Method for preparing microwave absorbing fiber with high microwave absorbing agent content by melt spinning and its product

Absorbing fibers with high absorber content are prepared through melt spinning technology, which solves the problems of low fiber absorber content and poor spinnability in the existing technology, and achieves efficient absorbing performance and continuous spinnability, which is suitable for military applications. Stealth technology.

CN116516519BActive Publication Date: 2024-10-01DONGHUA UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310421914.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-01
Estimated Expiration
2043-04-19

AI Technical Summary

Technical Problem

The existing technology is difficult to prepare polymer fibers filled with high inorganic components, and cannot maintain continuous spinnability of absorbing fibers, resulting in low absorber content and poor absorbing effect.

Method used

The melt spinning method is used to prepare the skin layer and core layer masterbatch through a twin-screw extruder. They are used as skin material and core material respectively for coaxial melt spinning to form a skin-core structure of the wave-absorbing fiber to ensure that the wave absorbers are in the core layer. high content and continuous spinnability.

Benefits of technology

It improves the absorbing performance of the fiber and solves the problem of low addition of absorbing components. The fiber does not lose its absorbing ability after external friction or washing, and has a wider absorbing range and stronger absorbing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116516519B_ABST
    Figure CN116516519B_ABST
Patent Text Reader

Abstract

A method for preparing absorbing fibers with high absorber content by melt spinning, comprising the steps of: taking a polymer and passing it through a twin-screw extruder to obtain a skin masterbatch; taking the same polymer, adding absorbers and coupling agents, and obtaining a core masterbatch with a mass fraction ratio of absorbers to polymer of 1:10 to 1:1 through a twin-screw extruder; selecting a skin-core spinning assembly for coaxial melt spinning, and extruding the skin masterbatch and the core masterbatch as skin material and core material from the skin-core spinning assembly respectively to obtain nascent fibers; and obtaining absorbing fibers with a skin-core structure through stretching and heat setting. The method for preparing absorbing fibers with high absorber content by melt spinning of the present invention adopts a coaxial melt spinning process for spinning, and then undergoes stretching, heat setting and other processes. The obtained absorbing fibers have good absorbing effects in the range of 18 GHz to 2 GHz, and can be widely used in civilian or military applications. They can not only protect some electronic devices from electromagnetic interference, but also improve the stealth performance of some military weapons.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of melt spinning and microwave absorbing fibers, and in particular to a method for preparing microwave absorbing fibers with high microwave absorbing agent content by melt spinning and the products thereof. Background Art

[0002] With the rapid development of military information technology and the replacement of global military equipment, absorbing materials have become the technical core of military equipment stealth and the focus and key of my country's military technology development. The development of absorbing technology can improve the anti-detection and anti-reconnaissance capabilities of various weapons and equipment. Therefore, absorbing materials have attracted the attention of more and more countries and become a hot spot for research and development in various countries. Absorbers can absorb electromagnetic waves and convert them into heat or other forms of energy and dissipate them, so they are widely used in military stealth technology. Compared with coating technology, absorbing fibers have the characteristics of flexibility, lightness, and easy to use, but there are problems such as low addition ratio and poor absorbing effect. Based on the magnetoelectric coupling theory, when electromagnetic waves enter the absorbing material, the conductive carriers inside the material are directional moved by the magnetic field to generate current, thereby dissipating the electromagnetic waves. According to theoretical calculations, the fiber can only have absorbing properties when the absorber content reaches more than 10wt%, and the absorbing properties tend to be practical when it reaches more than 30wt%. Therefore, it is of great significance to construct fibers with high absorber content. Summary of the invention

[0003] Based on this, the present invention provides a method for preparing absorbing fibers with high absorber content by melt spinning and its products, so as to solve the technical problems that polymer fibers in the prior art are difficult to achieve high inorganic component filling and cannot maintain continuous spinnability.

[0004] To achieve the above object, the present invention provides a method for preparing microwave absorbing fibers with a high microwave absorbing agent content by melt spinning, which comprises the following steps:

[0005] (1) taking a polymer and passing it through a twin-screw extruder to obtain a skin masterbatch; taking the same polymer, adding a wave absorber and a coupling agent, and passing it through a twin-screw extruder to obtain a core masterbatch in which the mass fraction of the wave absorber to the mass fraction of the polymer is 1:10 to 1:1; wherein the polymer is polyethylene terephthalate, polyamide, polyphenylene sulfide or polypropylene, and the wave absorber is an inorganic wave absorber with a particle size of less than 500 nm;

[0006] (2) selecting a sheath-core spinning assembly for coaxial melt spinning, and extruding the sheath masterbatch and the core masterbatch as the sheath material and the core material from the sheath-core spinning assembly, respectively, to obtain primary fibers;

[0007] (3) The spun fibers are stretched and heat-set to obtain a sheath-core structured absorbing fiber, wherein the core material diameter of the absorbing fiber is not less than 1 / 3 of the total diameter.

