbent requires a high temperature of more than 500°C, and the high temperature process will cause the sintering of zinc oxide, reducing its desulfurization performance during recycling. In view of this, how to reduce the size of zinc oxide particles while inhibiting their sintering in the high-temperature regeneration link is a key issue in the development of desulfurization adsorbents. Summary of the invention

[0004] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, one object of the present invention is to provide a hydrogen sulfide removal adsorbent and a preparation method thereof. The metal oxide nanoparticles of the hydrogen sulfide removal adsorbent are highly dispersed, the diffusion resistance of hydrogen sulfide in the metal oxide nanoparticle crystal is small, the desulfurization activity is still high under low temperature and low concentration difference driving force, and the sintering of the metal oxide nanoparticles during high temperature regeneration can be effectively avoided.

[0005] In one aspect of the present invention, the present invention provides a hydrogen sulfide removal adsorbent. According to an embodiment of the present invention, the hydrogen sulfide removal adsorbent comprises an MFI type molecular sieve and metal oxide nanoparticles, wherein the metal oxide nanoparticles are distributed in the pores of the MFI type molecular sieve.

[0006] The hydrogen sulfide removal adsorbent according to the above embodiment of the present invention includes an MFI molecular sieve and metal oxide nanoparticles, wherein the metal oxide nanoparticles are distributed in the pores of the MFI molecular sieve. Specifically, the pores of the MFI molecular sieve have silanol nest sites, and the metal oxide nanoparticles are anchored in the pores of the MFI molecular sieve through van der Waals forces, electrostatic interactions, etc., and at the same time, the silanol nest sites in the pores of the MFI molecular sieve are abundant and evenly distributed, so that the metal oxide nanoparticles can be highly dispersed in the pores, thereby effectively reducing the diffusion resistance of hydrogen sulfide in the metal oxide nanoparticle crystals, so that the metal oxide nanoparticles still maintain high desulfurization activity under low temperature and low concentration driving force. On the other hand, due to the multi-porous skeleton structure of the MFI molecular sieve, the metal oxide nanoparticles are highly dispersed and isolated, which effectively prevents the aggregation of the metal oxide nanoparticles, thereby avoiding the sintering of the metal oxide nanoparticles during high-temperature regeneration. Therefore, the metal oxide nanoparticles of the hydrogen sulfide removal adsorbent are highly dispersed, the diffusion resistance of hydrogen sulfide in the metal oxide nanoparticle crystals is small, and high desulfurization activity is still maintained under low temperature and low concentration difference driving force, and the sintering of the metal oxide nanoparticles during high temperature regeneration can be effectively avoided.

[0007] In addition, the hydrogen sulfide removal adsorbent according to the above embodiment of the present invention may also have the following technical features:

[0008] In some embodiments of the present invention, the MFI molecular sieve comprises at least one of a solid straight hexagonal prism MFI molecular sieve and a hollow straight hexagonal prism MFI molecular sieve. Thus, the adsorbent can have excellent desulfurization activity and effectively avoid sintering of metal oxide nanoparticles.

[0009] In some embodiments of the present invention, the length of the main diagonal line of the hexagon in the straight hexagonal prism of the MFI molecular sieve is 0.05 μm to 10 μm. Thus, the adsorbent can have excellent desulfurization activity and effectively avoid sintering of metal oxide nanoparticles.

[0010] In some embodiments of the present invention, the thickness of the solid straight hexagonal prism-shaped MFI molecular sieve is 30 nm to 1000 nm. Thus, the adsorbent can have excellent desulfurization activity and effectively avoid sintering of metal oxide nanoparticles.

[0011] In some embodiments of the present invention, the shell thickness of the straight hexagonal prism of the MFI molecular sieve with the hollow straight hexagonal prism morphology is 10 nm to 80 nm. Thus, the adsorbent can have excellent desulfurization activity and effectively avoid sintering of metal oxide nanoparticles.

[0012] In some embodiments of the present invention, the metal oxide nanoparticles include at least one of zinc oxide and manganese oxide. Thus, the adsorbent can have excellent desulfurization activity.

[0013] In some embodiments of the present invention, the metal oxide nanoparticles include zinc oxide and manganese oxide, and the molar ratio of manganese in the manganese oxide to zinc in the zinc oxide is not greater than 1. Thus, the adsorbent can have excellent desulfurization activity.

