Polyvinyl acetal composite sponge with antibacterial function and preparation method thereof

By introducing antibacterial substances on polyvinyl acetal sponges and using acetal reaction and free radical polymerization, polyvinyl acetal composite sponges with excellent antibacterial properties and simple preparation processes were prepared, which solved the complex operation in the existing technology and the problem of difficulty in mass production.

CN116656000BInactive Publication Date: 2024-11-29CHUNYU TECH (GUANGDONG) CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310642796.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, the method of preparing polyvinyl acetal sponges with antibacterial functions is complicated to operate, the sponge performance is poor, the selection range of antibacterial raw materials is narrow, and it is difficult to achieve large-scale production.

Method used

By introducing substances with antibacterial functions on the polyvinyl acetal sponge, and using acetal reaction and free radical polymerization reaction, a polyvinyl acetal composite sponge with antibacterial properties is prepared. This method is simple to operate, has a wide range of raw materials, and has mild reaction conditions, which is suitable for large-scale production.

Benefits of technology

The antibacterial function of polyvinyl acetal sponge is realized, the three-dimensional pore structure and excellent mechanical properties of the sponge are maintained, the water absorption speed of the sponge is improved, and the preparation process is simple and feasible, suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116656000B_ABST
    Figure CN116656000B_ABST
Patent Text Reader

Abstract

The present invention provides a polyvinyl acetal composite sponge with antibacterial function and a preparation method thereof. A substance with antibacterial function is introduced into the polyvinyl acetal sponge through acetal reaction and free radical polymerization reaction, and a polyvinyl acetal sponge with antibacterial performance is prepared. With the polyvinyl acetal sponge as the base material, an antibacterial polyvinyl acetal sponge is obtained under mild conditions by an impregnation-grafting method. A composite antibacterial sponge material is obtained. The sponge preparation process is simple, the conditions are controllable, and large-scale production can be achieved. Compared with the basic sponge, it has a broader application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials, and in particular relates to a polyvinyl acetal composite sponge with antibacterial function and a preparation method thereof. Background Art

[0002] Polyvinyl acetal (PVF) sponge with open-pore structure has high water absorption capacity, excellent mechanical properties and good biocompatibility. It is widely used as a cleaning material and biomedical material. Expanding the function of polyvinyl alcohol sponge can meet more usage requirements. At present, polyvinyl alcohol acetal sponge with antibacterial function has broad application prospects in health, medical dressings, hemostatic materials, food industry and hygiene fields.

