Composite electrode sheet and preparation method thereof, lithium ion battery

The composite electrode sheet was prepared by dry process, and the synergistic effect of polyvinylidene fluoride and BaTiO3-Li0.33La0.56TiO3 was solved, and the problem of time and cost of solid electrolyte membrane preparation in traditional wet process was achieved, thus achieving high efficiency Lithium-ion battery battery performance improvement and environmentally friendly production process.

CN117117101BActive Publication Date: 2024-12-06SUZHOU QINGTAO NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311376600.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-24
Publication Date
2024-12-06
Estimated Expiration
2043-10-24

AI Technical Summary

Technical Problem

The traditional wet process takes a long time to prepare solid electrolyte membranes, is expensive to dry, is high in production, and is difficult to solve the problems of solvent recovery and compatibility, which affects the safety performance and battery circulation performance of lithium-ion batteries.

Method used

Polyvinylidene fluoride and BaTiO3-Li0.33La0.56TiO3 were premixed by dry process, and fibrosis was performed under high shear force. Polytetrafluoroethylene was added to form a solid electrolyte film by rolling pressure, and the electrode film was added. Recombination under dry heat conditions to form a composite electrode sheet with high mechanical strength and high ionic conductivity.

Benefits of technology

It significantly improves the ionic conductivity and battery cycling performance of lithium-ion batteries, extends the service life of the battery, and avoids environmental protection and compatibility problems caused by solvent use, reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117117101B_ABST
    Figure CN117117101B_ABST
Patent Text Reader

Abstract

The present application relates to a composite electrode sheet and a preparation method thereof, and a lithium-ion battery. The preparation method comprises: 0.33 La 0.56 TiO3 is pre-mixed to obtain a mixture; polytetrafluoroethylene is added to the mixture and subjected to fiberization treatment to obtain a fiberized mixture; the fiberized mixture is subjected to roller pressing to obtain a solid electrolyte membrane; an electrode membrane is prepared; the solid electrolyte membrane and the electrode membrane are dry-compounded at a temperature of 60°C-160°C to obtain a composite electrode plate. BaTiO3-Li 0.33 La 0.56 The addition of TiO3 and polyvinylidene fluoride alleviates the instability of PTFE alone as a binder, resulting in a solid electrolyte membrane with good mechanical strength and high ionic conductivity. In addition, due to the addition of PVDF, the mechanical strength of the composite of the solid electrolyte membrane and the electrode plate is even greater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of composite electrode plate materials, and in particular to a composite electrode plate and a preparation method thereof, and a lithium-ion battery. Background Art

[0002] In order to overcome the shortcomings of the traditional wet process for preparing solid electrolyte membranes, such as long time consumption, expensive drying process and high production cost, people have gradually developed dry preparation processes. The current dry preparation process often uses solid electrolyte materials and polytetrafluoroethylene (PTFE) binder to fiberize and calender to form a solid electrolyte membrane prepared by dry method.

[0003] In lithium-ion batteries, in order to improve the safety performance of the battery, it is a known method to set a layer of solid electrolyte membrane on the surface of the positive electrode or negative electrode layer. However, the solid electrolyte membrane is usually set on the surface of the electrode layer by wet coating. This wet process faces the same problems as the traditional electrode wet process, such as solvent recovery and environmental protection, compatibility of solid electrolyte membrane with solvent, etc. Therefore, how to learn from the dry process and compound the electrode membrane and the solid electrolyte membrane by rolling under solvent-free conditions is a new technology with broad application prospects. Summary of the invention

[0004] Based on this, in order to solve the above problems, the present application provides a composite electrode plate and a preparation method thereof, and a lithium-ion battery to solve the above technical problems.

[0005] The first aspect of the present application provides a method for preparing a composite electrode sheet, comprising the following steps:

[0006] S1. Preparation of solid electrolyte membrane:

[0007] S1-1, polyvinylidene fluoride, BaTiO3-Li 0.33 La 0.56 TiO3 is premixed to obtain a mixed material;

[0008] S1-2, adding polytetrafluoroethylene to the mixture and performing fiberization treatment to obtain a fiberized mixture;

[0009] S1-3, rolling the fiberized mixture to obtain a solid electrolyte membrane;

[0010] S2, preparing electrode film;

[0011] S3, dry-compounding the solid electrolyte membrane prepared in step S1 and the electrode membrane prepared in step S2 at a temperature of 60° C. to 160° C.;

[0012] S4, obtaining a composite electrode plate.

[0013] In some embodiments, in step S1-1 of preparing the mixture, the premixing treatment is performed by at least one of ball milling, air flow mixing, and pulverizer.

[0014] In some embodiments, in step S1-2 of preparing the fiberized mixture, a high-speed shearing machine is used to perform fiberization treatment at a rotation speed of 20,000 r / min to 28,000 r / min.

[0015] In some embodiments, in the step of preparing the solid electrolyte membrane, a double-roll device is used to perform a hot rolling process on the fiberized mixture.

