A quaternary piezoelectric ceramic material and preparation method thereof
By introducing specific components into the PZT matrix and adjusting the process, the prepared quaternary piezoelectric ceramic material has improved piezoelectric properties, solved the performance deficiencies of existing PZT materials in high-tech fields, and realized the preparation of high-performance ceramic materials.
Patent Information
- Application Number
- CN202311666262.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-06
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-12-06
AI Technical Summary
Existing PZT piezoelectric ceramic materials offer limited performance improvements in high-tech fields and are insufficient to meet the requirements of medical, electronic, and aerospace applications.
Quaternary piezoelectric ceramic materials were prepared by introducing Pb(Mn,Sb)O3 and Pb(Mn,Nb)O3 into the PZT matrix, combining Sr ion substitution, adding BiFeO3, SmAlO3 and CuO, and using a two-stage pre-firing process of low temperature followed by high temperature.
It improves piezoelectric properties, reduces internal stress, promotes ceramic grain development and sintering density, and enhances the piezoelectric properties and sintering density of the material, thus meeting the application requirements of piezoelectric ceramic components.
Smart Images

Figure CN117843363B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of piezoelectric ceramic materials, in particular to a quaternary piezoelectric ceramic material and a preparation method thereof. Background Art
[0002] Lead zirconate titanate (Pb(Zr,Ti)O 3 , PZT) has a higher piezoelectric constant d 33 , Curie temperature T c and electromechanical coupling coefficient k p , has become the most widely used type of piezoelectric ceramics, and is widely used in sensors, transducers, ultrasonic motors and other fields, especially as a key component in some medical equipment, such as the piezoelectric valve of the ventilator, the welding tools in the working process of the mask machine, and the core components of ultrasonic medical equipment.
[0003] When the PZT ceramic component is near the morphotropic phase boundary (MPB) where the rhombohedral phase and the tetragonal phase coexist, that is, when the Zr / Ti molar ratio is 53 / 47, the ceramic obtains a comprehensive PbZrO 3 、PbTiO 3 However, simply adjusting the performance parameters of ceramics by changing the Zr / Ti ratio is far from meeting the requirements for material performance in the development of high-tech fields such as medicine, electronics, and aerospace. At present, the focus of researchers is to try to add one or more composite perovskite relaxor ferroelectrics to the PZT system to form a ternary or even quaternary piezoelectric ceramic solid solution system in order to obtain piezoelectric ceramic materials with superior performance. Summary of the invention
[0004] Purpose of the invention: In view of the above technical problems, the present invention proposes a quaternary piezoelectric ceramic material and a preparation method thereof.
[0005] The technical solutions adopted are as follows:
[0006] A quaternary piezoelectric ceramic material, the chemical structure of which is shown below:
[0007] αPb 1-x Sr x [(Zr y Ti 1-y ) q (Mn z Nb p Sb 1-z-p ) 1-q ]O 3 -βBiFeO 3 -γSmAlO 3 -ωCuO
[0008] Among them, α, β, γ, and ω are mole fractions;
[0009] x, y, z, q, and p are molar ratios;
[0010] β is 1-5%, γ is 1-5%, ω is 0.1-1%, and the rest is α;
[0011] x is 0.01-0.05, y is 0.4-0.6, z is 0.3-0.7, p is 0.3-0.7, and q is 0.8-0.95.
[0012] Further, β is 1-3%, γ is 1-3%, ω is 0.1-0.5%, and the rest is α.
[0013] Furthermore, α is 97.75%, β is 1%, γ is 1%, and ω is 0.25%.
[0014] Further, x is 0.02-0.03, y is 0.45-0.55, z is 1 / 3-2 / 3, p is 1 / 3-2 / 3, and q is 0.85-0.9.
[0015] Further, x is 0.02, y is 0.5, z is 1 / 3, p is 1 / 3, and q is 0.9.