[0003] At present, there are two common methods for preparing polyvinyl acetal sponge with antibacterial function. One is to prepare or load inorganic and organic antibacterial agents such as nano silver, graphene oxide, chitosan and other materials with antibacterial function in the sponge preparation process, so that the sponge has antibacterial function. For example, patent CN101954115A "Antibacterial medical sponge dressing and its preparation method" mixes a certain amount of polyvinyl alcohol, foaming agent, silk protein and deionized water evenly, stirs and foams at high speed, and then adds aldehyde and acid solution, stirs polyvinyl alcohol and silk protein under acid catalysis, and then puts them into an oven for curing and molding to obtain a sponge substrate. Then, the cleaned sponge is placed in a nano silver aqueous solution and soaked for 30 minutes, and then freeze-dried and processed. Obtain a polyvinyl alcohol medical sponge dressing with antibacterial function. However, the antibacterial function of the sponge obtained by this method is short in time, pollutes the environment, and the large-scale release of antibacterial agents is easy to cause harm to the human body. Another method for preparing polyvinyl acetal sponge with antibacterial function is to graft monomers with antibacterial function on the surface of the material by chemical crosslinking, polymerization or physical crosslinking, or to introduce materials with antibacterial properties during the preparation. The antibacterial material prepared by this method has the advantages of long-lasting antibacterial property, stable antibacterial function, and good biocompatibility, and has broad application prospects. For example, Chen Xue (Chen Xue. Preparation and performance study of antibacterial chitosan / polyvinyl alcohol silver-loaded composite sponge dressing [D]. Chongqing University, 2021. DOI: 10.27670 / d.cnki.gcqdu.2021.004011.) mixed chitosan solution and polyvinyl alcohol solution in a certain proportion, added glutaraldehyde for crosslinking, and then added a certain amount of glycerol plasticizer to improve the mechanical properties of the sponge. After mixing evenly, the material was freeze-dried to obtain a polyvinyl alcohol sponge material with antibacterial function. Sha et al. (Sha, D., et al., ACS APPLIED POLYMER MATERIALS, 2020.2(11): p.4936-4942.) cleaned the homemade polyvinyl alcohol formal sponge and soaked it in an alkaline solution. Under nitrogen atmosphere, the homemade quaternary ammonium salt epoxypropyl-n,n-dimethyldodecyl ammonium chloride (EDAC) was added to the alkaline solution at the same time. The epoxy group in the quaternary ammonium salt is very active and can undergo a ring-opening reaction with the hydroxyl group in PVF under alkaline conditions. A polyvinyl alcohol formal sponge with excellent antibacterial function was successfully prepared.Yang et al. (Yang, X., et al., Journal of Applied Polymer Science, 2019.136(6): p.47047; Yang, X., et al., New journal of chemistry, 2019.43(37): p.14961-14971.) used polyvinyl formal sponge as the substrate, and grafted zwitterions, cations, etc. with antibacterial functions on the polyvinyl formal sponge by initiating a free radical reaction with ammonium cerium nitrate under acidic conditions to obtain an antibacterial material with antibacterial function. Another method is to functionalize PVA to obtain a polyvinyl acetal sponge with excellent antibacterial function. For example, in patent CN114106400A "An aziridine cross-linked N-halamine antibacterial PVA sponge and its preparation method and application", PVA is reacted with chloroacetaldehyde and glyoxylic acid to obtain PVA containing carbon-chlorine bonds and carboxyl groups, which is then reacted with 1-chloro-2,2,5,5-tetramethyl-4-imidazolidinone to obtain PVA molecules with halamine groups. After further cross-linking with an aziridine cross-linker and emulsification molding, an N-halamine antibacterial PVA sponge is obtained through freeze-drying. The prepared N-halamine PVA sponge has good antibacterial properties and liquid absorption, and can be used as a hemostatic material and wound dressing.

[0004] However, the antibacterial effect of antibacterial monomers such as cross-linked chitosan in the above modification methods is limited, the antibacterial performance is not ideal, and the experimental equipment requirements are high, making it difficult to achieve large-scale production; the modification using antibacterial monomers containing homemade epoxy groups is also relatively complicated, the selectivity of the raw materials that can be used is small, the reaction efficiency is low, and it is difficult to obtain high-density grafting. The performance of polyvinyl alcohol after direct modification is difficult to determine, which is easy to affect the mechanical properties and reactions of the sponge itself, and the obtained sponge effect is not good. Summary of the invention

[0005] Based on the shortcomings of the above methods, the purpose of the present invention is to provide a polyvinyl acetal composite sponge with antibacterial function and a preparation method thereof. The preparation method has a simple and convenient operation process, a wide source of raw materials, and mild reaction conditions, which solves the problems of complex modification operation of polyvinyl acetal sponge, poor sponge performance, and narrow selection range of antibacterial raw materials in the prior art. At the same time, a polyvinyl acetal composite sponge with excellent antibacterial performance is obtained. The present invention has a simple operation process, low equipment requirements, and can achieve large-scale production.

[0006] The purpose of the present invention is achieved through the following technical solutions.

[0007] A method for preparing a polyvinyl acetal composite sponge with antibacterial function comprises the following steps:

[0008] (1) dissolving an unsaturated monomer containing a hydroxyl group and a monomer having an antibacterial function in an aqueous solution;

[0009] (2) adding polyvinyl acetal sponge to the mixed solution;

[0010] (3) adjusting the mixed solution to be acidic;

[0011] (4) adding an initiator to the acidic mixed solution to obtain an initiator system to cause a double bond free radical reaction, and reacting at 30-80° C. for 2-15 hours;

[0012] (5) mixing the initiator solution and the dialdehyde solution obtained in step (4) to continue the reaction, and cleaning the sponge after the reaction to obtain a polyvinyl acetal composite sponge with antibacterial function.

