A high temperature and salt resistant coiled tubing drilling fluid and preparation method thereof
Through the continuous oil pipe drilling plug solution formula using polymer suspension stabilizer and other components in high temperature and high salt environment, the problems of perishable deterioration and inability to decompose large bridge plug fragments in the prior art are solved, and the downhole stable operation is achieved and Equipment protection.
Patent Information
- Application Number
- CN202310709339.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing continuous oil pipe drilling plug fluid is prone to rot and deterioration in high temperature and high salt environments, has low carrying capacity, is complex in preparation and use and cannot quickly decompose large blocks of bridge plug fragments, resulting in difficulty in downhole operation and wear of equipment.
Using a formula with tap water as the dispersion medium, including polymer suspension stabilizer, bridge plug decomposition agent, anti-wear drag reducing agent, diluent and defoaming agent, terpolymer is synthesized by solution polycondensation method to form a simple and easy-to-prepared drill. The plug liquid can maintain stable performance under high temperature and high mineralization environment, and has strong bridge plug decomposition capabilities.
The drilling plug fluid maintains stable performance in a high-temperature and high-salt environment, and has strong carrying capacity. It can quickly decompose large blocks of bridge plug fragments, reduce the number of downhole operations, extend the service life of continuous oil pipes, and avoid drilling and equipment wear.
Smart Images

Figure CN116769457B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil and gas well fracturing engineering, and in particular to a high temperature and salt resistant continuous oil pipe drilling fluid and a preparation method thereof. Background Art
[0002] Staged fracturing technology is one of the necessary means for the commercial exploitation of unconventional oil and gas resources such as shale gas, tight gas, and shale oil. After staged fracturing operations, the segmented bridge plugs are retained at the bottom of the well, affecting the production of oil and gas wells. Therefore, the bridge plugs in the wellbore must be removed after fracturing to prevent them from affecting later production. At present, continuous tubing drilling and grinding bridge plugs is a simple operation, the lowest operating cost, and safe and reliable bridge plug removal technology. With the continuous development of horizontal well drilling technology and fracturing technology, the horizontal sections are getting longer and longer, and the number of segments and the number of bridge plugs used are increasing, which brings challenges to post-fracturing drilling and plugging. In order to cope with the complex drilling and plugging conditions downhole, continuous tubing drilling and plugging fluid is particularly important.
[0003] The coiled tubing drilling fluid needs to have the following excellent properties: 1) strong carrying capacity, that is, it can carry out the metal cuttings, bridge plug rubber, proppant and other solid particles in the wellbore out of the wellbore in a complex downhole environment; 2) good resistance reduction effect, that is, high resistance reduction rate and low friction resistance. After being pumped from the wellhead to the target well section, it can also provide effective power for the downhole screw motor to drive the grinding shoe to rotate; 3) good friction reduction effect, that is, it can reduce the friction between the coiled tubing and the drill shoe and the casing to prevent "self-locking"; 4) high temperature and high salt resistance, that is, it can maintain the same performance for a long time in the high temperature and high mineralization environment underground.
[0004] However, the coiled tubing drilling fluid currently used has the following disadvantages: 1) It contains guar gum, xanthan gum and other easily corrupted plant gums (patent CN 105419755A "A coiled tubing drilling fluid system and its preparation method"; Xu Qingxiang et al., Practice and understanding of coiled tubing drilling technology in GD14H well. Drilling and Production Technology, 2019, 42(3): 114-116), which makes the drilling fluid difficult to preserve and requires the addition of fungicides; at the same time, the plant gum can maintain its performance unchanged for less than 3 hours in the complex underground environment of high temperature 60°C and ion concentration 50000 mg / L, and its performance is prone to change, resulting in reduced carrying capacity and easy drilling. 2) The formula is complex, and the preparation and use are complicated, which is not conducive to on-site construction. For example, the already disclosed patent CN 111423865A "coiled tubing drilling fluid and its use method" requires the use of agent A first, and then the mixture of agents A and B, which is easy to cause on-site workers to add the wrong agent. 3) It is not possible to quickly decompose large pieces of bridge plug fragments. The drilling fluid is not easy to bring large pieces of bridge plugs out of the ground. It is necessary to carry large pieces of bridge plug fragments through short-start continuous oil pipes. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art, and to provide a high temperature and salt resistant continuous tubing drilling fluid that overcomes the shortcomings of being prone to corruption, low carrying capacity under high temperature and high mineralization, complex preparation and use, and inability to decompose large pieces of bridge plug fragments. Specifically disclosed is a high temperature and salt resistant continuous tubing drilling fluid and a preparation method; the drilling fluid is composed of: 100 parts by weight of tap water as a dispersion medium, 0.3 to 0.4 parts by weight of a polymer suspension stabilizer, 15 to 25 parts by weight of a bridge plug decomposer, 1 to 2 parts by weight of an anti-wear and drag reducing agent, 0 to 1 parts by weight of a diluent, and 0.1 to 0.2 parts by weight of a defoaming agent. The preparation method is: first completely decompose the solid bridge plug decomposer in tap water, and then slowly add the polymer suspension agent, the anti-wear and drag reducing agent, the diluent, and the defoaming agent in sequence while stirring. The system has a simple formula and is easy to prepare. It has good compatibility with wellbore and formation fluids, can withstand temperatures not lower than 90°C, and is suitable for formation water with a mineralization of at least 1000 mg / L. It has a strong ability to carry bridge plug debris and decompose large bridge plug fragments, and can achieve a bridge plug fragment decomposition rate of more than 3g / h. The use of this system can achieve one-trip drilling and plugging, reduce the number of coiled tubing trips, avoid drill sticking and wear on the coiled tubing, and extend the service life of the coiled tubing.