[0016] In some embodiments, the solid electrolyte membrane further includes a lithium salt in terms of mass percent.

[0017] In some embodiments, the solid electrolyte membrane includes 70% to 97% BaTiO3-Li 0.33 La 0.56 TiO3, 0.1%~3% polyvinylidene fluoride, 1%~15% polytetrafluoroethylene and 1%-15% lithium salt.

[0018] In some embodiments, the preparation method further comprises preparing BaTiO3-Li 0.33 La 0.56 TiO3 step, including BaTiO3 and Li 0.33 La 0.56 TiO3 is ball-milled, dried, pressed and calcined.

[0019] In some embodiments, step S2 comprises the following steps:

[0020] S2-1, mixing the active material, the conductive agent and the binder to prepare a mixture;

[0021] S2-2, subjecting the mixture to fiberization treatment to obtain a fiberized mixture;

[0022] S2-3, calendering the fiberized mixture to obtain an electrode membrane.

[0023] The second aspect of the present application provides a composite electrode plate, which is prepared according to the preparation method provided in the first aspect.

[0024] A third aspect of the present application provides a lithium-ion battery, which includes a composite electrode sheet prepared according to the preparation method provided in the first aspect.

[0025] This application aims at BaTiO3-Li 0.33 La0.56 The synergistic effect of TiO3 material and polyvinylidene fluoride (PVDF) in the solid electrolyte membrane uses fiberized polytetrafluoroethylene (PTFE) to provide mechanical properties. BaTiO3-Li is added in the traditional dry preparation process. 0.33 La 0.56 TiO3 and polyvinylidene fluoride (PVDF), due to BaTiO3-Li 0.33 La 0.56 TiO3 has good ion transport capacity and can significantly improve ion conductivity. At the same time, it has a high dielectric constant and can polarize and dissociate lithium salts under the action of an external electric field, producing more free lithium ions for transmission, overcoming the problem of reduced ion conductivity due to the low dielectric constant of the electrolyte and the low degree of dissociation of lithium salts. In addition, the addition of PVDF, which also has a high dielectric constant, can further promote the ionization of lithium salts, which is a good choice for BaTiO3-Li 0.33 La 0.56 TiO3 provides more free lithium ions for transmission; on the other hand, the addition of PVDF can also improve the overall mechanical properties of the solid electrolyte membrane, which is beneficial to ensure the ability of the solid electrolyte membrane to resist the deformation of the battery electrode, thereby extending the cycle performance of the battery. 0.33 La 0.56 The addition of TiO3 and polyvinylidene fluoride (PVDF) also alleviates the instability of PTFE when used alone as a binder, and ultimately obtains a solid electrolyte membrane with good mechanical strength and high ion conductivity. At the same time, since some PVDF is added to the solid electrolyte membrane, the mechanical strength of the solid electrolyte membrane and the electrode plate during the heating and rolling process is greater. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The present invention is a flow chart of a method for preparing a composite electrode sheet in one embodiment of the present application. DETAILED DESCRIPTION

[0027] References to embodiments of the present application will now be provided in detail, one or more embodiments of which are described below. Each embodiment is provided as an explanation rather than a limitation of the present application. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the present application without departing from the scope or spirit of the present application. For example, a feature described or described as part of one embodiment may be used in another embodiment to produce a further embodiment.

[0028] Therefore, it is intended that the present application covers such modifications and variations that fall within the scope of the appended claims and their equivalents. Other objects, features and aspects of the present application are disclosed in or are apparent from the following detailed description. It will be appreciated by those of ordinary skill in the art that this discussion is merely a description of exemplary embodiments and is not intended to limit the broader aspects of the present application.

[0029] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0030] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0031] In this article, when referring to the unit of a data range, if there is a unit only after the right endpoint, it means that the units of the left and right endpoints are the same. For example, 100~150 nm means that the units of the left endpoint "100" and the right endpoint "150" are both nm (nanometers).

[0032] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0033] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0034] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, mentioning that the method may also include step (c) means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0035] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0036] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0037] like Figure 1 As shown, the first aspect of the present application provides a method for preparing a composite electrode sheet, comprising the following steps:

[0038] S1. Preparation of solid electrolyte membrane:

[0039] S1-1: Polyvinylidene fluoride (PVDF), BaTiO3-Li 0.33 La 0.56 TiO3 is premixed to obtain a mixed material;

[0040] S1-2: adding polytetrafluoroethylene (PTFE) to the mixture and performing fiberization treatment to obtain a fiberized mixture;

[0041] S1-3: Roll-pressing the fiberized mixture to obtain a solid electrolyte membrane;

[0042] S2, preparing electrode film;

[0043] S3, dry-compounding the solid electrolyte membrane prepared in step S1 and the electrode membrane prepared in step S2 at a temperature of 60° C. to 160° C.;

[0044] S4, obtaining a composite electrode plate.