[0014] In some embodiments of the present invention, the average particle size of the metal oxide nanoparticles is 0.5 nm to 5 nm. Thus, the adsorbent can have excellent desulfurization activity.

[0015] In some embodiments of the present invention, based on the total mass of the adsorbent, the content of the MFI molecular sieve is 80 wt% to 99.5 wt%, and the content of the metal oxide nanoparticles is 0.5 wt% to 20 wt%, thereby enabling the adsorbent to have excellent desulfurization activity.

[0016] In another aspect of the present invention, a method for preparing the above-mentioned hydrogen sulfide removal adsorbent is provided. According to an embodiment of the present invention, the method comprises: mixing a metal salt solution and an MFI molecular sieve, impregnating the mixture, drying the mixture, and then calcining the mixture to obtain the hydrogen sulfide removal adsorbent.

[0017] According to the method for preparing the hydrogen sulfide removal adsorbent of the present invention, the metal salt solution and the MFI type molecular sieve are mixed and impregnated, dried, and then calcined. The metal salt solution and the MFI type molecular sieve are mixed and impregnated to allow the metal ions to interact with the hydroxyl defects in the molecular sieve, and then dried to remove excess water. Finally, the dried product is calcined in an air atmosphere to burn off inactive components such as nitrates, and metal oxide nanoclusters are obtained at the same time. Thus, the method can be used to prepare a hydrogen sulfide removal adsorbent having excellent desulfurization activity and effectively avoiding sintering of metal oxide nanoparticles.

[0018] In addition, the method for preparing a hydrogen sulfide removal adsorbent according to the above embodiment of the present invention may also have the following technical features:

[0019] In some embodiments of the present invention, the metal salt solution includes at least one of zinc nitrate, zinc sulfate, zinc chloride, manganese chloride, manganese nitrate, manganese acetate, manganese sulfate, zinc nitrate hexahydrate, zinc sulfate heptahydrate, manganese chloride tetrahydrate, hydrated manganese nitrate, manganese nitrate hexahydrate, manganese acetate dihydrate, manganese acetate tetrahydrate, hydrated manganese sulfate, manganese sulfate tetrahydrate, manganese sulfate pentahydrate and manganese sulfate heptahydrate. Thus, an adsorbent with excellent desulfurization activity can be prepared.

[0020] In some embodiments of the present invention, the concentration of the metal salt solution is 0.1 mol / L to 2.0 mol / L. Thus, an adsorbent with excellent desulfurization activity can be prepared.

[0021] In some embodiments of the present invention, the solvent of the metal salt solution is water.

[0022] In some embodiments of the present invention, the immersion time is 2 hours to 72 hours, and the immersion temperature is 20° C. to 50° C. Thus, an adsorbent with excellent desulfurization activity can be prepared.

[0023] In some embodiments of the present invention, the drying temperature is 70° C. to 150° C., and the drying time is 2 h to 24 h. Thus, an adsorbent with excellent desulfurization activity can be prepared.

[0024] In some embodiments of the present invention, it is characterized in that the calcination temperature is 350° C. to 500° C. and the calcination time is 2 h to 12 h. Thus, an adsorbent with excellent desulfurization activity can be prepared.

[0025] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0027] Figure 1 This is a high-resolution transmission electron microscopy image of 5% ZnO@Silicalite-1 of Example 1 of the present invention;

[0028] Figure 2 It is a desulfurization breakthrough curve diagram of 2% ZnO@Silicalite-1 of Example 5 of the present invention. DETAILED DESCRIPTION

[0029] The embodiments of the present invention are described in detail below, which are intended to explain the present invention but are not to be construed as limiting the present invention.

[0030] In one aspect of the present invention, the present invention provides a hydrogen sulfide removal adsorbent. According to an embodiment of the present invention, the hydrogen sulfide removal adsorbent comprises an MFI type molecular sieve and metal oxide nanoparticles, wherein the metal oxide nanoparticles are distributed in the pores of the MFI type molecular sieve.

