Positive electrode active material for lithium secondary battery and lithium secondary battery comprising same

By using lithium-nickel metal composite oxide particles in the positive electrode active material of the lithium secondary battery and introducing tungsten compounds, the problem of poor structural stability of the lithium secondary battery is solved, and the charging and discharging efficiency and life characteristics of the battery are improved.

CN119008932APending Publication Date: 2024-11-22SK INNOVATION CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410496712.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-16
Filing Date
2024-04-24
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The structural stability of nickel-based lithium metal oxides in lithium secondary batteries leads to a reduction in battery life characteristics, and the existing metal doping methods are not sufficient to improve performance.

Method used

Using a positive electrode active material containing lithium-nickel metal composite oxide particles, a permeability area is formed in the area below 70% of the particle surface to the center direction and tungsten compound is included to improve lithium ion conductivity, reduce resistance, and coat it by dry method. and calcining process enhance structural stability.

Benefits of technology

It effectively improves the charging and discharging efficiency and power characteristics of lithium secondary batteries, inhibits the structural collapse and internal resistance of the positive electrode active substance, and extends the battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008932A_ABST
    Figure CN119008932A_ABST
Patent Text Reader

Abstract

A positive electrode active material for a lithium secondary battery according to an embodiment of the present invention contains lithium-nickel metal composite oxide particles in the form of secondary particles in which a plurality of primary particles are aggregated, the lithium-nickel metal composite oxide particles including a permeation region, the permeation region is formed in a region extending from the surface to a position of 70% or less of the radius in the center direction of the particle, and contains a tungsten compound at the interface between the primary particles. The relative standard deviation (RSD) value as a result of measuring the tungsten content 10 times at mutually different positions from the surface of the secondary particles to a depth of 10 nm by X-ray photoelectron spectroscopy is 10-40%. The present invention can provide a lithium secondary battery including a positive electrode having improved structural stability, reduced resistance, and high capacity and high power characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention provides a positive electrode active material for a lithium secondary battery and a lithium secondary battery comprising the positive electrode active material. Background Art

[0002] Secondary batteries are batteries that can be repeatedly charged and discharged. With the development of the information communication and display industries, secondary batteries are widely used as a power source for portable electronic communication devices such as camcorders, mobile phones, and notebook computers. In addition, in recent years, battery packs including secondary batteries are being developed and used as a power source for environmentally friendly vehicles such as hybrid vehicles.

[0003] Examples of secondary batteries include lithium secondary batteries, nickel-cadmium batteries, and nickel-metal hydride batteries. Among them, lithium secondary batteries have high operating voltage and energy density per unit weight, and are advantageous in terms of charging speed and light weight, and therefore are actively being researched and developed.

[0004] A lithium secondary battery may include: an electrode assembly including a positive electrode, a negative electrode and a separation membrane (diaphragm); and an electrolyte in which the electrode assembly is impregnated. The lithium secondary battery may also include an outer packaging material such as a soft-pack outer packaging material that accommodates the electrode assembly and the electrolyte.

[0005] Lithium-transition metal composite oxides can be used as positive electrode active materials for lithium secondary batteries. Examples of the lithium-transition metal composite oxides include nickel-based lithium metal oxides. Nickel-based lithium metal oxides contain a high content of nickel, so the capacity of the battery can be increased.

[0006] However, when the nickel content in the nickel-based lithium metal oxide increases, the structural stability is poor during repeated charge and discharge of the battery, so there is a problem of reduced battery life characteristics. In order to solve this problem, a metal doping method has been proposed, but it is not enough to fully improve the performance of the battery. Summary of the invention

[0007] Technical issues to be solved

[0008] An object of the present invention is to provide a positive electrode active material for a lithium secondary battery having improved structural stability and a lithium secondary battery including the positive electrode active material.

[0009] Technical Solution

[0010] According to an exemplary embodiment, a positive electrode active material for a lithium secondary battery comprising lithium-nickel metal composite oxide particles is provided. The lithium-nickel metal composite oxide particles are in the form of secondary particles formed by the aggregation of multiple primary particles. The lithium-nickel metal composite oxide particles include a permeation region, which is formed in a region from the surface to a position below 70% of the radius along the center direction of the particle and contains a tungsten compound at the interface between the primary particles. The relative standard deviation (RSD) value of the results of measuring the tungsten content 10 times at different positions from the surface of the secondary particles to a depth of 10 nm using X-ray photoelectron spectroscopy is 10-40%.