[0016] The present invention also provides a method for preparing a quaternary piezoelectric ceramic material, comprising the following steps:
[0017] Lead tetraoxide, strontium carbonate, zirconium dioxide, titanium dioxide, manganese dioxide, niobium pentoxide and antimony trioxide are mixed and ball-milled, dried and pre-calcined once to obtain a first mixed material;
[0018] The first mixed material, BiFeO 3 、SmAlO 3 , CuO and mixed with ball mill, dried and pre-fired for the second time, the second mixture obtained after the second pre-fired is ball milled again, dried and added with binder for granulation, aged and pressed into shape, placed in a muffle furnace and heated to 600-700°C for debinding for 1-3h, and then heated to 1300-1350°C for sintering for 2-4h in the second stage.
[0019] Furthermore, the primary pre-firing temperature is 900-950° C., and the primary pre-firing time is 1-3 hours.
[0020] Furthermore, the secondary pre-firing temperature is 1000-1050° C., and the secondary pre-firing time is 1-3 hours.
[0021] Furthermore, during compression molding, preliminary molding is first performed at 5-10 MPa, and then compression molding is performed at 200-250 MPa using an isostatic press.
[0022] Furthermore, the first stage heating rate is 10-30°C / min, and the second stage heating rate is 1-5°C / min.
[0023] Beneficial effects of the present invention:
[0024] The present invention provides a quaternary piezoelectric ceramic material, Pb(Mn,Sb)O 3 and Pb(Mn,Nb)O 3 It is a common relaxor ferroelectric component that improves power characteristics. The present invention introduces the two together into the PZT matrix, and replaces them with Sr ions with smaller ion radius, which produces shrinkage distortion in the unit cell and reduces internal stress, making it easier for the 90° electric domain to turn, thereby improving its piezoelectric performance.
[0025] BiFeO 3 With excellent ferroelectric properties, Bi 3+ and Fe 3+ Both can be dissolved in the perovskite lattice, which has a doping modification effect on the piezoelectric properties and can promote the growth of ceramic grains and sintering density. 3 As perovskite oxides, they can be combined with BiFeO 3 Forming solid solution reduces the tendency of grain boundary phase to form at grain boundaries, thereby reducing porosity and improving sintering density;
[0026] Cu 2+ In ABO 3 The substitution effect in the perovskite crystal structure shows typical soft doping characteristics. The appropriate amount of CuO can cause oxygen vacancies in the crystal during the formation process, resulting in a significant reduction in the activation energy of material transfer during the sintering process, thereby promoting the densification of ceramic sintering and improving the piezoelectric properties.
[0027] There are also reports on two-stage pre-firing, but most of them are high-temperature pre-firing first and then low-temperature pre-firing. In the present invention, on the contrary, a two-stage pre-firing method of low-temperature pre-firing first and high-temperature pre-firing is adopted, and it has been verified that it also plays a positive role in improving the piezoelectric properties of ceramics. The reason may be that the sample prepared by the two-step pre-firing process has a higher crystal phase purity and inhibits the performance degradation caused by the pyrochlore phase. In addition, the low-temperature pre-firing first can prevent excessive crystallization, and then the ball milling and the secondary pre-firing at a higher temperature are more conducive to the growth of ceramic grains, forming a ceramic with a dense structure.
[0028] After testing, it is found that the quaternary piezoelectric ceramic material prepared by the present invention has excellent piezoelectric properties and can meet the application requirements of piezoelectric ceramic components. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a SEM image of the quaternary piezoelectric ceramic material prepared in Example 1. It can be seen from the image that the grains and grain boundary contours are clearly visible, and no obvious pores are found. DETAILED DESCRIPTION
[0030] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.