[0031] The hydrogen sulfide removal adsorbent according to the above embodiment of the present invention includes an MFI molecular sieve and metal oxide nanoparticles, wherein the metal oxide nanoparticles are distributed in the pores of the MFI molecular sieve. Specifically, the pores of the MFI molecular sieve have silanol nest sites, and the metal oxide nanoparticles are anchored in the pores of the MFI molecular sieve through van der Waals forces, electrostatic interactions, etc., and at the same time, the silanol nest sites in the pores of the MFI molecular sieve are abundant and evenly distributed, so that the metal oxide nanoparticles can be highly dispersed in the pores, thereby effectively reducing the diffusion resistance of hydrogen sulfide in the metal oxide nanoparticle crystals, so that the metal oxide nanoparticles still maintain high desulfurization activity under low temperature and low concentration driving force. On the other hand, due to the multi-porous skeleton structure of the MFI molecular sieve, the metal oxide nanoparticles are highly dispersed and isolated, which effectively prevents the aggregation of the metal oxide nanoparticles, thereby avoiding the sintering of the metal oxide nanoparticles during high-temperature regeneration. Therefore, the metal oxide nanoparticles of the hydrogen sulfide removal adsorbent are highly dispersed, the diffusion resistance of hydrogen sulfide in the metal oxide nanoparticle crystals is small, and high desulfurization activity is still maintained under low temperature and low concentration difference driving force, and the sintering of the metal oxide nanoparticles during high temperature regeneration can be effectively avoided.

[0032] It should be noted that the MFI type molecular sieve includes at least one of a solid straight hexagonal prism MFI type molecular sieve and a hollow straight hexagonal prism MFI type molecular sieve; the metal oxide nanoparticles include at least one of zinc oxide and manganese oxide.

[0033] According to an embodiment of the present invention, the length of the main diagonal of the hexagon in the straight hexagonal prism of the MFI type molecular sieve is 0.05 μm to 10 μm. The inventors found that if the length of the main diagonal of the hexagon in the straight hexagonal prism of the MFI type molecular sieve is too large, the volume of the corresponding molecular sieve becomes larger, which is not conducive to the implementation of the impregnation process. Therefore, the present application adopts an MFI type molecular sieve with a main diagonal length of the hexagon in the straight hexagonal prism of 0.05 μm to 10 μm, which can make the adsorbent have excellent desulfurization activity and effectively avoid the sintering of metal oxide nanoparticles.

[0034] According to an embodiment of the present invention, the thickness of the MFI type molecular sieve with a solid straight hexagonal prism morphology is 30nm to 1000nm. The inventors found that the thickness of the MFI type molecular sieve with a solid straight hexagonal prism morphology cannot be too large, otherwise it will cause serious intracrystalline diffusion of the molecular sieve. Therefore, the present application adopts a MFI type molecular sieve with a solid straight hexagonal prism morphology with a thickness of 30nm to 1000nm, which can make the adsorbent have excellent desulfurization activity and effectively avoid the sintering of metal oxide nanoparticles.

[0035] According to an embodiment of the present invention, the shell thickness of the straight hexagonal prism of the MFI type molecular sieve with a hollow straight hexagonal prism morphology is 10nm to 80nm. The inventor found that if the shell thickness of the straight hexagonal prism of the MFI type molecular sieve with a hollow straight hexagonal prism morphology is too small, it cannot play its carrier role well, making the loading amount too low or even difficult to load, and the shell thickness of the straight hexagonal prism of the MFI type molecular sieve with a hollow straight hexagonal prism morphology is too large, which leads to the aggravation of the intracrystalline diffusion of hydrogen sulfide molecules inside it. Thus, the present application adopts a hollow straight hexagonal prism morphology MFI type molecular sieve with a shell thickness of 10nm to 80nm, which can make the adsorbent have excellent desulfurization activity and effectively avoid the sintering of metal oxide nanoparticles.

[0036] According to an embodiment of the present invention, the metal oxide nanoparticles include zinc oxide and manganese oxide, and the molar ratio of manganese in manganese oxide to zinc in zinc oxide is not greater than 1. The inventors found that the desulfurization rate of manganese oxide is faster than that of zinc oxide, but if the ideal desulfurization depth (ppb level) is achieved, the required desulfurization temperature is relatively high, while zinc oxide can reach the desulfurization depth at 150 degrees Celsius. Therefore, the adsorbent with zinc oxide as the main active substance and manganese oxide as an auxiliary agent can enable the obtained adsorbent to achieve the effect of deep desulfurization at a higher desulfurization rate at a lower temperature. Therefore, the present application uses metal oxide nanoparticles in which the molar ratio of manganese in manganese oxide to zinc in zinc oxide is not greater than 1, which can enable the adsorbent to have excellent desulfurization activity at a lower temperature.