[0013] Furthermore, the mass ratio of the unsaturated monomer containing hydroxyl group to the monomer having antibacterial function is 1-3:3-13.

[0014] Furthermore, the mass ratio of the total mass of the unsaturated monomer containing hydroxyl group and the monomer having antibacterial function to water is 0.2-6g:20-200g;

[0015] Furthermore, the mass ratio of the total mass of the unsaturated monomer containing hydroxyl group and the monomer having antibacterial function to the mass ratio of the polyvinyl acetal sponge is 0.2-1:1;

[0016] Further, the acidic solution is an acidic solution with a pH of 2-6;

[0017] Furthermore, the mass ratio of the initiator to the total mass of the unsaturated monomer containing a hydroxyl group and the monomer having an antibacterial function is 0.0005-0.01:1;

[0018] Furthermore, the mass ratio of the dialdehyde solution to the aqueous solution is 0.01-0.05:1.

[0019] Furthermore, the unsaturated monomer containing a hydroxyl group is one or more of 3-butene-1-ol, hydroxyethyl acrylate, 3-methyl-3-butene-1-ol, 1,4-butynediol, 2-methyl-3-butene-2-ol, and N-(2-hydroxypropyl)methacrylamide.

[0020] Furthermore, the monomer with antibacterial function is one or more of 4-acryloylmorpholine, methacryloyloxyethylbenzyldimethylammonium chloride, allyltrimethylammonium chloride, (3-acrylamidopropyl)trimethylammonium chloride, and 2-acrylamido-2-methylpropanesulfonic acid.

[0021] Furthermore, the substance for adjusting the acidity is sulfuric acid, hydrochloric acid or sodium hydroxide. The pH of the solution is adjusted to 2-6.

[0022] Furthermore, the initiator is one or more of potassium persulfate, sodium bisulfite, ammonium persulfate or azobisisobutylamidine hydrochloride.

[0023] Furthermore, the dialdehyde solution is one or more of glyoxal, succinaldehyde, and glutaraldehyde.

[0024] Furthermore, the reaction temperature after adding the dialdehyde solution is 50-70°C.

[0025] Furthermore, the reaction time after adding the dialdehyde solution is 5-60 minutes.

[0026] According to the above method, a polyvinyl acetal composite sponge with antibacterial function is prepared.

[0027] The present invention introduces a substance with antibacterial function into the polyvinyl acetal sponge through acetal reaction and free radical polymerization reaction, and prepares the polyvinyl acetal sponge with antibacterial property, which solves the technical problems that the current polyvinyl alcohol sponge does not have antibacterial property, the operation is complicated and the preparation cycle is long during the antibacterial modification process, and the original excellent performance and three-dimensional structure of the sponge are affected, resulting in the sponge being unable to better meet application requirements. The present invention brings about a technical effect with excellent performance, simple and easy preparation method, good antibacterial effect, short preparation cycle, simple and controllable conditions, and is expected to achieve large-scale production.

[0028] Compared with the prior art, the advantages and beneficial technical effects of the present invention are:

[0029] (1) The present invention imparts antibacterial function to the polyvinyl acetal sponge while retaining the three-dimensional porous structure of the sponge, so that the sponge can meet more usage requirements.

[0030] (2) The present invention attaches an antibacterial layer to the polyvinyl acetal sponge substrate by polymerizing the sponge, and then chemically cross-links the antibacterial layer and the sponge by dialdehyde. The sponge prepared by this method can not only effectively ensure the number of antibacterial monomers on the sponge, but also make the connection more stable.

[0031] (3) The sponge prepared by the preparation method of the present invention grafts antibacterial materials into the sponge structure while maintaining the original excellent properties of the polyvinyl acetal sponge. Since the antibacterial monomer has polar groups, the water absorption speed of the sponge is greatly improved.

[0032] (4) The preparation process of the sponge of the present invention has the advantages of mild reaction conditions, short operation time, simple and feasible method, etc., and therefore it is expected to achieve large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1This is a mechanical property diagram of the cyclic compression test of the antibacterial polyvinyl formal composite sponge prepared in Example 1 in a swollen state.