[0045] In step S1-1, the premixing treatment includes but is not limited to premixing the materials under the action of low shear force such as ball milling, air flow mixing, and pulverizer. It is understood that any known mixing treatment method can be used in this application without violating the inventive concept of the present application.

[0046] In step S1-2, a high-speed shearing machine is used to perform fiberization treatment at a rotation speed of 20000 r / min to 28000 r / min. Including but not limited to 20000 r / min, 21000 r / min, 22000 r / min, 23000 r / min, 24000 r / min, 25000 r / min, 26000 r / min, 27000 r / min, 28000 r / min. Preferably, a high-speed shearing machine is used to perform fiberization treatment at a rotation speed of 22000 r / min to 26000 r / min. More preferably, a high-speed shearing machine is used to perform fiberization treatment at a rotation speed of 25000 r / min.

[0047] In some embodiments, the fibrosis treatment is performed for 8 min to 15 min, including but not limited to 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, and 15 min. Preferably, the fibrosis treatment is performed for 10 min to 12 min.

[0048] Under the action of high shear force, the polytetrafluoroethylene (PTFE) in the binder is transformed from a powder state to a fibrous state, and is evenly distributed between the particles of other components of the solid electrolyte membrane, thereby forming a fiber network structure, providing the required structural support for the various components in the solid electrolyte membrane, while providing abundant channels for the rapid migration of free lithium ions in the solid electrolyte membrane.

[0049] In step S1-3, the fiberized mixture in step S1-2 may be subjected to hot rolling treatment using a double-roll device to prepare a solid electrolyte membrane.

[0050] In some embodiments, the temperature of the roller device is 60° C.-160° C., including but not limited to 60° C., 70° C., 80° C., 90° C., 100° C., 110° C., 120° C., 130° C., 140° C., 150° C., 160° C. Preferably, the temperature of the roller device is 110° C.-130° C.

[0051] In some embodiments, the solid electrolyte membrane further includes a lithium salt.

[0052] In some embodiments, the lithium salt includes, but is not limited to, one or more of lithium hexafluorophosphate, lithium perchlorate, lithium tetrachloroaluminate, lithium iodide, lithium bromide, lithium thiocyanate, lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium tetraphenylborate, lithium bis(oxalate)borate, lithium tetrafluorooxalatophosphate, lithium nitrate, lithium hexafluoroarsenate, lithium trifluoromethanesulfonate, lithium bis(trifluoromethanesulfonyl imide), and lithium bis(fluorosulfonyl imide).

[0053] In some embodiments, the solid electrolyte membrane includes 70% to 97% BaTiO3-Li 0.33 La 0.56 TiO3, including but not limited to 70%, 75%, 80%, 85%, 90%, 95%, 97%, preferably 80% to 95%.

[0054] In some embodiments, the solid electrolyte membrane includes 0.1% to 3% polyvinylidene fluoride by mass, including but not limited to 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, preferably 0.5% to 1.5%.

[0055] In some embodiments, the solid electrolyte membrane includes 1% to 15% polytetrafluoroethylene by mass, including but not limited to 1%, 3%, 5%, 7%, 9%, 11%, 13%, 15%, preferably 3% to 10%.

[0056] In some embodiments, the solid electrolyte membrane includes 1%-15% lithium salt by mass, including but not limited to 1%, 3%, 5%, 7%, 9%, 11%, 13%, 15%, preferably 3%-5%.

[0057] The polyvinylidene fluoride (PVDF) selected in this application has a high dielectric constant, high temperature resistance, stability and excellent mechanical properties. On the one hand, the high dielectric constant can further promote the ionization of lithium salts and provide more free lithium ions; on the other hand, the addition of PVDF can enhance the overall mechanical properties of the solid electrolyte membrane, which is beneficial to ensure the ability of the solid electrolyte membrane to resist deformation of the battery electrode, thereby extending the cycle performance of the battery.

[0058] Studies have shown that BaTiO3-Li 0.33 La 0.56 The special structure of TiO3 effectively weakens the space charge layer strength between it and the PVDF phase. This coupling effect provides high lithium ion concentration and PVDF phase, BaTiO3-Li 0.33 La 0.56 The interfacial effect of the LLTO phase in TiO3 provides a more efficient ion transport effect, improving the overall ionic conductivity of the solid electrolyte membrane.

[0059] At the same time, since some PVDF is added to the solid electrolyte membrane, the mechanical strength of the solid electrolyte membrane and the electrode plate is greater during the heating and rolling process.

[0060] In some embodiments, the method for preparing the solid electrolyte membrane further comprises preparing BaTiO3-Li 0.33 La0.56 TiO3 step, which includes BaTiO3 and Li 0.33 La 0.56 TiO3 is ball-milled, dried, pressed and calcined.