[0011] According to an exemplary embodiment, the relative standard deviation value may be 20-30%.

[0012] According to an exemplary embodiment, the thickness of the permeation region may correspond to 10-55% of the radius of the secondary particle from the surface of the secondary particle in the center direction of the particle.

[0013] According to an exemplary embodiment, the lithium-nickel metal composite oxide particle may include a chemical structure represented by Chemical Formula 1 below.

[0014] [Chemical formula 1]

[0015] Li a [Ni b Co c Mn d X y ]O e

[0016] In the chemical formula 1, X may include at least one of W, S, Al, Ti, Sr, Zr, P, and K, and may be 0.5 <a<1.5,0.8<b≤1,0<c<0.1,0<d<0.1,1.5<e<2.5,0<y<0.1。

[0017] According to an exemplary embodiment, the tungsten compound may include lithium-tungsten oxide.

[0018] According to an exemplary embodiment, the lithium-tungsten oxide may be represented by Chemical Formula 2 below.

[0019] [Chemical formula 2]

[0020] Li x W y O z

[0021] In the chemical formula 2, it can be 0 <x≤3,0<y≤5,0<z≤8。

[0022] According to an exemplary embodiment, the content of tungsten may be 500-10000 ppm in the total weight of the lithium-nickel metal composite oxide particles.

[0023] According to an exemplary embodiment, the content of tungsten may be 1000-5000 ppm in the total weight of the lithium-nickel metal composite oxide particles.

[0024] According to an exemplary embodiment, at least a portion of the plurality of primary particles in the permeation region may include a rock salt phase region formed from the surface along the center direction, and the thickness of the rock salt phase region may be 5-10 nm from the surface of the primary particle to the center direction.

[0025] According to an exemplary embodiment, the average particle size (D50) of the lithium-nickel metal composite oxide particles may be 10-30 μm.

[0026] According to an exemplary embodiment, the resistivity of the positive electrode active material for a lithium secondary battery defined by the following Formula 1 may be 30-120 Ω·cm.

[0027] [Formula 1]

[0028] ρ=4×r×R sp

[0029] In the above formula 1, ρ can be the resistivity, R sp It can be the average value of the spreading resistance of the lithium-nickel metal composite oxide particles measured from the spreading resistance distribution image, wherein the spreading resistance distribution image is obtained by contacting a needle tip coated with a conductive component of an atomic force microscope (Atomic force microscopy, AFM) to an area of ​​200nm×200nm in the cross-section of the positive electrode containing the positive electrode active material and applying a voltage of 3V and photographing it in a scanning spreading resistance microscope (Scanning Spreading Resistance Microscopy, SSRM) mode, and r can be the contact radius of the needle tip.

[0030] According to an exemplary embodiment, the resistivity may be 40-105 Ω·cm.

[0031] According to an exemplary embodiment, a lithium secondary battery is provided, including: a positive electrode for a lithium secondary battery, the positive electrode for a lithium secondary battery including the positive electrode active material; and a negative electrode, the negative electrode being disposed opposite to the positive electrode.

[0032] Beneficial Effects

[0033] The positive active material for a lithium secondary battery according to an exemplary embodiment may include secondary particles including primary particles of a lithium-nickel metal composite oxide, and may include a permeation region which is a region from a surface of the secondary particle to an internal position and includes a tungsten compound at an interface between the primary particles.

[0034] Therefore, the tungsten compound can reduce the resistance in the positive electrode active material by improving the lithium ion conductivity between the primary particles. In addition, the structural stability of the positive electrode active material containing the tungsten compound is improved, thereby effectively reducing the collapse of the layered structure of the positive electrode active material and the generation of gas caused by the surface side reaction with the electrolyte.

[0035] The lithium secondary battery according to the exemplary embodiment includes the positive active material, so that the charge and discharge efficiency and power characteristics can be improved, and even when charging and discharging are repeated, the structural collapse of the positive active material is suppressed, so that the life characteristics and the increase of internal resistance (IR) during life can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 and Figure 2 1 and 2 are a schematic plan view and a schematic cross-sectional view, respectively, showing a lithium secondary battery according to an exemplary embodiment.

[0037] Figure 3 TEM image and EDS tungsten element mapping image of the positive electrode active material of Example 3.

[0038] Figure 4 TEM image and EDS tungsten element mapping image of the positive electrode active material of Comparative Example 1.