[0031] Embodiment 1:
[0032] A quaternary piezoelectric ceramic material, the chemical structure of which is shown below:
[0033] 97.75%Pb 0.98 Sr 0.02 [(Zr 0.5 Ti 0.5 ) 0.9 (Mn 1 / 3 Nb 1 / 3 Sb 1 / 3 ) 0.1 ]O 3 -1%BiFeO 3 -1% SmAlO 3 -0.25% CuO
[0034] The preparation method of the above-mentioned quaternary piezoelectric ceramic material is as follows:
[0035] According to the above molar ratio, lead tetroxide, strontium carbonate, zirconium dioxide, titanium dioxide, manganese dioxide, niobium pentoxide and antimony trioxide were weighed and added to the ball mill of a planetary ball mill. Ethanol was used as the ball milling medium. After mixing and ball milling for 10 hours, the mixture was dried in an oven at 70°C for 24 hours, and then taken out and placed in a muffle furnace and heated to 950°C for a pre-calcination. The pre-calcination time was 2 hours to obtain Pb 0.98 Sr 0.02 [(Zr 0.5 Ti 0.5 ) 0.9 (Mn 1 / 3 Nb 1 / 3 Sb 1 / 3 ) 0.1 ]O 3 ;
[0036] Pb 0.98 Sr 0.02 [(Zr 0.5 Ti 0.5 ) 0.9 (Mn 1 / 3 Nb 1 / 3 Sb 1 / 3 ) 0.1 ]O 3、BiFeO 3 、SmAlO 3 , CuO is added to the ball mill of the planetary ball mill according to the above molar fraction, ethanol is used as the ball milling medium, and the mixture is ball milled for 5 hours, and then dried in an oven at 70°C for 24 hours, taken out and placed in a muffle furnace and heated to 1050°C for secondary pre-calcination, and the secondary pre-calcination time is 2 hours. The powder after the secondary pre-calcination is added to the ball mill of the planetary ball mill again, ethanol is used as the ball milling medium, and the mixture is ball milled for 5 hours, and then dried in an oven at 70°C for 24 hours, and a PVA aqueous solution with a mass concentration of 10% is added for granulation, aged for 24 hours, first pressed at 10MPa for 5min for preliminary forming, and then pressed at 200MPa for 20s with an isostatic press to form a green body, which is placed in a muffle furnace and heated to 700°C at a speed of 30°C / min in one stage to debind for 2h, and then heated to 1350°C in a second stage at a speed of 5°C / min and sintered for 4h.
[0037] Embodiment 2:
[0038] A quaternary piezoelectric ceramic material, the chemical structure of which is shown below:
[0039] 97.75%Pb 0.98 Sr 0.02 [(Zr 0.5 Ti 0.5 ) 0.9 (Mn 1 / 3 Nb 1 / 3 Sb 1 / 3 ) 0.1 ]O 3 -1%BiFeO 3 -1% SmAlO 3 -0.25% CuO
[0040] The preparation method of the above-mentioned quaternary piezoelectric ceramic material is as follows:
[0041] According to the above molar ratio, lead tetroxide, strontium carbonate, zirconium dioxide, titanium dioxide, manganese dioxide, niobium pentoxide and antimony trioxide were weighed and added to the ball mill of a planetary ball mill. Ethanol was used as the ball milling medium. After mixing and ball milling for 10 hours, the mixture was dried in an oven at 70°C for 24 hours, and then taken out and placed in a muffle furnace and heated to 900°C for a pre-calcination. The pre-calcination time was 2 hours to obtain Pb 0.98 Sr 0.02 [(Zr 0.5 Ti 0.5 ) 0.9 (Mn 1 / 3 Nb 1 / 3 Sb 1 / 3 ) 0.1 ]O 3 ;
[0042] Pb0.98 Sr 0.02 [(Zr 0.5 Ti 0.5 ) 0.9 (Mn 1 / 3 Nb 1 / 3 Sb 1 / 3 ) 0.1 ]O 3 、BiFeO 3 、SmAlO 3 , CuO is added to the ball mill of the planetary ball mill according to the above molar fraction, ethanol is used as the ball milling medium, and the mixture is ball milled for 5 hours, and then dried in an oven at 70°C for 24 hours, taken out and placed in a muffle furnace and heated to 1000°C for secondary pre-calcination, and the secondary pre-calcination time is 2 hours. The powder after the secondary pre-calcination is added to the ball mill of the planetary ball mill again, ethanol is used as the ball milling medium, and the mixture is ball milled for 5 hours, and then dried in an oven at 70°C for 24 hours, and a PVA aqueous solution with a mass concentration of 10% is added for granulation, aged for 24 hours, first pressed at 10MPa for 5min for preliminary forming, and then pressed at 200MPa for 20s with an isostatic press to form a green body, which is placed in a muffle furnace and heated to 600°C at a speed of 10°C / min in one stage to debind for 2h, and then heated to 1300°C in a second stage at a speed of 1°C / min and sintered for 4h.