[0008] In the specific preparation process, the relative size of the skin and the core can be changed by changing the relative aperture of the coaxial needle in the skin-core spinning assembly. At the same time, in order to achieve a high absorbency, the absorber content must be as high as possible under the premise of meeting continuous spinnability. The skin layer is a pure polymer material with good spinnability, and its purpose is to cover the core layer with poor spinnability, so that both the skin layer and the core layer can meet the requirements of continuous spinnability. Preferably, the thickness of the skin layer is not less than 1 / 10 of the total diameter.

[0009] As a further preferred technical solution of the present invention, the inorganic absorber is a carbon absorber (such as graphite, graphene, carbon nanotube or carbon black) or a carbonyl iron absorber. The carbonyl iron absorber is an absorbing material with carbonyl iron as the main component, and the carbonyl iron is composed of iron and a certain amount of carbon monoxide, and the chemical formula is Fe(CO)5.

[0010] As a further preferred technical solution of the present invention, the coupling agent is a silane coupling agent or a titanate coupling agent.

[0011] As a further preferred technical solution of the present invention, in step (1), before preparing the skin layer masterbatch and the core layer masterbatch, the polymer is dried in a drum oven, and the absorber is dried in a vacuum oven at 90-95° C. for 10-12 hours.

[0012] As a further preferred technical solution of the present invention, in step (2), the spinning temperature of the melt spinning process is 150-300°C, the cooling blowing temperature is 20-30°C, the wind speed is 0.3-0.5 m / s, and the humidity is 60-75%.

[0013] As a further preferred technical solution of the present invention, in step (3), stretching and heat setting are performed successively, wherein the stretching temperature is 80-135°C, the stretching ratio is 2-5 times, and the heat setting temperature is 180-230°C.

[0014] As a further preferred technical solution of the present invention, in the core layer masterbatch prepared in step (1), the mass fraction ratio of the absorber to the mass fraction of the polymer is 1:5 to 1:1, and more preferably 1:2 to 1:1.

[0015] According to another aspect of the present invention, the present invention further provides an absorbing fiber, which is prepared by any of the above methods for preparing absorbing fibers with high absorber content by melt spinning.

[0016] The method for preparing microwave absorbing fibers with high microwave absorbing agent content by melt spinning and the product thereof of the present invention can achieve the following beneficial effects by adopting the above technical scheme:

[0017] 1) The ratio of the mass fraction of the absorber in the core layer to the polymer material fraction is up to 1:1, which solves the problem of low addition of absorbing components in the fiber, improves the absorbing performance of the fiber, and the process can be extended to other high-filling spinning fields.

[0018] 2) The fiber prepared by the present invention has a skin-core structure, and the skin layer and the core layer are made of the same polymer, which solves the problem of skin-core interface bonding. Compared with coated absorbing fibers, it will not lose its absorbing ability even if it is subjected to external friction or washing. Moreover, it also has a wider absorbing range and stronger absorbing performance than ordinary absorbing materials.

[0019] 3) The absorbent component of the absorbing fiber prepared in the present invention is a continuous phase in the core layer, which has a promoting significance for the conductivity loss. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0021] Figure 1 An optical microscope image of a cross section of the PET absorbing fiber with a skin-core structure obtained in Example 1;

[0022] Figure 2 The reflection loss curve of the PET absorbing fiber with a skin-core structure obtained in Example 1 in the range of 2 to 4 GHz;

[0023] Figure 3 This is an optical microscope image of the cross section of the PP absorbing fiber with a skin-core structure obtained in Example 2;

[0024] Figure 4 The reflection loss curve of the PP absorbing fiber with a skin-core structure obtained in Example 2 in the range of 12 to 18 GHz;

[0025] Figure 5 This is an optical microscope image of the cross section of the PE absorbing fiber with a skin-core structure obtained in Example 4;

[0026] Figure 6 This is the reflection loss curve of the PE absorbing fiber with a skin-core structure prepared in Example 4 in the range of 6 to 8 GHz.