[0034] Figure 2 This is a mechanical property diagram of a cyclic compression test of the antibacterial polyvinyl acetal composite sponge prepared in Example 6 in a swollen state.

[0035] Figure 3 This is a dynamic diagram of surface water penetration of the antibacterial polyvinyl formal composite sponge prepared in Example 5.

[0036] Figure 4 The following are scanning electron microscope photos of the external morphology of the sponge before modification, and the polyvinyl formal sponge of Example 1, Example 2, and Example 5. DETAILED DESCRIPTION

[0037] The preferred embodiments of the present invention are described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.

[0038] Example 1

[0039] (1) Dissolve 0.05 g of 3-butene-1-ol and 0.15 g of allyltrimethylammonium chloride in 20 mL of distilled water;

[0040] (2) adding 1 g of polyvinyl formal sponge to the mixed solution;

[0041] (3) adjusting the mixed solution to a pH of 5 using sulfuric acid;

[0042] (4) Add 0.002 g of ammonium persulfate to the acidic mixed solution and react at 80°C for 2 h;

[0043] (5) The initiator solution obtained in step (4) and 1 g of glutaraldehyde solution are mixed and reacted at 50° C. for 5 min. The sponge after the reaction is cleaned to obtain a polyvinyl formal composite sponge with antibacterial function.

[0044] According to GB / T 20944.3-2008 "Evaluation of Antibacterial Properties of Textiles", the antibacterial properties were tested by oscillation method. The test showed that the antibacterial rate of the polyvinyl formal composite sponge against Escherichia coli and Staphylococcus aureus was above 72%.

[0045] Figure 1The 5-cycle compression curve of the polyvinyl formal sponge grafted with antibacterial substance prepared in Example 1 in a swollen state under 60% deformation compression shows that when the strain of the modified sponge reaches 60%, the sample stress is 19.4 KPa, and after 5 cycles, the stress remains basically unchanged, indicating that the material has excellent mechanical properties and fatigue resistance.

[0046] Example 2

[0047] (1) Dissolve 0.08 g of hydroxyethyl acrylate and 0.32 g of 4-acryloylmorpholine in 50 mL of distilled water;

[0048] (2) adding 1.5 g of polyvinyl formal sponge to the mixed solution;

[0049] (3) adjusting the pH of the mixed solution to 6 with sodium hydroxide;

[0050] (4) Add 0.0002 g of initiator potassium persulfate and 0.0002 g of initiator sodium bisulfite to the acidic mixed solution and react at 30° C. for 3 h;

[0051] (5) The initiator solution obtained in step (4) and 1.5 g of succinaldehyde solution were mixed and reacted at 55° C. for 20 min. The sponge after the reaction was cleaned to obtain a polyvinyl formal composite sponge with antibacterial function.

[0052] According to GB / T 20944.3-2008 "Evaluation of Antibacterial Properties of Textiles" standard, the antibacterial properties were tested by oscillation method. After testing, it was found that the antibacterial rate of the polyvinyl formal composite sponge against Escherichia coli and Staphylococcus aureus was above 87%.

[0053] Example 3

[0054] (1) Dissolve 0.12 g of hydroxyethyl acrylate and 0.78 g of methacryloyloxyethyl benzyl dimethyl ammonium chloride monomer in 100 mL of distilled water;

[0055] (2) adding 3 g of polyvinyl propionaldehyde sponge to the mixed solution;

[0056] (3) adjusting the mixed solution to a pH of 5.6 using sodium hydroxide;

[0057] (4) adding potassium persulfate as an initiator to the acidic mixed solution and reacting at 50° C. for 7 h;

[0058] (5) The initiator solution obtained in step (4) and 0.48 g of succinaldehyde solution were mixed at 60° C. and the reaction was continued for 60 min. The sponge after the reaction was cleaned to obtain a polyvinyl acetal composite sponge with antibacterial function.

[0059] According to GB / T 20944.3-2008 "Evaluation of Antibacterial Properties of Textiles", the antibacterial properties were tested by oscillation method. The test showed that the antibacterial rate of the polyvinyl alcohol propionaldehyde composite sponge against Escherichia coli and Staphylococcus aureus was above 95%.