[0006] In order to achieve the above technical effects, the following technical solutions are adopted:
[0007] A high temperature and salt resistant continuous oil pipe drilling plug fluid, the formula composition is: 100 weight parts of tap water as a dispersion medium, 0.3-0.4 weight parts of a polymer suspension stabilizer, 15-25 weight parts of a bridge plug decomposer, 1-2 weight parts of an anti-wear drag reducer, 0-1 weight parts of a diluent, and 0.1-0.2 weight parts of a defoamer.
[0008] Furthermore, the polymer suspension stabilizer is a terpolymer synthesized by a solution polycondensation method with N,N-dimethylacrylamide, 2-acrylamido-2-methylpropanesulfonic acid, and sodium allyl sulfonate as monomers, deionized water as solvent, a mixed solution of ammonium persulfate and sodium bisulfite as initiator, and sodium hydroxide as pH adjuster.
[0009] Furthermore, the temperature for synthesizing the terpolymer by the solution polycondensation method is 60°C.
[0010] Furthermore, the bridge plug decomposing agent is one or more soluble chloride salts.
[0011] Furthermore, the bridge plug decomposing agent is sodium chloride or potassium chloride or a mixture of the two.
[0012] Furthermore, the anti-wear and drag reducing agent is an oil-in-water emulsion formed by mixing 35 to 55 parts by weight of tap water, 10 to 15 parts by weight of tall oil, 15 to 20 parts by weight of isopropanol, and 20 to 30 parts by weight of modified isomeric tridecanol ether.
[0013] Furthermore, the diluent is a condensation product of formaldehyde and acetone.
[0014] Furthermore, the defoaming agent is one or more of emulsified silicone oil or polyoxypropylene polyether modified silicone.
[0015] A method for preparing a high temperature and salt resistant coiled tubing drilling fluid comprises the following steps:
[0016] Step S1: weighing tap water, polymer suspension stabilizer, bridge plug decomposer, anti-wear drag reducer, diluent, and defoaming agent;
[0017] Step S2: First, add the bridge plug decomposer into tap water and stir until it is completely dissolved, then slowly add the polymer suspension stabilizer, anti-wear drag reducer, diluent, and defoamer in sequence while stirring, and stir evenly to obtain the coiled tubing drilling plug fluid.
[0018] Furthermore, the tap water is 100 parts by weight, the polymer suspension stabilizer is 0.3-0.4 parts by weight, the bridge plug decomposer is 15-25 parts by weight, the anti-wear and drag reducer is 1-2 parts by weight, the diluent is 0-1 parts by weight, and the defoaming agent is 0.1-0.2 parts by weight.