[0027] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings in conjunction with the embodiments. DETAILED DESCRIPTION

[0028] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0029] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0030] Example 1

[0031] A method for preparing absorbing fibers with high absorber content by melt spinning. The prepared absorbing fibers include a skin layer and a core layer. The skin layer is pure polyethylene terephthalate (PET), and the core layer is a polyethylene terephthalate-based composite filled with carbon-based absorbers.

[0032] The molecular weight of the polyethylene terephthalate slices in the skin layer and the core layer is 22000, and the particle size of the carbon-based absorber in the core layer is 10 nm.

[0033] The specific preparation method is as follows:

[0034] 500 g of polyethylene terephthalate (PET) chips were weighed and passed through a twin-screw extruder to obtain skin layer masterbatch.

[0035] Weigh 500g of carbon-based absorbers and 150g of silane coupling agent, add them to 500g of polyethylene terephthalate (PET) chips, mix them evenly, and pass them through a twin-screw extruder to obtain a core layer masterbatch (the ratio of the mass fraction of the absorber to the mass fraction of polyethylene terephthalate is 1:1; the mass fraction of the silane coupling agent is 33% of the mass fraction of the absorber).

[0036] Then, a sheath-core spinning assembly is selected for spinning. The sheath-core spinning assembly has two coaxially arranged needles. The cortex masterbatch is extruded from the outer needle, and the core masterbatch is extruded from the inner core needle. The spinning process parameters are: spinning temperature is 270°C, cold blowing temperature is 20°C during spinning, wind speed is 0.3m / s, humidity is 60%, and primary fiber is obtained.

[0037] The raw fiber is stretched and heat-set in sequence, the stretching temperature is 90°C, the stretching ratio is 2 times, and the heat setting temperature is 200°C, and finally a PET absorbing fiber with a skin-core structure and a core material diameter of 1 / 3 of the total diameter is obtained.

[0038] Figure 1 This is an optical microscope image of the cross-section of the prepared PET absorbing fiber with a skin-core structure, and a clear interface of the skin-core structure can be seen.

[0039] The electromagnetic parameters of the fiber were measured using a vector network analyzer in the test range of 2 to 18 GHz, and the reflection loss (RL) was calculated using the complex dielectric constant and complex magnetic permeability. Figure 2As shown, the prepared PET absorbing fiber with a skin-core structure has a minimum reflection loss of -15dB in the range of 2 to 4GHz.

[0040] Example 2

[0041] A method for preparing absorbing fibers with high absorber content by melt spinning. The prepared absorbing fibers include a skin layer and a core layer. The skin layer is pure polypropylene (PP), and the core layer is a polypropylene-based composite filled with carbonyl iron absorbers.

[0042] The molecular weight of the polypropylene slices in the skin layer and the core layer is 180000, and the particle size of the carbonyl iron absorber in the core layer is 200nm.

[0043] Weigh 500 g of polypropylene (PP) chips and pass them through a twin-screw extruder to obtain a skin layer masterbatch.

[0044] Weigh 100g of carbonyl iron absorber and 40g of titanate coupling agent, add them to 500g of polypropylene (PP) chips, mix them evenly, and pass them through a twin-screw extruder to obtain a core layer masterbatch (the ratio of the mass fraction of the absorber to the mass fraction of the polypropylene is 1:5; the mass fraction of the titanate coupling agent is 40% of the mass fraction of the absorber).

[0045] Then, a sheath-core spinning assembly is selected for spinning. The sheath-core spinning assembly has two coaxially arranged needles. The sheath masterbatch is extruded from the outer needle, and the core masterbatch is extruded from the inner core needle. The spinning process parameters are: spinning temperature is 180°C, cold blowing temperature is 25°C during spinning, wind speed is 0.4m / s, humidity is 70%, and primary fiber is obtained.

[0046] The raw fiber was stretched and heat-set in sequence, with the stretching temperature being 130°C, the stretching ratio being 3 times, and the heat-setting temperature being 180°C, to finally obtain a PP absorbing fiber with a skin-core structure and a core diameter being 3 / 5 of the total diameter.

[0047] Figure 3 This is an optical microscope image of the cross-section of the prepared PP absorbing fiber with a skin-core structure, and a clear interface of the skin-core structure can be seen.