[0060] Example 4

[0061] (1) Dissolve 0.9 g of 2-methyl-3-butene-2-ol and 3.92 g of (3-acrylamidopropyl)trimethylammonium chloride in 100 mL of distilled water;

[0062] (2) adding 5 g of polyvinyl butyral sponge to the mixed solution;

[0063] (3) adjusting the mixed solution to a pH of 6 using sodium hydroxide;

[0064] (4) Add 0.0156 g of potassium persulfate as an initiator to the acidic mixed solution and react at 65° C. for 5 h;

[0065] (5) The initiator solution obtained in step (4) and 1.0 g of glyoxal solution were mixed and reacted at 55° C. for 60 min. The sponge after the reaction was cleaned to obtain a polyvinyl butyral composite sponge with antibacterial function.

[0066] According to GB / T 20944.3-2008 "Evaluation of Antibacterial Properties of Textiles" standard, the antibacterial properties were tested by oscillation method. After testing, it was found that the antibacterial rate of the polyvinyl butyral composite sponge against Escherichia coli and Staphylococcus aureus was above 99%.

[0067] Example 5

[0068] (1) Dissolve 1.5 g of 3-methyl-3-butene-1-ol and 4 g of 2-acrylamido-2-methylpropanesulfonic acid monomer in 200 mL of distilled water;

[0069] (2) adding 6 g of polyvinyl formal sponge to the mixed solution;

[0070] (3) adjusting the mixed solution to a pH of 4.0 with sodium hydroxide;

[0071] (4) Add 0.055 g of initiator potassium persulfate to the acidic mixed solution and react at 50° C. for 3 h;

[0072] (5) The initiator solution obtained in step (4) and 3 g of glutaraldehyde solution were mixed and reacted at 60° C. for 50 min. The sponge after the reaction was cleaned to obtain a polyvinyl formal composite sponge with antibacterial function.

[0073] According to GB / T 20944.3-2008 "Evaluation of Antibacterial Properties of Textiles" standard, the antibacterial properties were tested by oscillation method. After testing, it was found that the antibacterial rate of the polyvinyl formal composite sponge against Escherichia coli and Staphylococcus aureus was above 99%.

[0074] Figure 3 This is a dynamic diagram of surface water penetration of the polyvinyl formal composite sponge with antibacterial function prepared in Example 5. It can be seen that the water penetration rate on the sponge surface is very fast, taking only 2 seconds.

[0075] Example 6

[0076] (1) 1.43 g of N-(2-hydroxypropyl)methacrylamide, 3.11 g of 2-acrylamido-2-methylpropanesulfonic acid and 1.46 g of allyltrimethylammonium chloride were dissolved in 200 mL of aqueous solution;

[0077] (2) adding 6 g of polyvinyl acetal sponge to the mixed solution;

[0078] (3) adjusting the mixed solution to a pH of 2 with hydrochloric acid;

[0079] (4) Add 0.024 g of initiator azobisisobutylamidine dihydrochloride to the acidic mixed solution and react at 55° C. for 15 h;

[0080] (5) The initiator solution obtained in step (4) and 8 g of glutaraldehyde solution were mixed and reacted at 70° C. for 40 min. The sponge after the reaction was cleaned to obtain a polyvinyl acetal composite sponge with antibacterial function.

[0081] According to GB / T 20944.3-2008 "Evaluation of Antibacterial Properties of Textiles", the antibacterial properties were tested by oscillation method. The test showed that the antibacterial rate of the polyvinyl acetal composite sponge against Escherichia coli and Staphylococcus aureus was above 99.9%.

[0082] Figure 2 This is the 5-cycle compression curve of the polyvinyl acetal composite sponge with antibacterial function prepared in Example 6 in a swollen state under 60% deformation compression. It can be seen from the figure that when the strain of the modified sponge reaches 60%, the sample stress is 74Kpa, and after 5 cycles, the stress remains basically unchanged, indicating that the material has excellent mechanical properties and fatigue resistance.