[0019] The beneficial effects of the present invention are:
[0020] 1) The coiled tubing drilling fluid can maintain stable performance in the high-temperature and high-mineralization environment underground, and has a strong ability to carry solid particles such as drill cuttings and rubber, ensuring the one-trip drilling of the coiled tubing;
[0021] 2) Under room temperature conditions, it is stable for a long time without corruption or deterioration;
[0022] 3) Good compatibility with fracturing fluid, formation water, etc., simple and easy operation of on-site operation procedures, low friction coefficient and high drag reduction rate;
[0023] 4) The bridge plug can be decomposed, and the large drill cuttings that cannot be carried by the drill shoe can be decomposed into a portable size. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The present invention is a flow chart of a method for preparing a high temperature and salt resistant coiled tubing drilling fluid according to an embodiment of the present invention. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0026] Embodiment 1:
[0027] Weigh 500g of tap water, 1.5g of polymer suspension stabilizer, 75g of bridge plug decomposer, 5g of anti-wear and drag reducer, 2.5g of diluent, and 0.5g of defoamer. The polymer suspension stabilizer is a terpolymer synthesized at 60°C by solution polycondensation method with N,N-dimethylacrylamide, 2-acrylamido-2-methylpropanesulfonic acid, sodium allyl sulfonate as monomers, deionized water as solvent, ammonium persulfate and sodium bisulfite mixed solution as initiator, and sodium hydroxide as pH regulator; the bridge plug decomposer is sodium chloride; the anti-wear and drag reducer is a water-in-oil emulsion formed by mixing 35g of tap water, 10g of tall oil, 15g of isopropanol, and 20g of modified isomeric tridecanol ether; the diluent is a condensation product of formaldehyde and acetone; and the defoamer is emulsified silicone oil.
[0028] like Figure 1 As shown, the bridge plug decomposer is first added into tap water and stirred until completely decomposed, and then a polymer suspension stabilizer, an anti-wear drag reducer, a diluent, and a defoaming agent are slowly added in sequence while stirring to obtain a continuous tubing drilling plug fluid.
[0029] According to the industry standards "NB / T14003.2-2016 Shale Gas Fracturing Fluid Part 2: Performance Indicators and Test Methods of Drag Reducing Agents" and "GB / T 16783.1-2006 Petroleum and Natural Gas Industry Drilling Fluid Field Test Part 1", the friction coefficient reduction rate, drag reduction rate, apparent viscosity, plastic viscosity, and dynamic shear force of the coiled tubing drilling fluid prepared in Example 1 were tested, and the decomposition rate of the drilling fluid was tested. The test results are shown in Table 1. The drilling fluid aging experiment was conducted at 90°C and then tested at 90°C under normal pressure after hot rolling aging in a roller furnace at 90°C for 5 hours.
[0030] Table 1 Summary of performance tests of coiled tubing drilling fluid prepared in Example 1
[0031]
[0032] From the test results in Table 1, it can be seen that the friction coefficient reduction rate of the drill plug fluid prepared in Example 1 is ≥74.2%, and the drag reduction rate is ≥70.4%. The apparent viscosity evaluates the thickening ability; the dynamic shear force evaluates the ability to form a spatial network structure. The larger the value, the stronger the ability to suspend and carry bridge plug debris. It can be seen that the drill plug fluid prepared in Example 1 has a strong ability to carry drill cuttings. In addition, the decomposition ability of the drill plug fluid to bridge plug fragments is ≥3.1g / h. The performance of the drill plug fluid after aging at 90°C is not much different from that under non-aging conditions, which shows that the drill plug fluid system can remain undamaged in an underground environment at 90°C, and has outstanding anti-aging performance while maintaining excellent friction coefficient reduction rate, drag reduction rate, apparent viscosity, plastic viscosity, dynamic shear force and decomposition rate.
[0033] Example 2
[0034] Weigh 500g of tap water, 2g of polymer suspension stabilizer, 125g of bridge plug decomposer, 10g of anti-wear drag reducer, 5g of diluent, and 1g of defoamer. The polymer suspension stabilizer is a terpolymer synthesized at 60°C by solution polycondensation method with N,N-dimethylacrylamide, 2-acrylamido-2-methylpropanesulfonic acid, sodium allyl sulfonate as monomers, deionized water as solvent, ammonium persulfate and sodium bisulfite mixed solution as initiator, and sodium hydroxide as pH regulator; the bridge plug decomposer is a mixture of sodium chloride and potassium chloride; the anti-wear drag reducer is a water-in-oil emulsion formed by mixing 55g of tap water, 15g of tall oil, 20g of isopropanol, and 30g of modified isomeric tridecanol ether; the diluent is a condensation product of formaldehyde and acetone; and the defoamer is polyoxypropylene polyether modified silicon.
[0035] like Figure 1 As shown, the bridge plug decomposer is first added into tap water and stirred until completely decomposed, and then a polymer suspension stabilizer, an anti-wear drag reducing agent, a diluent, and a defoaming agent are slowly added in sequence while stirring to obtain a continuous tubing drilling plug fluid.