[0048] The electromagnetic parameters of the fiber were measured using a vector network analyzer in the test range of 2 to 18 GHz, and the reflection loss (RL) was calculated using the complex dielectric constant and complex magnetic permeability. Figure 4 As shown, the prepared PP absorbing fiber with a skin-core structure has a minimum reflection loss of -30 dB in the range of 12 to 18 GHz.

[0049] Example 3

[0050] A method for preparing absorbing fibers with high absorber content by melt spinning. The prepared absorbing fibers include a skin layer and a core layer. The skin layer is pure polypropylene (PP), and the core layer is a polypropylene-based composite filled with carbonyl iron absorbers.

[0051] The molecular weight of the polypropylene slices in the skin layer and the core layer is 180000, and the particle size of the carbonyl iron absorber in the core layer is 200nm.

[0052] Weigh 500 g of polypropylene (PP) chips and pass them through a twin-screw extruder to obtain a skin layer masterbatch.

[0053] Weigh 500g of carbonyl iron absorber and 200g of titanate coupling agent, add them to 500g of polypropylene (PP) chips, mix them evenly, and pass through a twin-screw extruder to obtain a core layer masterbatch (the ratio of the mass fraction of the absorber to the mass fraction of the polypropylene is 1:1; the mass fraction of the titanate coupling agent is 40% of the mass fraction of the absorber).

[0054] Then, a sheath-core spinning assembly is selected for spinning. The sheath-core spinning assembly has two coaxially arranged needles. The sheath masterbatch is extruded from the outer needle, and the core masterbatch is extruded from the inner core needle. The spinning process parameters are: spinning temperature is 180°C, cold blowing temperature is 25°C during spinning, wind speed is 0.4m / s, humidity is 70%, and primary fiber is obtained.

[0055] The raw fiber was stretched and heat-set in sequence, with the stretching temperature being 130°C, the stretching ratio being 3 times, and the heat-setting temperature being 180°C, to finally obtain a PP absorbing fiber with a skin-core structure and a core diameter being 3 / 5 of the total diameter.

[0056] The electromagnetic parameters of the fiber are measured using a vector network analyzer in the test range of 2 to 18 GHz, and the reflection loss (RL) is calculated using the complex dielectric constant and complex magnetic permeability. The minimum reflection loss of the PP absorbing fiber is -35 dB in the range of 12 to 18 GHz.

[0057] Example 4

[0058] A method for preparing absorbing fibers with high absorber content by melt spinning. The prepared absorbing fibers include a skin layer and a core layer. The skin layer is pure polyethylene (PE), and the core layer is a polyethylene-based composite filled with carbonyl iron absorbers.

[0059] The molecular weight of polyethylene in the skin layer and the core layer is 200000, and the particle size of the carbonyl iron absorber in the core layer is 480nm.

[0060] Weigh 500 g of polyethylene (PE) chips and pass them through a twin-screw extruder to obtain skin layer masterbatch.

[0061] Weigh 50g of carbonyl iron absorber and 25g of titanate coupling agent, add them to 500g of polyethylene (PE) chips, mix them evenly, and pass them through a twin-screw extruder to obtain a core layer masterbatch (the ratio of the mass fraction of the absorber to the mass fraction of the polyethylene is 1:10; the mass fraction of the titanate coupling agent is 50% of the mass fraction of the absorber).

[0062] Then, a sheath-core spinning assembly is selected for spinning. The sheath-core spinning assembly has two coaxially arranged needles. The sheath masterbatch is extruded from the outer needle, and the core masterbatch is extruded from the inner core needle. The spinning process parameters are: spinning temperature is 160°C, cold blowing temperature is 30°C during spinning, wind speed is 0.5m / s, humidity is 65%, and primary fiber is obtained.

[0063] The raw fiber was stretched and heat-set in sequence, with the stretching temperature being 100° C., the stretching ratio being 5 times, and the heat-setting temperature being 230° C., and finally a PE absorbing fiber with a skin-core structure and a core diameter being 4 / 5 of the total diameter was obtained.

[0064] Figure 5 This is an optical microscope image of the cross-section of the prepared PE absorbing fiber with a skin-core structure, and a clear interface of the skin-core structure can be seen.

[0065] The electromagnetic parameters of the fiber were measured using a vector network analyzer in the test range of 2 to 18 GHz, and the reflection loss (RL) was calculated using the complex dielectric constant and complex magnetic permeability. Figure 6 As shown, the prepared PE absorbing fiber with a skin-core structure has a minimum reflection loss of -15.5 dB in the range of 6 to 8 GHz.