[0043] Embodiment 3:
[0044] A quaternary piezoelectric ceramic material, the chemical structure of which is shown below:
[0045] 97.75%Pb 0.98 Sr 0.02 [(Zr 0.5 Ti 0.5 ) 0.9 (Mn 1 / 3 Nb 1 / 3 Sb 1 / 3 ) 0.1 ]O 3 -1%BiFeO 3 -1% SmAlO 3 -0.25% CuO
[0046] The preparation method of the above-mentioned quaternary piezoelectric ceramic material is as follows:
[0047] According to the above molar ratio, lead tetroxide, strontium carbonate, zirconium dioxide, titanium dioxide, manganese dioxide, niobium pentoxide and antimony trioxide were weighed and added to the ball mill of a planetary ball mill. Ethanol was used as the ball milling medium. After mixing and ball milling for 10 hours, the mixture was dried in an oven at 70°C for 24 hours, and then taken out and placed in a muffle furnace and heated to 900°C for a pre-calcination. The pre-calcination time was 2 hours to obtain Pb 0.98 Sr 0.02 [(Zr0.5 Ti 0.5 ) 0.9 (Mn 1 / 3 Nb 1 / 3 Sb 1 / 3 ) 0.1 ]O 3 ;
[0048] Pb 0.98 Sr 0.02 [(Zr 0.5 Ti 0.5 ) 0.9 (Mn 1 / 3 Nb 1 / 3 Sb 1 / 3 ) 0.1 ]O 3 、BiFeO 3 、SmAlO 3 , CuO is added to the ball mill of the planetary ball mill according to the above molar fraction, ethanol is used as the ball milling medium, and the mixture is ball milled for 5 hours, and then dried in an oven at 70°C for 24 hours, taken out and placed in a muffle furnace and heated to 1050°C for secondary pre-calcination, and the secondary pre-calcination time is 2 hours. The powder after the secondary pre-calcination is added to the ball mill of the planetary ball mill again, ethanol is used as the ball milling medium, and the mixture is ball milled for 5 hours, and then dried in an oven at 70°C for 24 hours, and a PVA aqueous solution with a mass concentration of 10% is added for granulation, aged for 24 hours, first pressed at 10MPa for 5min for preliminary forming, and then pressed at 200MPa for 20s with an isostatic press to form a green body, which is placed in a muffle furnace and heated to 600°C at a speed of 30°C / min in one stage to debind for 2h, and then heated to 1300°C at a speed of 5°C / min in two stages and sintered for 4h.