[0036] According to the industry standards "NB / T14003.2-2016 Shale Gas Fracturing Fluid Part 2: Performance Indicators and Test Methods of Drag Reducing Agents" and "GB / T 16783.1-2006 Petroleum and Natural Gas Industry Drilling Fluid Field Test Part 1", the friction coefficient reduction rate, drag reduction rate, apparent viscosity, plastic viscosity, and dynamic shear force of the coiled tubing drilling fluid prepared in Example 2 were tested, and the decomposition rate of the drilling fluid was tested. The test results are shown in Table 2. The drilling fluid aging experiment was actually tested at 93°C and normal pressure after hot rolling aging in a roller furnace at 120°C for 5 hours.
[0037] Table 2 Summary of performance tests of coiled tubing drilling fluid prepared in Example 2
[0038]
[0039] From the test results in Table 2, it can be seen that the friction coefficient reduction rate of the drilling fluid prepared in Example 2 is greater than or equal to 79.4%, and the drag reduction rate is greater than or equal to 79.1%. In addition, the decomposition capacity of the drilling fluid for bridge plug fragments is greater than or equal to 4.0 g / h. The performance of the drilling fluid after aging under 120°C is not much different from the performance under the condition of non-aging of mineralization, which shows that the drilling fluid system can withstand high temperatures while ensuring basic performance and has excellent temperature resistance.
[0040] Example 3
[0041] The drilling fluid prepared in Example 1 was subjected to salt resistance test. 20 g of formation water with salinity of 1000 mg / L and 50000 mg / L was added to the drilling fluid prepared in Example 1 and stirred evenly. The friction coefficient reduction rate, drag reduction rate, apparent viscosity, plastic viscosity, and dynamic shear force were tested at 90°C, and the decomposition rate of the drilling fluid was tested. The test results are shown in Table 3.
[0042] Table 3 Summary of drilling fluid performance tests at different mineralization levels
[0043]
[0044]
[0045] From the test results in Table 3, it can be seen that after adding formation water with different salinities, the friction coefficient reduction rate, drag reduction rate, apparent viscosity, plastic viscosity, dynamic shear force and other properties of the drilling fluid do not change much, while the bridge plug decomposition rate is further enhanced. This shows that the drilling fluid prepared in Example 1 has excellent salt resistance.
[0046] Comparative Example 1
[0047] The preparation method of Comparative Example 1 is the same as that of Example 1, except that 1.5 g of the polymer suspension stabilizer is removed and the drilling fluid is prepared according to the preparation method of Example 1 to obtain the drilling fluid.
[0048] According to the industry standards "NB / T14003.2-2016 Shale Gas Fracturing Fluid Part 2: Performance Indicators and Test Methods of Drag Reducing Agents" and "GB / T 16783.1-2006 Petroleum and Natural Gas Industry Drilling Fluid Field Test Part 1", the friction coefficient reduction rate, drag reduction rate, apparent viscosity, plastic viscosity, and dynamic shear force of the coiled tubing drilling fluid prepared in Comparative Example 1 were tested, and the decomposition rate of the drilling fluid was tested. The test results are shown in Table 4. The drilling fluid aging experiment was conducted at 90°C and then tested at 90°C under normal pressure after hot rolling aging in a roller furnace at 90°C for 5 hours.
[0049] Table 4 Summary of performance tests of coiled tubing drilling fluid prepared in comparative example 1
[0050]
[0051]
[0052] From the test results in Table 4, it can be seen that the friction coefficient reduction rate of the drill plug fluid prepared in Comparative Example 1 is less than 70%, and there is almost no drag reduction effect, while the apparent viscosity and plastic viscosity of the drill plug fluid are very low, and the dynamic shear force is 0. Such a drill plug fluid is difficult to suspend drill cuttings and other solids in the wellbore. It can be seen that the polymer suspension stabilizer has a good effect on reducing the friction coefficient, reducing drag and suspending.
[0053] Comparative Example 2
[0054] The preparation method of Comparative Example 2 is consistent with that of Example 1, except that after removing 75 g of the bridge plug decomposer, the drilling fluid is prepared according to the preparation method of Example 1 to obtain the drilling fluid.