[0061] Specifically, weigh an appropriate amount of Li 0.33 La 0.56 TiO3 powder and BaTiO3; the weighed materials are added into a ball mill for mixing. After drying, they are molded under a pressure of 500 MPa for 3 min. The sheets are placed on an alumina substrate and calcined in a high-temperature furnace. During the entire calcination process, in order to reduce the loss of lithium, the heating rate is set to 4°C / min and the temperature is kept at 1350°C for 6 h.

[0062] BaTiO3-Li in this application 0.33 La 0.56 BaTiO3 in TiO3 has a high dielectric constant and can undergo polarization and dissociation of lithium salts under the action of an external electric field, generating more free lithium ions for transmission; Li 0.33 La 0.56 TiO3 is a fast ion conductor with ion transport capability, which can significantly improve ion conduction efficiency.

[0063] It is understandable that the solid electrolyte membrane may also include conventional additives. Without violating the inventive concept of the present application, the present application does not specifically limit the types and amounts of conventional additives. Adjustments to the types and amounts of conventional additives based on conventional purposes should be deemed to be within the scope of protection of the present application.

[0064] In some embodiments, step S2 comprises the following steps:

[0065] S2-1, mixing the active material, the conductive agent and the binder to prepare a mixture;

[0066] S2-2, subjecting the mixture to fiberization treatment to obtain a fiberized mixture;

[0067] S2-3, calendering the fiberized mixture to obtain an electrode membrane.

[0068] It can be understood that the active material in the present application can be a positive electrode active material or a negative electrode active material.

[0069] In this application, there is no particular limitation on the types of positive electrode active materials and negative electrode active materials. Any known positive electrode active materials and negative electrode active materials can be applied to this application without violating the inventive concept of this application. The following description of positive electrode active materials and negative electrode active materials is only for illustrative purposes and is not intended to limit the scope of protection.

[0070] In some embodiments, the positive electrode active material is not limited to lithium cobalt oxide (LiCoO2), lithium nickel cobalt manganese oxide (LiNi x Mn y Co 1-x-y O2, referred to as NMC), lithium nickel cobalt aluminum oxide (LiNiCoAlO2, referred to as NCA), lithium manganese oxide (LiMn2O4), lithium manganese iron phosphate (LiMn x Fe 1-x PO4, referred to as LMFP), lithium vanadium phosphate (Li3V2(PO4)3), lithium vanadium phosphate (LiVOPO4), lithium iron phosphate (LiFePO4), lithium titanate (Li2TiO3) and one or more of lithium-rich manganese-based materials.

[0071] In some embodiments, the negative electrode active material includes, but is not limited to, one or more of artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, lithium titanate (Li2TiO3) and tin-based materials.

[0072] In the present application, there is no particular limitation on the type of conductive agent, and any known conductive agent can be applied to the present application without violating the inventive concept of the present application. The following description of the conductive agent is only for illustrative purposes and is not intended to limit the scope of protection.

[0073] In some embodiments, the conductive agent includes, but is not limited to, one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, carbon nanofibers, and graphene.

[0074] In some embodiments, the binder includes polytetrafluoroethylene.

[0075] In step S2-1, the active material, conductive agent and binder can be mixed by ball milling, air flow mixing or pulverizer. In the present application, there is no particular limitation on the mixing method. Any known mixing method can be used in the present application without violating the inventive concept of the present application.

[0076] In step S2-2, the fiberization treatment of the mixed material includes at least one of air flow milling, mechanical stirring, shearing by a shearing machine, mechanical fusion, and twin-screw extrusion.

[0077] Furthermore, in step S2-2, a high-speed shearing machine is used to perform fiberization treatment on the mixture.

[0078] In step S2-3, the fiberized mixture may be calendered using a double-roll device and / or a flat plate device. Further, the fiberized mixture may be hot-calendered using a double-roll device.

[0079] In step S3, the electrode membrane and the solid electrolyte membrane are dry-compounded by an elastic roller. The elastic roller includes a rigid roller and an elastic member, and the elastic member is coated on the outside of the rigid roller. In the process of rolling the electrode membrane and the solid electrolyte by the elastic roller, the elastic member in the elastic roller provides a buffer, so that the solid electrolyte membrane can better cover the electrode membrane.

[0080] In some of the embodiments, in step S3, when the electrode membrane and the solid electrolyte membrane are dry-compounded, a heating process is also included. After heating, the electrode membrane and the solid electrolyte membrane will soften compared to before heating, so that the ductility of the electrode membrane and the solid electrolyte membrane is improved, and the electrode membrane and the solid electrolyte membrane are more tightly bonded, the bonding strength is stronger, and the composite effect is better.

[0081] Specifically, during the dry compounding process, the pressing temperature is 60°C to 160°C, including but not limited to 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, and 160°C.