[0066] Example 5

[0067] A method for preparing absorbing fibers with high absorber content by melt spinning. The prepared absorbing fibers include a skin layer and a core layer. The skin layer is pure polyethylene (PE), and the core layer is a polyethylene-based composite filled with carbonyl iron absorbers.

[0068] The molecular weight of polyethylene in the skin layer and the core layer is 200000, and the particle size of the carbonyl iron absorber in the core layer is 480nm.

[0069] Weigh 500 g of polyethylene (PE) chips and pass them through a twin-screw extruder to obtain skin layer masterbatch.

[0070] Weigh 500g of carbonyl iron absorber and 250g of titanate coupling agent, add them to 500g of polyethylene (PE) chips, mix them evenly, and pass them through a twin-screw extruder to obtain a core layer masterbatch (the ratio of the mass fraction of the absorber to the mass fraction of the polyethylene is 1:1; the mass fraction of the titanate coupling agent is 50% of the mass fraction of the absorber).

[0071] Then, a sheath-core spinning assembly is selected for spinning. The sheath-core spinning assembly has two coaxially arranged needles. The sheath masterbatch is extruded from the outer needle, and the core masterbatch is extruded from the inner core needle. The spinning process parameters are: spinning temperature is 160°C, cold blowing temperature is 30°C during spinning, wind speed is 0.5m / s, humidity is 65%, and primary fiber is obtained.

[0072] The raw fiber was stretched and heat-set in sequence, with the stretching temperature being 100° C., the stretching ratio being 5 times, and the heat-setting temperature being 230° C., and finally a PE absorbing fiber with a skin-core structure and a core diameter being 4 / 5 of the total diameter was obtained.

[0073] The electromagnetic parameters of the fiber were measured using a vector network analyzer in the test range of 2 to 18 GHz, and the reflection loss (RL) was calculated using the complex dielectric constant and complex magnetic permeability. The minimum reflection loss of the PE absorbing fiber was -23 dB in the range of 6 to 8 GHz.

[0074] In addition, the present invention also provides an absorbing fiber with a high content of microwave absorber prepared by melt spinning, which is prepared by the method for preparing absorbing fiber with a high content of microwave absorber prepared by melt spinning described in any of the above embodiments.

[0075] Although specific embodiments of the present invention are described above, those skilled in the art should understand that these are merely examples and that various changes or modifications may be made to the embodiments without departing from the principles and essence of the present invention. The scope of protection of the present invention is limited only by the appended claims.

Claims

1. A method for preparing microwave absorbing fibers with high microwave absorbing agent content by melt spinning, characterized in that: The following steps are involved: (1) taking a polymer and passing it through a twin-screw extruder to obtain a skin masterbatch; taking the same polymer and adding a wave absorber and a coupling agent, and passing it through a twin-screw extruder to obtain a core masterbatch in which the mass fraction of the wave absorber and the mass fraction of the polymer are 1:1; wherein the polymer is polyethylene with a molecular weight of 200,000, and the wave absorber is a carbonyl iron-based wave absorber with a particle size of 480 nm; (2) A sheath-core spinning assembly was selected for coaxial melt spinning, and the sheath masterbatch and the core masterbatch were extruded from the sheath-core spinning assembly as the sheath material and the core material, respectively, to obtain nascent fibers. The spinning temperature of the melt spinning process was 160°C, the cooling air temperature was 30°C, the wind speed was 0.5 m / s, and the humidity was 65%; (3) The spun fibers are stretched and heat-set in succession to obtain a sheath-core structured absorbing fiber, wherein the core diameter of the absorbing fiber is 4 / 5 of the total diameter, the stretching temperature is 100°C, the stretching ratio is 5 times, and the heat-setting temperature is 230°C.

2. The method for preparing microwave absorbing fibers with high microwave absorbing agent content by melt spinning according to claim 1, characterized in that: The coupling agent is a silane coupling agent or a titanate coupling agent.

3. The method for preparing microwave absorbing fibers with high microwave absorbing agent content by melt spinning according to claim 1, characterized in that: Step (1) Before preparing the skin layer masterbatch and the core layer masterbatch, the polymer is dried in a drum oven, and the absorber is dried in a vacuum oven at 90-95° C. for 10-12 hours.

4. A microwave absorbing fiber, characterized in that: The microwave absorbing fiber is prepared by the method for preparing microwave absorbing fiber with high microwave absorbing agent content by melt spinning as described in any one of claims 1 to 3.