[0049] Embodiment 4:
[0050] A quaternary piezoelectric ceramic material, the chemical structure of which is shown below:
[0051] 97.75%Pb 0.98 Sr 0.02 [(Zr 0.5 Ti 0.5 ) 0.9 (Mn 1 / 3 Nb 1 / 3 Sb 1 / 3 ) 0.1 ]O 3 -1%BiFeO 3 -1% SmAlO 3 -0.25% CuO
[0052] The preparation method of the above-mentioned quaternary piezoelectric ceramic material is as follows:
[0053] According to the above molar ratio, lead tetroxide, strontium carbonate, zirconium dioxide, titanium dioxide, manganese dioxide, niobium pentoxide and antimony trioxide were weighed and added to the ball mill of a planetary ball mill. Ethanol was used as the ball milling medium. After mixing and ball milling for 10 hours, the mixture was dried in an oven at 70°C for 24 hours, and then taken out and placed in a muffle furnace and heated to 950°C for a pre-calcination. The pre-calcination time was 2 hours to obtain Pb 0.98 Sr 0.02 [(Zr 0.5 Ti 0.5 ) 0.9 (Mn 1 / 3 Nb 1 / 3 Sb 1 / 3 ) 0.1 ]O 3 ;
[0054] Pb 0.98 Sr 0.02 [(Zr 0.5 Ti 0.5 ) 0.9 (Mn 1 / 3 Nb 1 / 3 Sb 1 / 3 ) 0.1 ]O 3 、BiFeO 3 、SmAlO 3 , CuO is added to the ball mill of the planetary ball mill according to the above molar fraction, ethanol is used as the ball milling medium, and the mixture is ball milled for 5 hours, and then dried in an oven at 70°C for 24 hours, taken out and placed in a muffle furnace and heated to 1000°C for secondary pre-calcination, and the secondary pre-calcination time is 2 hours. The powder after the secondary pre-calcination is added to the ball mill of the planetary ball mill again, ethanol is used as the ball milling medium, and the mixture is ball milled for 5 hours, and then dried in an oven at 70°C for 24 hours, and a PVA aqueous solution with a mass concentration of 10% is added for granulation, aged for 24 hours, first pressed at 10MPa for 5min for preliminary forming, and then pressed at 200MPa for 20s with an isostatic press to form a green body, which is placed in a muffle furnace and heated to 700°C at a rate of 10°C / min in one stage to debind for 2h, and then heated to 1350°C in two stages at a rate of 1°C / min and sintered for 4h.
[0055] Comparative Example 1:
[0056] The same as Example 1, except that BiFeO is not added. 3 、SmAlO 3 and CuO.
[0057] Comparative Example 2:
[0058] The same as Example 1, except that BiFeO is not added. 3 .
[0059] Comparative Example 3:
[0060] The same as Example 1, except that SmAlO 3 .
[0061] Comparative Example 4:
[0062] It is basically the same as Example 1, except that CuO is not added.
[0063] Comparative Example 5:
[0064] The embodiment is basically the same as the first embodiment, except that a quaternary piezoelectric ceramic material is used, and its chemical structure is as follows:
[0065] 97.75%Pb 0.98 Sr 0.02 [(Zr 0.5 Ti 0.5 ) 0.9 (Mn 1 / 3 Nb 1 / 3 Sb 1 / 3 ) 0.1 ]O 3 -1%BiFeO 3 -1% SmAlO 3 -0.25% CuO
[0066] The preparation method of the above-mentioned quaternary piezoelectric ceramic material is as follows:
[0067] According to the above molar ratio, lead tetroxide, strontium carbonate, zirconium dioxide, titanium dioxide, manganese dioxide, antimony trioxide, BiFeO 3 、SmAlO 3 , CuO are added to the ball mill of the planetary ball mill, and ethanol is used as the ball milling medium. After mixing and ball milling for 5 hours, the mixture is dried in an oven at 70°C for 24 hours, taken out and placed in a muffle furnace and heated to 1050°C for pre-calcination for 2 hours. The pre-calcination time is 2 hours. The pre-calcined powder is added to the ball mill of the planetary ball mill again, and ethanol is used as the ball milling medium. After mixing and ball milling for 5 hours, the mixture is dried in an oven at 70°C for 24 hours, and a 10% mass concentration of PVA aqueous solution is added to granulate. After aging for 24 hours, the mixture is first pressed at 10MPa for 5 minutes for preliminary forming, and then pressed at 200MPa for 20s with an isostatic press to form a green body. The green body is placed in a muffle furnace and heated to 700°C at a speed of 30°C / min in one stage to debind for 2 hours, and then heated to 1350°C at a speed of 5°C / min in a second stage and sintered for 4 hours.