[0037] According to an embodiment of the present invention, the average particle size of the metal oxide nanoparticles is 0.5nm to 5nm. The inventors have found that if the average particle size of the metal oxide nanoparticles is too small, the metal species are mostly present in the form of ions rather than oxides, and the desulfurization activity is insufficient; if the average particle size of the metal oxide nanoparticles is too large, the intracrystalline diffusion of hydrogen sulfide on the metal oxide is aggravated, thereby affecting its desulfurization kinetics and utilization rate. Therefore, the present application uses metal oxide nanoparticles with an average particle size of 0.5nm to 5nm, which can make the adsorbent have excellent desulfurization activity.

[0038] According to an embodiment of the present invention, based on the total mass of the adsorbent, the content of the MFI type molecular sieve is 80wt% to 99.5wt%, and the content of the metal oxide nanoparticles is 0.5wt% to 20wt%. The inventors found that if the content of the metal oxide nanoparticles is too little based on the total mass of the adsorbent, the sulfur capacity of the adsorbent is too low; if the content of the metal oxide nanoparticles is too much, large metal oxide particles will be generated on the surface of the molecular sieve, and the large surface particles are prone to sintering during the desulfurization and circulation process. Therefore, the present application adopts the above-mentioned MFI type molecular sieve and the adsorbent with the content of metal oxide nanoparticles, which can make the adsorbent have excellent desulfurization activity.

[0039] In another aspect of the present invention, a method for preparing the above-mentioned hydrogen sulfide removal adsorbent is provided. According to an embodiment of the present invention, the method comprises: mixing a metal salt solution and an MFI molecular sieve, impregnating the mixture, drying the mixture, and then calcining the mixture to obtain the hydrogen sulfide removal adsorbent.

[0040] According to the method for preparing the hydrogen sulfide removal adsorbent of the present invention, the metal salt solution and the MFI type molecular sieve are mixed and impregnated, dried, and then calcined. The metal ions interact with the hydroxyl defects in the molecular sieve by mixing the metal salt solution and the MFI type molecular sieve, and then dried to remove excess water. Finally, the dried product is calcined in an air atmosphere to burn inactive components and obtain metal oxide nanoclusters. Thus, the method can be used to prepare a hydrogen sulfide removal adsorbent having excellent desulfurization activity and effectively avoiding sintering of metal oxide nanoparticles.

[0041] It should be noted that the metal salt solution is a conventional reagent in the art, and those skilled in the art can select it according to actual conditions. For example, the metal salt solution includes at least one of zinc nitrate, zinc sulfate, zinc chloride, manganese chloride, manganese nitrate, manganese acetate, manganese sulfate, zinc nitrate hexahydrate, zinc sulfate heptahydrate, manganese chloride tetrahydrate, hydrated manganese nitrate, manganese nitrate hexahydrate, manganese acetate dihydrate, manganese acetate tetrahydrate, hydrated manganese sulfate, manganese sulfate tetrahydrate, manganese sulfate pentahydrate and manganese sulfate heptahydrate. Further, the solvent of the metal salt solution is water. According to an embodiment of the present invention, the concentration of the metal salt solution is 0.1mol / L to 2.0mol / L. The inventors have found that the use of a metal salt solution with a concentration of 0.1mol / L to 2.0mol / L can make the impregnation more uniform.

[0042] According to an embodiment of the present invention, the impregnation time is 2h to 72h, and the impregnation temperature is 20°C to 50°C. The inventors found that if the impregnation time is too short or the impregnation temperature is too low, it is difficult for the metal ions to completely reach the interior of the molecular sieve; if the impregnation time is too long or the impregnation temperature is too high, the impregnation rate is too fast, which can easily cause uneven impregnation and increase energy consumption in the preparation process. Therefore, the impregnation time of this application is 2h to 72h, and the impregnation temperature is 20°C to 50°C, and an adsorbent with excellent desulfurization activity can be prepared.

[0043] According to an embodiment of the present invention, the drying temperature is 70°C to 150°C, and the drying time is 2h to 24h. The inventors found that if the drying temperature is too low or the drying time is too short, the excess water cannot be completely removed; if the drying temperature is too high or the drying time is too long, the preparation energy consumption is increased and the preparation efficiency is affected. Therefore, the drying temperature of the present application is 70°C to 150°C, and the drying time is 2h to 24h, and an adsorbent with excellent desulfurization activity can be prepared.