[0083] Figure 4The external morphology scanning electron microscope photos of the polyvinyl alcohol formal sponge before modification, and the polyvinyl alcohol formal composite sponge prepared in Example 1, Example 2 and Example 5. It can be seen that although the pore size of the sponge after surface modification is increased, all samples have similar pore structure and surface morphology to the blank sponge, indicating that the modified sponge still retains the three-dimensional network structure and high porosity of the original sponge, and the sponge still has excellent morphology.

[0084] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. It is feasible for those skilled in the art to make further improvements and modifications without departing from the working principle of the present invention, and these improvements and modifications should also be included in the scope of the present invention.

Claims

1. A method for preparing a polyvinyl acetal composite sponge with antibacterial function, comprising the following steps: (1) dissolving an unsaturated monomer containing a hydroxyl group and a monomer having an antibacterial function in an aqueous solution; the unsaturated monomer containing a hydroxyl group is one or more of 3-butene-1-ol, hydroxyethyl acrylate, 3-methyl-3-butene-1-ol, 1,4-butynediol, 2-methyl-3-butene-2-ol, and N-(2-hydroxypropyl)methacrylamide; the monomer having an antibacterial function is one or more of 4-acryloylmorpholine, methacryloyloxyethylbenzyldimethylammonium chloride, allyltrimethylammonium chloride, (3-acrylamidopropyl)trimethylammonium chloride, and 2-acrylamido-2-methylpropanesulfonic acid; (2) adding polyvinyl acetal sponge to the mixed solution; (3) adjusting the mixed solution to be acidic; (4) adding an initiator to the acidic mixed solution to obtain an initiator system to cause a double bond free radical reaction, and reacting at 30-80° C. for 2-15 hours; (5) mixing the initiator solution and the dialdehyde solution obtained in step (4) to continue the reaction, and cleaning the sponge after the reaction to obtain a polyvinyl acetal composite sponge with antibacterial function.

2. The method for preparing the polyvinyl acetal composite sponge with antibacterial function according to claim 1, characterized in that: The mass ratio of the unsaturated monomer containing hydroxyl group to the monomer having antibacterial function is 1-3:3-13; The mass ratio of the total mass of the unsaturated monomer containing hydroxyl group and the monomer having antibacterial function to water is 0.2-6g:20-200g; The mass ratio of the total mass of the unsaturated monomer containing hydroxyl group and the monomer having antibacterial function to the mass ratio of the polyvinyl acetal sponge is 0.2-1:1; The mass ratio of the initiator to the total mass of the unsaturated monomer containing a hydroxyl group and the monomer having an antibacterial function is 0.0005-0.01:1; The mass ratio of the dialdehyde solution to the aqueous solution is 0.01-0.05:

1.

3. The method for preparing the polyvinyl acetal composite sponge with antibacterial function according to claim 1, characterized in that: The substance used for adjusting pH is hydrochloric acid, sulfuric acid or sodium hydroxide, and the pH of the solution is adjusted to 2-6.

4. The method for preparing the polyvinyl acetal composite sponge with antibacterial function according to claim 1, characterized in that: The initiator is one or more of potassium persulfate, sodium sulfite, ammonium persulfate or azobisisobutylamidine hydrochloride.

5. The method for preparing the polyvinyl acetal composite sponge with antibacterial function according to claim 1, characterized in that: The dialdehyde solution is one or more of glyoxal, succinaldehyde and glutaraldehyde.

6. The method for preparing the polyvinyl acetal composite sponge with antibacterial function according to claim 1, characterized in that: The reaction temperature after adding the dialdehyde solution is 50-70°C.

7. The method for preparing the polyvinyl acetal composite sponge with antibacterial function according to claim 1, characterized in that: The reaction time after adding the dialdehyde solution is 5-60 minutes.

8. A polyvinyl acetal composite sponge with antibacterial function prepared by the preparation method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Medical antibacterial sponge dressing and preparation method thereof

    CN101954115A

  • Aziridine cross-linked N-halamine type antibacterial PVA sponge as well as preparation method and application thereof

    CN114106400A

  • Antibacterial material and preparation method and application thereof

    CN110105686A

  • Antibacterial anti-pollution microporous membrane and preparation method thereof

    CN112237853A

  • N-halamine type acrylamide / polyvinyl alcohol based antibacterial hydrogel and preparation method thereof

    CN113896930A