[0082] This application aims at BaTiO3-Li 0.33 La 0.56 The synergistic effect of TiO3 material and polyvinylidene fluoride (PVDF) in the solid electrolyte membrane uses fiberized polytetrafluoroethylene (PTFE) to provide mechanical properties. BaTiO3-Li is added in the traditional dry preparation process. 0.33 La 0.56 TiO3 and polyvinylidene fluoride (PVDF), due to BaTiO3-Li 0.33 La 0.56 TiO3 has good ion transport capacity and can significantly improve ion conductivity. At the same time, it has a high dielectric constant and can polarize and dissociate lithium salts under the action of an external electric field, producing more free lithium ions for transmission, overcoming the problem of reduced ion conductivity due to the low dielectric constant of the electrolyte and the low degree of dissociation of lithium salts. In addition, the addition of PVDF, which also has a high dielectric constant, can further promote the ionization of lithium salts, which is a good choice for BaTiO3-Li 0.33 La 0.56TiO3 provides more free lithium ions for transmission; on the other hand, the addition of PVDF can also improve the overall mechanical properties of the solid electrolyte membrane, which is beneficial to ensure the ability of the solid electrolyte membrane to resist the deformation of the battery electrode, thereby extending the cycle performance of the battery. 0.33 La 0.56 The addition of TiO3 and polyvinylidene fluoride (PVDF) also alleviates the instability of PTFE when used alone as a binder, and ultimately obtains a solid electrolyte membrane with good mechanical strength and high ion conductivity. At the same time, since some PVDF is added to the solid electrolyte membrane, the mechanical strength of the solid electrolyte membrane and the electrode plate during the heating and rolling process is greater.

[0083] The second aspect of the present application provides a composite electrode plate, which is prepared according to the preparation method provided in the first aspect.

[0084] A third aspect of the present application provides a lithium-ion battery, which includes a composite electrode sheet prepared according to the preparation method provided in the first aspect.

[0085] The present application will be further described below with reference to specific embodiments and comparative examples.

[0086] Example 1

[0087] Preparation of composite positive electrode sheet;

[0088] S1. Preparation of solid electrolyte membrane:

[0089] According to the BaTiO3-Li 0.33 La 0.56 The mass percentages of TiO3, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and lithium salt are 85%, 2%, 10%, and 3%, respectively, and the materials are weighed.

[0090] Polyvinylidene fluoride, BaTiO3-Li 0.33 La 0.56 TiO3 and lithium salt are premixed under low shear force to obtain a mixture.

[0091] Polytetrafluoroethylene was added to the mixture, and the mixture including polytetrafluoroethylene was subjected to fiberization treatment by a high-speed shearing machine at a rotation speed of 25000 r / min for 10 minutes to obtain a fiberized mixture.

[0092] The fiberized mixture is subjected to roller pressing treatment on a double-roll device at a temperature of 120° C. to form a solid electrolyte membrane.

[0093] S2. Preparation of positive electrode film:

[0094] Materials were weighed according to the mass percentages of positive electrode active material lithium manganese oxide, conductive agent Ketjen black, and binder polytetrafluoroethylene in the mixture being 96%, 2%, and 2%, respectively, and mixed by a jet mill to obtain a mixture.

[0095] The mixture was subjected to fiberization treatment by a high-speed shearing machine at a rotation speed of 25000 r / min for 10 minutes to obtain a fiberized mixture.

[0096] The fiberized mixture is subjected to film forming and thinning in sequence to prepare a positive electrode membrane.

[0097] S3, dry-compounding the solid electrolyte membrane prepared in step S1 and the positive electrode membrane prepared in step S2 at a temperature of 60° C.-160° C.

[0098] S4, obtaining a composite positive electrode sheet.

[0099] Preparation of negative electrode sheet:

[0100] Materials were weighed according to the mass percentages of negative electrode active material graphite, conductive agent acetylene black, and binder polytetrafluoroethylene in the mixture being 95%, 2%, and 3%, respectively, and mixed by a jet mill to obtain a mixture.

[0101] The mixture was subjected to fiberization treatment by a high-speed shearing machine at a rotation speed of 25000 r / min for 10 minutes to obtain a fiberized mixture.

[0102] The fiberized mixture is subjected to roll-compounding film formation and thinning in sequence to prepare a negative electrode sheet.

[0103] Preparation of lithium-ion batteries:

[0104] The composite positive electrode sheet, separator and negative electrode sheet are stacked in sequence, rolled and injected with liquid and electrolyte (EC:DMC=1:1vol%) and formed to obtain a lithium-ion battery.

[0105] Example 2

[0106] The difference between Example 2 and Example 1 is that the BaTiO3-Li 0.33 La 0.56 The mass percentages of TiO3, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and lithium salt are different, and the rest are the same.

[0107] S1. Preparation of solid electrolyte membrane:

[0108] According to the BaTiO3-Li 0.33 La 0.56The mass percentages of TiO3, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and lithium salt are 90%, 2%, 6%, and 2%, respectively, and the materials are weighed.

[0109] Polyvinylidene fluoride, BaTiO3-Li 0.33 La 0.56 TiO3 and lithium salt are premixed under low shear force to obtain a mixture.