[0068] Performance Test:
[0069] The surfaces of the quaternary piezoelectric ceramic materials prepared in Examples 1-4 and Comparative Examples 1-5 of the present invention were silvered on both sides, and then subjected to high-voltage polarization in silicone oil at 110°C to prepare samples. The polarization voltage was 4 kV / mm, and the polarization time was 20 min. After the polarized samples were allowed to stand at room temperature for 7 days, the resonant frequency f of the components was measured using the bridge method on a TH2828S impedance analyzer. r , anti-resonance frequency f a , and the corresponding capacitance C T The electromechanical coupling coefficient kp and relative dielectric constant ε are calculated by referring to the "Measurement and Calculation Method of Performance Parameters of Practical Piezoelectric Ceramic Components for Underwater Acoustics" (CB / T 4314-2013). T 33 / ε 0 ; Using ZJ-2 quasi-static d 33 The longitudinal piezoelectric constant d of the measuring instrument test element 33 .
[0070] The test results are shown in Table 1:
[0071] Table 1:
[0072]
[0073] It can be seen from Table 1 above that the quaternary piezoelectric ceramic material prepared in the present invention has excellent piezoelectric properties and can meet the application requirements of piezoelectric ceramic components.
[0074] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A quaternary piezoelectric ceramic material, characterized in that: Its chemical structure is shown below: <h2 style=";text-align:left;direction:ltr">αPb<h2 style=";text-align:left;direction:ltr"> 1-x <h2 style=";text-align:left;direction:ltr"> Sr<h2 style=";text-align:left;direction:ltr"> x <h2 style=";text-align:left;direction:ltr"> [(Zr<h2 style=";text-align:left;direction:ltr"> y <h2 style=";text-align:left;direction:ltr"> Ti<h2 style=";text-align:left;direction:ltr"> 1-y <h2 style=";text-align:left;direction:ltr"> )<h2 style=";text-align:left;direction:ltr"> q <h2 style=";text-align:left;direction:ltr"> (Mn<h2 style=";text-align:left;direction:ltr"> z <h2 style=";text-align:left;direction:ltr"> Nb<h2 style=";text-align:left;direction:ltr"> p <h2 style=";text-align:left;direction:ltr"> Sb<h2 style=";text-align:left;direction:ltr"> 1-z-p <h2 style=";text-align:left;direction:ltr"> )<h2 style=";text-align:left;direction:ltr"> 1-q <h2 style=";text-align:left;direction:ltr"> ]O3-βBiFeO3-γSmAlO3-ωCuO Among them, α, β, γ, and ω are mole fractions; x, y, z, q, and p are molar ratios; α is 97.75%, β is 1%, γ is 1%, and ω is 0.25%; x is 0.02, y is 0.5, z is 1 / 3, p is 1 / 3, q is 0.9; The method for preparing the above-mentioned quaternary piezoelectric ceramic material comprises the following steps: Lead tetraoxide, strontium carbonate, zirconium dioxide, titanium dioxide, manganese dioxide, niobium pentoxide and antimony trioxide are mixed and ball-milled, dried and pre-calcined once to obtain a first mixed material; The first mixed material, BiFeO3, SmAlO3, and CuO are mixed and ball-milled, dried, and then pre-fired twice. The second mixed material obtained after the second pre-fired is ball-milled again, dried, added with a binder, granulated, aged, and pressed into shape, and then placed in a muffle furnace and heated to 600-700°C for debinding for 1-3 hours in the first stage, and heated to 1300-1350°C for sintering for 2-4 hours in the second stage; The primary pre-burning temperature is 900-950℃, and the primary pre-burning time is 1-3h; The secondary pre-burning temperature is 1000-1050℃, and the secondary pre-burning time is 1-3h; During compression molding, the mold is initially formed at 5-10 MPa, and then compressed at 200-250 MPa using an isostatic press. The heating rate of the first stage is 10-30℃ / min, and the heating rate of the second stage is 1-5℃ / min.