[0044] According to an embodiment of the present invention, the calcination temperature is 350°C to 500°C, and the calcination time is 2h to 12h. The inventors found that if the calcination temperature is too low or the time is too short, impurities such as inactive components cannot be completely removed; if the calcination temperature is too high or the time is too long, the energy consumption of the preparation will increase, and too high a temperature will affect the stability of the molecular sieve structure. Therefore, the calcination temperature of the present application is 350°C to 500°C, and the calcination time is 2h to 12h, and an adsorbent with excellent desulfurization activity can be prepared.

[0045] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0046] Example 1

[0047] Step 1: 12.7 g of tetraethyl orthosilicate (TEOS), 12.4 g of tetrapropylammonium hydroxide (TPAOH) (25 wt%), and 14.9 g of water were weighed and mixed at room temperature for 15 min. The resulting solution was transferred to a reaction kettle and kept at a constant temperature of 170° C. for 24 h.

[0048] Step 2, washing, drying and calcining the product obtained in step 1 at 550° C. for 6 h;

[0049] Step 3: Take 1.0g of the product obtained in step 2, add 6.5mL of 0.1mol / L zinc nitrate solution, ultrasonically treat for 30min, then place at room temperature for 3h, then dry at 80℃ for 10h, and then calcine at 500℃ for 6h to obtain the finished adsorbent. The length of the main diagonal of the hexagon on the upper and lower bottom surfaces of the adsorbent is 400nm, the thickness is 200nm, the metal oxide content is 5% (weight ratio), and the nanoparticle size is 2.5nm. Marked as sample S-1.

[0050] Step 4: Perform a desulfurization performance evaluation test on the S-1 sample. The concentration of the hydrogen sulfide standard gas used is 100 ppm, and the balance gas is N 2 The first penetration sulfur capacity was measured to be 17.2 mg / g, and the metal oxide utilization rate was 83%. After six cycles, the penetration sulfur capacity was 9.2 mg / g, and the metal oxide utilization rate was 47%. The high-resolution transmission electron microscopy image of 5% ZnO@Silicalite-1 prepared in Example 1 is shown in FIG. Figure 1 As shown, from Figure 1 It can be seen that zinc oxide is uniformly impregnated into the molecular sieve, and the particle size is uniform, about 2.4 nm.

[0051] Example 2

[0052] Step 1: 12.7 g TEOS, 12.4 g TPAOH (25 wt%), and 14.9 g water were weighed and mixed at room temperature for 15 min. The resulting solution was transferred to a reactor and kept at 170° C. for 24 h.

[0053] Step 2, washing, drying and calcining the product obtained in step 1 at 550° C. for 6 h;

[0054] Step 3: Take 1.0g of the product obtained in step 2, add 10.3mL of 0.3mol / L zinc chloride solution, ultrasonically treat for 30min, then place at room temperature for 3h, then dry at 80°C for 10h, and then calcine at 500°C for 6h to obtain the finished adsorbent. The length of the main diagonal of the hexagon on the upper and lower bottom surfaces of the adsorbent is 400nm, the thickness is 200nm, the metal oxide content is 20% (weight ratio), and the nanoparticle size is 5.0nm. Marked as sample S-2.

[0055] Step 4: Perform a desulfurization performance evaluation test on the S-2 sample. The concentration of the hydrogen sulfide standard gas used is 100 ppm, and the balance gas is N 2 The first penetration sulfur capacity was measured to be 61.2 mg / g, and the metal oxide utilization rate was 62%. After six cycles, the penetration sulfur capacity was 39.5 mg / g, and the metal oxide utilization rate was 40%.

[0056] Example 3

[0057] Step 1: 12.7 g TEOS, 12.4 g TPAOH (25 wt%), and 14.9 g water were weighed and mixed at room temperature for 15 min. The resulting solution was transferred to a reactor and kept at 170° C. for 24 h.

[0058] Step 2, washing, drying and calcining the product obtained in step 1 at 550° C. for 6 h;

[0059] Step 3: Take 1.0g of the product obtained in step 2, add 7.3mL of 0.3mol / L zinc chloride solution, ultrasonically treat for 30min, then place at room temperature for 3h, then dry at 80°C for 10h, and then calcine at 500°C for 6h to obtain the finished adsorbent. The length of the main diagonal of the hexagon on the upper and lower bottom surfaces of the adsorbent is 400nm, the thickness is 200nm, the metal oxide content is 15% (weight ratio), and the nanoparticle size is 4.5nm. Marked as sample S-3.