[0110] Polytetrafluoroethylene was added to the mixture, and the mixture including polytetrafluoroethylene was subjected to fiberization treatment by a high-speed shearing machine at a rotation speed of 25000 r / min for 10 minutes to obtain a fiberized mixture.

[0111] The fiberized mixture is subjected to roller pressing treatment on a double-roll device at a temperature of 120° C. to form a solid electrolyte membrane.

[0112] S2. Preparation of positive electrode film:

[0113] Materials were weighed according to the mass percentages of positive electrode active material lithium manganese oxide, conductive agent Ketjen black, and binder polytetrafluoroethylene in the mixture being 96%, 2%, and 2%, respectively, and mixed by a jet mill to obtain a mixture.

[0114] The mixture was subjected to fiberization treatment by a high-speed shearing machine at a rotation speed of 25000 r / min for 10 minutes to obtain a fiberized mixture.

[0115] The fiberized mixture is subjected to film forming and thinning in sequence to prepare a positive electrode membrane.

[0116] S3, dry-compounding the solid electrolyte membrane prepared in step S1 and the positive electrode membrane prepared in step S2 at a temperature of 60° C.-160° C.

[0117] S4, obtaining a composite positive electrode sheet.

[0118] Preparation of negative electrode sheet:

[0119] Materials were weighed according to the mass percentages of negative electrode active material graphite, conductive agent acetylene black, and binder polytetrafluoroethylene in the mixture being 95%, 2%, and 3%, respectively, and mixed by a jet mill to obtain a mixture.

[0120] The mixture was subjected to fiberization treatment by a high-speed shearing machine at a rotation speed of 25000 r / min for 10 minutes to obtain a fiberized mixture.

[0121] The fiberized mixture is subjected to roll-compounding film formation and thinning in sequence to prepare a negative electrode sheet.

[0122] Preparation of lithium-ion batteries:

[0123] The composite positive electrode sheet, separator and negative electrode sheet are stacked in sequence, rolled and injected with liquid and electrolyte (EC:DMC=1:1vol%) and formed to obtain a lithium-ion battery.

[0124] Example 3

[0125] The difference between Example 3 and Example 1 lies in the preparation of a composite negative electrode sheet.

[0126] Preparation of positive electrode sheet;

[0127] Materials were weighed according to the mass percentages of positive electrode active material lithium manganese oxide, conductive agent Ketjen black, and binder polytetrafluoroethylene in the mixture being 96%, 2%, and 2%, respectively, and mixed by a jet mill to obtain a mixture.

[0128] The mixture was subjected to fiberization treatment by a high-speed shearing machine at a rotation speed of 25000 r / min for 10 minutes to obtain a fiberized mixture.

[0129] The fiberized mixture is subjected to roll-compounding film formation and thinning in sequence to prepare a positive electrode sheet.

[0130] Preparation of composite negative electrode sheet:

[0131] S1. Preparation of solid electrolyte membrane:

[0132] According to the BaTiO3-Li 0.33 La 0.56 The mass percentages of TiO3, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and lithium salt are 90%, 1%, 7%, and 2%, respectively, and the materials are weighed.

[0133] Polyvinylidene fluoride, BaTiO3-Li 0.33 La 0.56 TiO3 and lithium salt are premixed under low shear force to obtain a mixture.

[0134] Polytetrafluoroethylene was added to the mixture, and the mixture including polytetrafluoroethylene was subjected to fiberization treatment by a high-speed shearing machine at a rotation speed of 25000 r / min for 10 minutes to obtain a fiberized mixture.

[0135] The fiberized mixture is subjected to roller pressing treatment on a double-roll device at a temperature of 120° C. to form a solid electrolyte membrane.

[0136] S2. Preparation of negative electrode film:

[0137] Materials were weighed according to the mass percentages of negative electrode active material graphite, conductive agent acetylene black, and binder polytetrafluoroethylene in the mixture being 95%, 2%, and 3%, respectively, and mixed by a jet mill to obtain a mixture.

[0138] The mixture was subjected to fiberization treatment by a high-speed shearing machine at a rotation speed of 25000 r / min for 10 minutes to obtain a fiberized mixture.

[0139] The fiberized mixture is subjected to roll-pressing composite film formation and thinning in sequence to prepare a negative electrode membrane.

[0140] S3, dry-compounding the solid electrolyte membrane prepared in step S1 and the negative electrode membrane prepared in step S2 at a temperature of 60° C.-160° C.

[0141] S4, obtaining a composite negative electrode sheet.

[0142] Preparation of lithium-ion batteries:

[0143] The positive electrode sheet, separator, and composite negative electrode sheet are stacked in sequence, rolled, injected with liquid, electrolyte (EC:DMC=1:1vol%) and formed to produce a lithium-ion battery.