[0055] According to the industry standards "NB / T14003.2-2016 Shale Gas Fracturing Fluid Part 2: Performance Indicators and Test Methods of Drag Reducing Agents" and "GB / T 16783.1-2006 Field Test of Drilling Fluids in Petroleum and Natural Gas Industry Part 1", the friction coefficient reduction rate, drag reduction rate, apparent viscosity, plastic viscosity, and dynamic shear force of the coiled tubing drilling fluid prepared in Comparative Example 2 were tested, and the decomposition rate of the drilling fluid was tested. The test results are shown in Table 5. The drilling fluid aging experiment was conducted at 90°C and then at 90°C under normal pressure after hot rolling aging in a roller furnace at 90°C for 5 hours.
[0056] Table 5 Summary of performance tests of coiled tubing drilling fluid prepared in comparative example 2
[0057]
[0058]
[0059] It can be seen from the test results in Table 5 that the drilling fluid prepared in Comparative Example 2 has almost no changes in parameters such as friction coefficient reduction rate, drag reduction rate, apparent viscosity, plastic viscosity, dynamic shear force, etc. compared with Example 1; however, the decomposition rate of the bridge plug is 0 g / h, that is, the drilling fluid has no ability to decompose bridge plug fragments without adding a bridge plug decomposing agent.
[0060] Comparative Example 3
[0061] The preparation method of Comparative Example 3 is consistent with that of Example 1, except that 5 g of the anti-wear and drag reducing agent is removed and then the drilling fluid is prepared according to the preparation method of Example 1 to obtain the drilling fluid.
[0062] According to the industry standards "NB / T14003.2-2016 Shale Gas Fracturing Fluid Part 2: Performance Indicators and Test Methods of Drag Reducing Agents" and "GB / T 16783.1-2006 Petroleum and Natural Gas Industry Drilling Fluid Field Test Part 1", the friction coefficient reduction rate, drag reduction rate, apparent viscosity, plastic viscosity, and dynamic shear force of the coiled tubing drilling fluid prepared in Comparative Example 3 were tested, and the decomposition rate of the drilling fluid was tested. The test results are shown in Table 6. The drilling fluid aging experiment was conducted at 90°C and then tested at 90°C under normal pressure after hot rolling aging in a roller furnace at 90°C for 5 hours.
[0063] Table 6 Summary of performance tests of coiled tubing drilling fluid prepared in comparative example 3
[0064]
[0065]
[0066] From the test results in Table 6, it can be seen that the friction coefficient of the drilling fluid prepared in Comparative Example 3 is reduced by less than 30% compared with that in Example 1, while other parameters are not significantly affected. This shows that the anti-wear and drag reducing agent can greatly reduce the friction coefficient and reduce the friction between the coiled tubing and the casing.
[0067] Comparative Example 4
[0068] The preparation method of Comparative Example 4 is consistent with that of Example 1, except that after removing 2.5 g of the diluent, the drilling fluid is prepared according to the preparation method of Example 1 to obtain the drilling fluid.
[0069] According to the industry standards "NB / T14003.2-2016 Shale Gas Fracturing Fluid Part 2: Performance Indicators and Test Methods of Drag Reducing Agents" and "GB / T 16783.1-2006 Field Test of Drilling Fluids in Petroleum and Natural Gas Industry Part 1", the friction coefficient reduction rate, drag reduction rate, apparent viscosity, plastic viscosity, and dynamic shear force of the coiled tubing drilling fluid prepared in Comparative Example 4 were tested, and the decomposition rate of the drilling fluid was tested. The test results are shown in Table 7. The drilling fluid aging experiment was conducted at 90°C and then tested at 90°C under normal pressure after hot rolling aging in a roller furnace at 90°C for 5 hours.
[0070] Table 7 Summary of performance tests of coiled tubing drilling fluid prepared in comparative example 4
[0071]
[0072]
[0073] It can be seen from the test results in Table 7 that the friction coefficient reduction rate and bridge plug fragment decomposition rate of the drilling fluid prepared in Comparative Example 4 are not significantly changed compared with those in Example 1, but the drag reduction rate and suspension capacity of the drilling fluid are greatly affected.
[0074] Comparative Example 5
[0075] The preparation method of Comparative Example 5 is the same as that of Example 1, except that 0.5 g of the defoaming agent is removed and the drilling fluid is prepared according to the preparation method of Example 1 to obtain the drilling fluid.