[0060] Step 4: Perform a desulfurization performance evaluation test on the S-3 sample. The concentration of the hydrogen sulfide standard gas used is 100 ppm, and the balance gas is N 2The first breakthrough sulfur capacity was measured to be 41.8 mg / g, and the metal oxide utilization rate was 60%. After six cycles, the breakthrough sulfur capacity was 30.0 mg / g, and the metal oxide utilization rate was 43%.

[0061] Example 4

[0062] Step 1: 7.2 g TEOS, 11.2 g TPAOH (25 wt%), and 1.5 g water were weighed, mixed and stirred at room temperature for 15 min, then aged at 90° C. for 24 h, and the resulting solution was transferred to a reactor and kept at 170° C. for 24 h;

[0063] Step 2, washing, drying and calcining the product obtained in step 1 at 550° C. for 6 h;

[0064] Step 3: Take 1.0g of the product obtained in step 2, add 6.5mL of 0.1mol / L zinc acetate solution, ultrasonically treat for 30min, then place at room temperature for 3h, then dry at 80℃ for 10h, and then calcine at 500℃ for 6h to obtain the finished adsorbent. The length of the main diagonal of the hexagon on the upper and lower bottom surfaces of the adsorbent is 60nm, the thickness is 30nm, the metal oxide content is 5% (weight ratio), and the nanoparticle size is 3.0nm. Marked as sample S-4.

[0065] Step 4: Perform a desulfurization performance evaluation test on the S-4 sample. The concentration of the hydrogen sulfide standard gas used is 100 ppm, and the balance gas is N 2 The first penetration sulfur capacity was measured to be 19.2 mg / g, and the metal oxide utilization rate was 88%. After six cycles, the penetration sulfur capacity was 15.5 mg / g, and the metal oxide utilization rate was 69%.

[0066] Example 5

[0067] Step 1: 12.7 g TEOS, 12.4 g TPAOH (25 wt%), and 14.9 g water were weighed and mixed at room temperature for 15 min. The resulting solution was transferred to a reactor and kept at a constant temperature of 170° C. for 24 h.

[0068] Step 2, washing, drying and calcining the product obtained in step 1 at 550° C. for 6 h;

[0069] Step 3: Take 1.0g of the product obtained in step 2, add 2.5mL of 0.1mol / L zinc nitrate solution, ultrasonically treat for 30min, then place at room temperature for 3h, then dry at 80°C for 10h, and then calcine at 500°C for 6h to obtain the finished adsorbent. The length of the main diagonal of the hexagon on the upper and lower bottom surfaces of the adsorbent is 400nm, the thickness is 200nm, the metal oxide content is 2% (weight ratio), and the nanoparticle size is 2.5nm. Marked as sample S-5.

[0070] Step 4: Perform a desulfurization performance evaluation test on the S-5 sample. The concentration of hydrogen sulfide standard gas used is 10 ppm, and the balance gas is N 2 The first penetration sulfur capacity was measured to be 5.2 mg / g, and the metal oxide utilization rate was 87%. After six cycles, the penetration sulfur capacity was 4.4 mg / g, and the metal oxide utilization rate was 73%.

[0071] The desulfurization breakthrough curve of 2% ZnO@Silicalite-1 in Example 5 is as follows: Figure 2 As shown, from Figure 2 It can be seen that after six cycles, the sulfur capacity of the adsorbent decreases very little compared to the initial capacity, indicating that the adsorbent of the present application has good stability and is sintering-resistant during the adsorbent regeneration process.

[0072] Example 6

[0073] Step 1: 12.7 g TEOS, 12.4 g TPAOH (25 wt%), and 14.9 g water were weighed and mixed at room temperature for 15 min. The resulting solution was transferred to a reactor and kept at a constant temperature of 170° C. for 24 h.