[0039] Figure 5 These are a TEM image and an EDS tungsten element mapping image of the positive electrode active material of Comparative Example 2.

[0040] Figure 6 TEM image and EDS tungsten element mapping image of the positive electrode active material of Comparative Example 3 are shown.

[0041] Figure 7 TEM image and EDS tungsten element mapping image of the positive electrode active material of Comparative Example 4 are shown.

[0042] Figure 8 This is an EDS spectrum of the surface of the positive electrode active material of Example 3.

[0043] Fig. 9 and Fig.10These are EDS spectra of two locations inside the positive electrode active material of Example 3.

[0044] Fig.11 This is an EDS spectrum of the surface of the positive electrode active material of Comparative Example 1.

[0045] Fig.12 This is an EDS spectrum of the interior of the positive electrode active material of Comparative Example 1.

[0046] Fig.13 These are the TEM image and SAED image of Example 3.

[0047] Fig.14 These are the TEM image and SAED image of Comparative Example 1.

[0048] Fig.15 It is the SSRM extended resistance distribution image of the positive electrode cross section of Example 1 to Example 3, Comparative Examples 1 to Comparative Examples 4 and Reference Example.

[0049] Fig.16 This is a graph showing the average values ​​of spreading resistance of the positive electrode active materials of Examples 1 to 3, Comparative Example 1, and Reference Example. DETAILED DESCRIPTION

[0050] The present invention provides a positive electrode active material for a lithium secondary battery according to an exemplary embodiment and a lithium secondary battery including the positive electrode active material.

[0051] Hereinafter, embodiments of the present invention will be described in detail, however, these are merely exemplary embodiments, and the present invention is not limited to the specific embodiments described exemplarily.

[0052] A positive electrode active material for a lithium secondary battery according to an exemplary embodiment (hereinafter, may be simply referred to as “positive electrode active material”) may include lithium-nickel metal composite oxide particles.

[0053] The positive electrode active material may include particles of the lithium-nickel metal composite oxide. For example, the amount of the particles of the lithium-nickel metal composite oxide may be 50% by weight or more of the total weight of the positive electrode active material. In some embodiments, the amount of the particles of the lithium-nickel metal composite oxide may be 60% by weight or more, 70% by weight or more, 80% by weight or more, or 90% by weight or more of the total weight of the positive electrode active material.

[0054] In one embodiment, the positive electrode active material may consist essentially of particles of the lithium-nickel metal composite oxide.

[0055] For example, the lithium-nickel metal composite oxide is a metal oxide containing lithium and nickel, and may further contain other transition metals. For example, the transition metal may contain cobalt or manganese.

[0056] According to an exemplary embodiment, the positive active material for a lithium secondary battery may be represented by the following Chemical Formula 1.

[0057] [Chemical formula 1]

[0058] Li a [Ni b Co c Mn d X y ]O e

[0059] In the chemical formula 1, X may include at least one of W, S, Al, Ti, Sr, Zr, P, and K, and may be 0.5 <a<1.5,0.8<b≤1,0<c<0.1,0<d<0.1,1.5<e<2.5,0<y<0.1。

[0060] The chemical structure represented by the chemical formula 1 represents the bonding relationship contained in the layered structure or crystal structure of the positive electrode active material containing the lithium-nickel metal composite oxide, and does not exclude other additional elements. For example, the X can be provided as the main active element of the positive electrode active material. Chemical formula 1 is provided to represent the bonding relationship of the main active element and should be understood as a formula including the introduction and substitution of additional elements.

[0061] In one embodiment, in addition to the main active element, an auxiliary element for enhancing the chemical stability of the positive electrode active material or the layered structure / crystal structure may be further included. The auxiliary element may be mixed together into the layered structure / crystal structure to form a bond, and it should be understood that this situation is also included in the chemical structure represented by Chemical Formula 1.

[0062] The auxiliary element may include, for example, at least one of W, Na, Mg, Ca, Y, Ti, Hf, V, Nb, Ta, Cr, Mo, Fe, Cu, Ag, Zn, B, Al, Ga, C, Si, Sn, Sr, Ba, Ra, P, or Zr. The auxiliary element may be an auxiliary active element that contributes to the structural stability / power activity of the positive electrode active material together with Co or Mn, such as Al.

[0063] The positive electrode active material may further include a coating element or a doping element. For example, an element substantially the same as or similar to the auxiliary element may be used as the coating element or the doping element. For example, one or a combination of two or more of the auxiliary elements may be used as the coating element or the doping element.