[0076] According to the industry standards "NB / T14003.2-2016 Shale Gas Fracturing Fluid Part 2: Performance Indicators and Test Methods of Drag Reducing Agents" and "GB / T 16783.1-2006 Petroleum and Natural Gas Industry Drilling Fluid Field Test Part 1", the friction coefficient reduction rate, drag reduction rate, apparent viscosity, plastic viscosity, and dynamic shear force of the coiled tubing drilling fluid prepared in Comparative Example 5 were tested, and the decomposition rate of the drilling fluid was tested. The test results are shown in Table 8. The drilling fluid aging experiment was conducted at 90°C and then tested at 90°C under normal pressure after hot rolling aging in a roller furnace at 90°C for 5 hours.
[0077] Table 8 Summary of performance tests of coiled tubing drilling fluid prepared in comparative example 5
[0078]
[0079]
[0080] It can be seen from the test results in Table 8 that the friction coefficient reduction rate of the drill plug fluid prepared in Comparative Example 5 is not much different from that in Example 1, but the drag reduction rate and the ability to decompose bridge plug fragments are reduced, and the apparent viscosity, plastic viscosity and dynamic shear force are increased, indicating that the suspension ability is increased.
[0081] In summary, the present invention discloses a high temperature and salt resistant continuous tubing drilling fluid and a preparation method; the drilling fluid is composed of: 100 parts by weight of tap water as a dispersion medium, 0.3-0.4 parts by weight of a polymer suspension stabilizer, 15-25 parts by weight of a bridge plug decomposer, 1-2 parts by weight of an anti-wear and drag reducer, 0-1 parts by weight of a diluent, and 0.1-0.2 parts by weight of a defoamer. The preparation method is: first completely decompose the solid bridge plug decomposer in tap water, and then slowly add the polymer suspension, anti-wear and drag reducer, diluent, and defoamer in sequence while stirring. The system has a simple formula and is easy to prepare. It has good compatibility with wellbore and formation fluids, can withstand temperatures not lower than 90°C, is adaptable to formation water with a mineralization of at least 1000 mg / L, has a strong ability to carry bridge plug debris, has a strong ability to decompose bridge plugs, and can achieve a bridge plug fragment decomposition rate of more than 3g / h. The use of this system can achieve one-trip drilling and plugging, reduce the number of times the coiled tubing is tripped, avoid drill sticking and wear on the coiled tubing, and extend the service life of the coiled tubing.
[0082] At this point, those skilled in the art recognize that, although the embodiments of the present invention have been shown and described in detail herein, many other variations or modifications that conform to the principles of the present invention can still be directly determined or derived based on the contents disclosed in the present invention without departing from the spirit and scope of the present invention. Therefore, the scope of the present invention should be understood and recognized as covering all such other variations or modifications.
Claims
1. A high temperature and salt resistant coiled tubing drilling fluid, characterized in that: The formula of the high temperature and salt resistance coiled tubing drilling plug fluid is as follows: 100 parts by weight of tap water as a dispersion medium, 0.3-0.4 parts by weight of a polymer suspension stabilizer, 15-25 parts by weight of a bridge plug decomposer, 1-2 parts by weight of an anti-wear drag reducer, 0-1 parts by weight of a diluent, and 0.1-0.2 parts by weight of a defoamer; The polymer suspension stabilizer is a terpolymer synthesized by a solution polycondensation method using N,N-dimethylacrylamide, 2-acrylamido-2-methylpropanesulfonic acid, and sodium allylsulfonate as monomers, deionized water as a solvent, a mixed solution of ammonium persulfate and sodium bisulfite as an initiator, and sodium hydroxide as a pH regulator; The temperature for synthesizing the terpolymer by the solution polycondensation method is 60°C; The bridge plug decomposing agent is one of sodium chloride or potassium chloride or a mixture of the two; The anti-wear and drag reducing agent is an oil-in-water emulsion formed by mixing 35 to 55 parts by weight of tap water, 10 to 15 parts by weight of tall oil, 15 to 20 parts by weight of isopropanol, and 20 to 30 parts by weight of modified isomeric tridecanol ether; The diluent is a condensation product of formaldehyde and acetone; The defoaming agent is one or more of emulsified silicone oil or polyoxypropylene polyether modified silicone.
2. A method for preparing a high temperature and salt resistant coiled tubing drilling fluid as claimed in claim 1, characterized in that: The preparation method comprises the following steps: Step S1: weighing tap water, polymer suspension stabilizer, bridge plug decomposer, anti-wear drag reducer, diluent, and defoaming agent; Step S2: First, add the bridge plug decomposer into tap water and stir until it is completely dissolved, then slowly add the polymer suspension stabilizer, anti-wear drag reducer, diluent, and defoamer in sequence while stirring, and stir evenly to obtain the coiled tubing drilling plug fluid.