[0144] Comparative Example 1

[0145] The difference between the comparative example 1 and the embodiment 1 is that the solid electrolyte membrane in the comparative example does not contain BaTiO3-Li 0.33 La 0.56 TiO3, only Li added 0.33 La 0.56 TiO3, and the rest are the same.

[0146] According to the Li 0.33 La 0.56 The mass percentages of TiO3, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and lithium salt are 85%, 2%, 10%, and 3%, respectively, and the materials are weighed.

[0147] Polyvinylidene fluoride, Li 0.33 La 0.56 TiO3 and lithium salt are premixed under low shear force to obtain a mixture.

[0148] Polytetrafluoroethylene was added to the mixture, and the mixture including polytetrafluoroethylene was subjected to fiberization treatment by a high-speed shearing machine at a rotation speed of 25000 r / min for 10 minutes to obtain a fiberized mixture.

[0149] The fiberized mixture is subjected to roller pressing treatment on a double-roll device at a temperature of 120° C. to form a solid electrolyte membrane.

[0150] S2. Preparation of positive electrode film:

[0151] Materials were weighed according to the mass percentages of positive electrode active material lithium manganese oxide, conductive agent Ketjen black, and binder polytetrafluoroethylene in the mixture being 96%, 2%, and 2%, respectively, and mixed by a jet mill to obtain a mixture.

[0152] The mixture was subjected to fiberization treatment by a high-speed shearing machine at a rotation speed of 25000 r / min for 10 minutes to obtain a fiberized mixture.

[0153] The fiberized mixture is subjected to film forming and thinning in sequence to prepare a positive electrode membrane.

[0154] S3, dry-compounding the solid electrolyte membrane prepared in step S1 and the positive electrode membrane prepared in step S2 at a temperature of 60° C.-160° C.

[0155] S4, obtaining a composite positive electrode sheet.

[0156] Preparation of negative electrode sheet:

[0157] Materials were weighed according to the mass percentages of negative electrode active material graphite, conductive agent acetylene black, and binder polytetrafluoroethylene in the mixture being 95%, 2%, and 3%, respectively, and mixed by a jet mill to obtain a mixture.

[0158] The mixture was subjected to fiberization treatment by a high-speed shearing machine at a rotation speed of 25000 r / min for 10 minutes to obtain a fiberized mixture.

[0159] The fiberized mixture is subjected to roll-compounding film formation and thinning in sequence to prepare a negative electrode sheet.

[0160] Preparation of lithium-ion batteries:

[0161] The composite positive electrode sheet, separator and negative electrode sheet are stacked in sequence, rolled and injected with liquid and electrolyte (EC:DMC=1:1vol%) and formed to obtain a lithium-ion battery.

[0162] Comparative Example 2

[0163] The difference between Comparative Example 2 and Example 1 is that PVDF is not added to the solid electrolyte membrane in the comparative example, but only PTFE is added, and the rest are the same.

[0164] According to the BaTiO3-Li 0.33 La 0.56The materials were weighed with the mass percentages of TiO3, PTFE and lithium salt being 85%, 12% and 3% respectively.

[0165] PTFE, BaTiO3-Li 0.33 La 0.56 TiO3 and lithium salt are used to fiberize the mixture including polytetrafluoroethylene at a rotation speed of 25000r / min by a high-speed shearing machine for 10 minutes to obtain a fiberized mixture.

[0166] The fiberized mixture is subjected to roller pressing treatment on a double-roll device at a temperature of 120° C. to form a solid electrolyte membrane.

[0167] S2. Preparation of positive electrode film:

[0168] Materials were weighed according to the mass percentages of positive electrode active material lithium manganese oxide, conductive agent Ketjen black, and binder polytetrafluoroethylene in the mixture being 96%, 2%, and 2%, respectively, and mixed by a jet mill to obtain a mixture.

[0169] The mixture was subjected to fiberization treatment by a high-speed shearing machine at a rotation speed of 25000 r / min for 10 minutes to obtain a fiberized mixture.

[0170] The fiberized mixture is subjected to film forming and thinning in sequence to prepare a positive electrode membrane.

[0171] S3, dry-compounding the solid electrolyte membrane prepared in step S1 and the positive electrode membrane prepared in step S2 at a temperature of 60° C.-160° C.

[0172] S4, obtaining a composite positive electrode sheet.

[0173] Preparation of negative electrode sheet:

[0174] Materials were weighed according to the mass percentages of negative electrode active material graphite, conductive agent acetylene black, and binder polytetrafluoroethylene in the mixture being 95%, 2%, and 3%, respectively, and mixed by a jet mill to obtain a mixture.

[0175] The mixture was subjected to fiberization treatment by a high-speed shearing machine at a rotation speed of 25000 r / min for 10 minutes to obtain a fiberized mixture.

[0176] The fiberized mixture is subjected to roll-compounding film formation and thinning in sequence to prepare a negative electrode sheet.