[0064] The coating element or the doping element may exist on the surface of the lithium-nickel metal composite oxide particle, or may penetrate through the surface of the lithium-nickel metal composite oxide particle and be included in the bonding structure represented by the Chemical Formula 1.

[0065] According to an exemplary embodiment, the lithium-nickel metal composite oxide particles may be in the form of secondary particles formed by the aggregation of multiple primary particles. In this specification, "primary particle" may refer to a single particle (monolith) that exists alone without forming an aggregate. In this specification, "secondary particle" may refer to a particle having a structure formed by the aggregation of the primary particles.

[0066] According to an exemplary embodiment, the lithium-nickel metal composite oxide particle may include a permeation region, which is formed in a region from the surface to a position less than 70% of the radius along the center direction of the particle and contains a tungsten compound at the interface between the primary particles. In some embodiments, the permeation region may include a surface portion of a positive electrode active material. In this specification, "surface portion" may refer to a region from the outer surface of a particle to a position less than 30% of the radius along the center direction of the particle. For example, the surface portion of a secondary particle may refer to a region from the outer surface of a secondary particle to a distance of about 5 μm along the center direction of the particle. In addition, the surface portion of a primary particle may refer to a region from the outer surface of a primary particle to a distance of about 10 nm in the direction of the center portion of the particle.

[0067] According to an exemplary embodiment, the thickness of the permeable region may be less than 70% of the radius of the secondary particle from the surface of the secondary particle to the center direction of the particle. According to some embodiments, the thickness of the permeable region may correspond to 10-55% of the radius of the secondary particle from the surface of the secondary particle to the center direction of the particle. For example, the thickness of the permeable region may correspond to 40-55% of the radius of the secondary particle from the surface of the secondary particle to the center direction of the particle.

[0068] When there is a permeation region in the region from the surface of the positive electrode active material to the internal position within the above range, the tungsten compound can increase lithium ion conductivity at the interface between primary particles and improve the structural stability of the positive electrode active material during repeated charge and discharge of the battery.

[0069] According to an exemplary embodiment, the tungsten compound may include lithium-tungsten oxide.

[0070] According to an exemplary embodiment, the lithium-tungsten oxide may be represented by Chemical Formula 2 below.

[0071] [Chemical formula 2]

[0072] Li x W y O z

[0073] In the chemical formula 2, it can be 0 <x≤3,0<y≤5,0<z≤8。

[0074] When the lithium-tungsten oxide is present at the primary particle interface of the positive electrode active material, the lithium ion conductivity inside the positive electrode active material can be effectively improved, thereby reducing the resistance of the positive electrode active material. Therefore, even during repeated charge and discharge, the resistance of the positive electrode active material during lithium ion insertion / deinsertion is low, so a lithium secondary battery with less capacity reduction can be achieved.

[0075] According to an exemplary embodiment, in the positive electrode active material for lithium secondary batteries, the relative standard deviation (RSD) value of the results of measuring the tungsten content 10 times at different positions from the surface of the secondary particles to a depth of 10 nm by X-ray photoelectron spectroscopy can be 10-40%. According to some embodiments, the relative standard deviation (RSD) value can be 20-30%.

[0076] The relative standard deviation is a percentage value of the standard deviation value of the data relative to the average value of the data, and is a measure that can confirm the relative dispersion degree of the data. The closer the value is to 0, the more uniform the data is.

[0077] When the relative standard deviation value is less than 10%, it may mean that the tungsten element is evenly distributed on the surface of the positive electrode active material particles. That is, it may mean that the added tungsten element does not penetrate into the interior of the positive electrode active material particles, but is completely distributed on the surface, thereby showing a uniform content, and no penetration area is formed inside the particles.

[0078] Therefore, the tungsten compound is generally present on the surface of the positive electrode active material particles rather than inside, and the lithium-tungsten oxide formed on the surface of the positive electrode active material particles may form a thick rock salt phase. This increases the surface resistance of the positive electrode active material and may eventually increase the resistance of the entire electrode. When the resistance of the entire electrode increases, the charge and discharge efficiency characteristics of the battery may decrease.

[0079] According to an exemplary embodiment, the X-ray photoelectron spectroscopy (XPS) can be performed on the positive active material particles. For example, the X-ray photoelectron spectroscopy can use ESCALAB 250Xi (Thermo Scientific) Company) as an analysis device, and is not limited thereto. In addition, the XPS analysis can be performed under the following conditions.