[0074] Step 2, washing, drying and calcining the product obtained in step 1 at 550° C. for 6 h;

[0075] Step 3: Take 1.0g of the product obtained in step 2, add 6.0mL of 0.1mol / L manganese nitrate solution, ultrasonically treat for 30min, then place at room temperature for 3h, then dry at 80°C for 10h, and then calcine at 500°C for 6h to obtain the finished adsorbent. The length of the main diagonal of the hexagon on the upper and lower bottom surfaces of the adsorbent is 400nm, the thickness is 200nm, the metal oxide content is 5% (weight ratio), and the nanoparticle size is 3.5nm. Marked as sample S-6.

[0076] Step 4: Perform a desulfurization performance evaluation test on the S-6 sample. The concentration of the hydrogen sulfide standard gas used is 100 ppm, and the balance gas is N 2 The first penetration sulfur capacity was measured to be 8.1 mg / g, and the metal oxide utilization rate was 74%. After six cycles, the penetration sulfur capacity was 6.8 mg / g, and the metal oxide utilization rate was 62%.

[0077] Example 7

[0078] Step 1: 12.7 g TEOS, 12.4 g TPAOH (25 wt%), and 14.9 g water were weighed and mixed at room temperature for 15 min. The resulting solution was transferred to a reactor and kept at a constant temperature of 170° C. for 24 h.

[0079] Step 2, washing, drying and calcining the product obtained in step 1 at 550° C. for 6 h;

[0080] Step 3: Take 1.0g of the product obtained in step 2, add 6.0mL of 0.1mol / L mixed solution of zinc nitrate and manganese nitrate (molar ratio of manganese to zinc is 1:1), ultrasonically treat for 30min, then place at room temperature for 3h, then dry at 80°C for 10h, and then calcine at 500°C for 6h to obtain the finished adsorbent. The length of the main diagonal of the hexagon on the upper and lower bottom surfaces of the adsorbent is 400nm, the thickness is 200nm, the metal oxide content is 5% (weight ratio), and the particle size of the nanoparticles is 2.2nm. Marked as sample S-7.

[0081] Step 4: Perform a desulfurization performance evaluation test on the S-7 sample. The concentration of the hydrogen sulfide standard gas used is 100 ppm, and the balance gas is N 2 The first penetration sulfur capacity was measured to be 9.2 mg / g, and the metal oxide utilization rate was 83%. After six cycles, the penetration sulfur capacity was 7.5 mg / g, and the metal oxide utilization rate was 68%.

[0082] Example 8

[0083] Step 1: 12.7 g TEOS, 12.4 g TPAOH (25 wt%), and 14.9 g water were weighed and mixed at room temperature for 15 min. The resulting solution was transferred to a reactor and kept at a constant temperature of 170° C. for 24 h.

[0084] Step 2, washing, drying and calcining the product obtained in step 1 at 550° C. for 6 h;

[0085] Step 3: Mix 3.0 g of the solid powder obtained in step 2 with 30.0 g of TPAOH, transfer the obtained solid-liquid mixture into a reactor, and keep the temperature at 170° C. for 48 h;

[0086] Step 4: Take 1.0g of the product obtained in step 3, add 1.3mL of 0.1mol / L manganese nitrate solution, ultrasonically treat for 30min, then place at room temperature for 3h, then dry at 80°C for 10h, and then calcine at 500°C for 6h to obtain the finished adsorbent. The length of the main diagonal of the hexagon on the upper and lower bottom surfaces of the adsorbent is 450nm, the adsorbent is hollow, the wall thickness is 20nm, the metal oxide content is 1% (weight ratio), and the nanoparticle size is 1.5nm. Marked as sample S-8.

[0087] Step 5: Perform a desulfurization performance evaluation test on the S-8 sample. The concentration of the hydrogen sulfide standard gas used is 100 ppm, and the balance gas is N 2The first penetration sulfur capacity was measured to be 3.6 mg / g, and the metal oxide utilization rate was 93%. After six cycles, the penetration sulfur capacity was 3.4 mg / g, and the metal oxide utilization rate was 88%.

[0088] Comparative Example 1

[0089] The desulfurization performance of a commercial desulfurization adsorbent of UOP was tested under the same conditions as in Example 1. The adsorbent is composed of active material zinc oxide nanoparticles and a binder. The desulfurization cycle test shows that the first breakthrough sulfur capacity of the commercial adsorbent is 9.2 mg / g, and the zinc oxide utilization rate is only 2.6%; after only three cycles, the breakthrough sulfur capacity drops sharply to 2.1 mg / g, and the zinc oxide utilization rate is 0.5%.