[0177] Preparation of lithium-ion batteries:

[0178] The composite positive electrode sheet, separator and negative electrode sheet are stacked in sequence, rolled and injected with liquid and electrolyte (EC:DMC=1:1vol%) and formed to obtain a lithium-ion battery.

[0179] Test Case

[0180] (1) Cycle test

[0181] At a temperature of 25℃±2℃, the first step is to charge at 1C or the specified current to the final voltage, the cut-off current is 0.05C, and then stand for 30 minutes; the second step is to discharge at 1C to the final discharge voltage (2.75V), record the discharge capacity, and stand for 30 minutes; the first and second steps are cycled to test the cycle performance of the battery for 500 cycles. The results are shown in Table 1 below.

[0182] (2) Peel strength test method:

[0183] ① Use a flat paper cutter to cut the composite electrode sheets prepared in the examples and comparative examples into strips with the required width and length, and then use dust-free paper to wipe the scaleless steel ruler clean without leaving any stains or dust.

[0184] ② Then stick the double-sided tape on the unscaled steel ruler with a length of 70mm and center it.

[0185] ③Then stick the composite electrode plate on the double-sided tape with the end faces flush, and use a pressure wheel (2kg) with a diameter of 84mm and a height of 45mm to roll back and forth on the surface of the negative electrode plate three times.

[0186] ④ After folding the free end of the composite electrode sheet in the experimental sample 180°, clamp it on the upper fixture of the tensile tester, and clamp the unscaled steel ruler on the lower clamp. Under the conditions of 22~28℃ and humidity less than 25%, prepare several 20mm wide composite electrodes. The stretching speed of the composite electrode sheet is 200mm / min. The test takes the average value of the stretching of 25mm~80mm (total stretching distance of 100mm), peels off the composite electrode sheet, and reads the test result of the peeling strength of the composite electrode sheet when the electrode film of the composite electrode sheet and the solid electrolyte membrane are completely separated.

[0187]

[0188] From the above experimental data, it can be seen that by comparing Example 1 with Comparative Example 1, compared with adding Li 0.33 La 0.56 Composite electrode formed by TiO3, adding BaTiO3-Li 0.33 La 0.56 The composite electrode sheet finally formed by TiO3 brings better overall performance.

[0189] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0190] The above embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A method for preparing a composite electrode sheet, characterized in that: The following steps are involved: S1. Preparation of solid electrolyte membrane: S1-1, polyvinylidene fluoride, BaTiO3-Li 0.33 La 0.56 TiO3 is pre-mixed to prepare a mixture; S1-2, adding polytetrafluoroethylene to the mixture and performing a fiberization treatment to obtain a fiberized mixture; S1-3, rolling the fiberized mixture to obtain a solid electrolyte membrane; S2, preparing electrode film; S3, dry-compositing the solid electrolyte membrane prepared in step S1 and the electrode membrane prepared in step S2 at a temperature of 60° C. to 160° C.; S4, obtaining a composite electrode sheet; In step S1-2 of preparing the fiberized mixture, a high-speed shearing machine is used to perform fiberization treatment at a rotation speed of 20,000 to 28,000 r / min, and the fiberization treatment time is 8 to 15 minutes; The solid electrolyte membrane also includes lithium salt; in terms of mass percentage, the solid electrolyte membrane includes 70% to 97% BaTiO3-Li 0.33 La 0.56 TiO3, 0.1% to 3% of polyvinylidene fluoride, 1% to 15% of the polytetrafluoroethylene, and 1% to 15% of the lithium salt; In the step S3, the solid electrolyte membrane and the electrode membrane are dry-compounded using an elastic roller; The elastic roller comprises a rigid roller and an elastic member, wherein the elastic member is coated on the outer side of the rigid roller.

2. The preparation method according to claim 1, characterized in that In step S1-1 of preparing the mixed material, the premixing treatment is performed by at least one of ball milling, air flow mixing, and pulverizer.

3. The preparation method according to claim 1, characterized in that In step S1-3 of preparing the solid electrolyte membrane, the fiberized mixture is subjected to a hot rolling process using a double-roller device.

4. The preparation method according to claim 1, characterized in that The preparation method further comprises preparing the BaTiO3-Li 0.33 La 0.56 TiO3 step, including BaTiO3 and Li 0.33 La 0.56 TiO3 is subjected to ball milling, drying, pressure forming and calcination.

5. The preparation method according to claim 1, characterized in that Step S2 includes the following steps: S2-1, mixing the active material, the conductive agent, and the binder to prepare a mixture; S2-2, performing a fiberization treatment on the mixture to obtain a fiberized mixture; S2-3, calendering the fiberized mixture to obtain an electrode membrane.

6. A composite electrode plate, characterized in that: The composite electrode plate is prepared according to the preparation method according to any one of claims 1 to 5.

7. A lithium-ion battery, characterized in that: The lithium-ion battery comprises a composite electrode sheet prepared by the preparation method according to any one of claims 1 to 5.