[0090] From the desulfurization performance evaluation test results of the adsorbents obtained in Examples 1-8, it can be seen that the adsorbent of the present application has a high metal oxide utilization rate, and after 6 cycles, the sulfur capacity of the adsorbent decreases less than the initial capacity. The commercial adsorbent in Comparative Example 1 not only has a low metal oxide utilization rate for the initial desulfurization, but also a sharp drop in the metal oxide utilization rate after 3 cycles, indicating that this commercial adsorbent has low desulfurization activity, is not resistant to sintering, and has poor cyclic regeneration performance. From this comparison, it can be seen that the adsorbent of the present application not only has a high desulfurization activity, but also can effectively avoid the sintering of metal oxide nanoparticles during high-temperature regeneration, and has excellent cyclic regeneration performance.

[0091] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0092] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. Use of a hydrogen sulfide removal adsorbent in removing hydrogen sulfide, characterized in that: The hydrogen sulfide removal adsorbent comprises an MFI type molecular sieve and metal oxide nanoparticles, wherein the metal oxide nanoparticles are distributed in the pores of the MFI type molecular sieve. The MFI type molecular sieve includes at least one of a solid straight hexagonal prism-shaped MFI type molecular sieve and a hollow straight hexagonal prism-shaped MFI type molecular sieve. The length of the main diagonal line of the hexagon in the straight hexagonal prism of the MFI molecular sieve is 0.05 μm to 10 μm. The metal oxide nanoparticles include at least one of zinc oxide and manganese oxide, The average particle size of the metal oxide nanoparticles is 0.5 nm to 5 nm. Based on the total mass of the adsorbent, the content of the MFI molecular sieve is 80wt% to 99.5wt%, and the content of the metal oxide nanoparticles is 0.5wt% to 20wt%.

2. The use according to claim 1, characterized in that: The thickness of the MFI molecular sieve with the solid straight hexagonal prism morphology is 30nm-1000nm.

3. The use according to claim 1, characterized in that: The shell thickness of the straight hexagonal prisms of the MFI type molecular sieve with the hollow straight hexagonal prism morphology is 10nm~80nm.

4. The use according to claim 1, characterized in that: The metal oxide nanoparticles include zinc oxide and manganese oxide, and a molar ratio of manganese in the manganese oxide to zinc in the zinc oxide is not greater than 1.

5. The use according to claim 1, characterized in that: The method for preparing the hydrogen sulfide removal adsorbent comprises: The metal salt solution and the MFI molecular sieve are mixed and impregnated, dried, and then calcined to obtain a hydrogen sulfide removal adsorbent.

6. The use according to claim 5, characterized in that: The metal salt solution includes at least one of zinc nitrate, zinc sulfate, zinc chloride, manganese chloride, manganese nitrate, manganese acetate, manganese sulfate, zinc nitrate hexahydrate, zinc sulfate heptahydrate, manganese chloride tetrahydrate, manganese nitrate hexahydrate, manganese acetate dihydrate, manganese acetate tetrahydrate, manganese sulfate tetrahydrate, manganese sulfate pentahydrate and manganese sulfate heptahydrate.

7. The use according to claim 5, characterized in that: The concentration of the metal salt solution is 0.1 mol / L to 2.0 mol / L.

8. The use according to claim 5, characterized in that: The solvent of the metal salt solution is water.

9. The use according to claim 5, characterized in that: The immersion time is 2 hours to 72 hours, and the immersion temperature is 20° C. to 50° C.

10. The use according to claim 5, characterized in that: The drying temperature is 70° C. to 150° C., and the drying time is 2 h to 24 h.

11. The use according to claim 5, characterized in that: The calcination temperature is 350° C. to 500° C., and the calcination time is 2 h to 12 h.

Citation Information

Patent Citations

  • Preparation method of absorbent for removing indoor low-concentration hydrogen sulfide

    CN103962096A

  • Method for reinforcing acidity of Silicalite-1 zeolite molecular sieve and application thereof to dehydrogenation of alkane

    CN108745406A

  • Fine desulfurizer for zinc oxide at room temperature, preparation method and application

    CN109432999A

  • Preparation method and application of Zn-coated Silicalite-1 molecular sieve propane dehydrogenation catalyst

    CN115414959A

  • Nitrogen oxide remover

    JP2014108370A