[0080] -1) X-ray type: Source-Al k alpha, 1486.68 eV, beam size 900 μm

[0081] Analyzer: CAE Mode

[0082] -2) Scan conditions (including Al2p, Na1s):

[0083] Number of scans: 20 to 50

[0084] Pass energy: 20eV

[0085] Dwell time: 50-100ms

[0086] Energy step: 0.1eV

[0087] According to an exemplary embodiment, the content of tungsten in the total weight of the lithium-nickel metal composite oxide may be 500-10000 ppm. According to some embodiments, the content of tungsten in the total weight of the lithium-nickel metal composite oxide may be 500-10000 ppm, 1000-10000 ppm, 3000-10000 ppm or 1000-5000 ppm.

[0088] When the positive electrode active material contains tungsten in an amount within the above range, a lithium secondary battery having high charge and discharge capacity and improved power characteristics can be realized.

[0089] According to an exemplary embodiment, the permeable region may include a rock-salt region. The rock-salt phase may be formed by the tungsten compound. For example, the lithium-tungsten oxide itself may form a rock-salt phase, or the metal and / or oxygen of the lithium-nickel metal composite oxide may be dissolved and form a tungsten compound in a rock-salt phase together with the tungsten component.

[0090] According to an exemplary embodiment, at least a portion of the plurality of primary particles in the infiltration region may include a rock salt phase region formed from the surface along a central direction. In some embodiments, tungsten may infiltrate from the surface of the primary particles along a central direction, thereby forming a rock salt phase region.

[0091] According to an exemplary embodiment, the thickness of the rock salt phase region may be 5-10 nm from the surface of the primary particle to the center direction. When the rock salt phase region has a thickness within the above range, the surface and internal resistance of the positive electrode active material will not increase significantly while being structurally stable, thereby improving the high temperature stability and life characteristics of the positive electrode active material.

[0092] According to an exemplary embodiment, the average particle size (D50) of the secondary particles may be 10-30 μm. According to some embodiments, the average particle size (D50) of the secondary particles may be 10-20 μm. When the secondary particles have an average particle size within the above range, the total surface area of ​​the positive electrode active material is wide, and the positive electrode active material can be contained in the positive electrode active material layer at a high density, so a high-capacity lithium secondary battery can be achieved.

[0093] According to an exemplary embodiment, the resistivity of the positive electrode active material for a lithium secondary battery defined by the following Formula 1 may be 30-120 Ω·cm. According to some embodiments, the resistivity may be 40-105 Ω·cm.

[0094] [Formula 1]

[0095] ρ=4×r×R sp

[0096] In the above formula 1, ρ can be the resistivity, R sp It can be the average value of the spreading resistance of the positive electrode active material measured from the spreading resistance distribution image, which is obtained by contacting the tip of an atomic force microscope (AFM) coated with a conductive component to an area of ​​200nm×200nm in the cross-section of the positive electrode containing the positive electrode active material, applying a voltage of 3V and photographing in a scanning spreading resistance microscope (SSRM) mode, and r can be the contact radius of the tip.

[0097] When the AFM is used to bring a conductive tip into contact with the surface of a sample and scan, the entire area of ​​the sample surface is electrified, and by measuring the amount of current relative to the applied voltage in the local area in contact with the tip, a resistance distribution image can be displayed with high resolution.

[0098] For the image, a local resistance value may be obtained by two-dimensionally measuring a distribution of resistance values ​​in an SSRM mode, and an image may be obtained by visualizing the extended resistance.

[0099] This local resistance can be called spreading resistance, and an image can be obtained that uses light and dark colors to represent the high and low resistance values. The spreading resistance distribution image can be measured using, for example, an AFM from Bruker.

[0100] The spreading resistance average value of the positive electrode active material can be obtained from the spreading resistance distribution image. For example, the spreading resistance distribution image can display the resistance distribution of the cross section of multiple lithium-nickel metal composite oxide particles. Thus, the resistance of the cross section of each lithium-nickel metal composite oxide particle contained in the measurement area can be obtained, and the average value of multiple resistance values ​​can be calculated as the spreading resistance average value.

[0101] The tip of the AFM may have a bending radius of 30-100 nm, and the tip may use, for example, a conductive diamond-coated tip.

[0102] When the resistivity is within the above range, the positive electrode active material has low cross-sectional resistance, thereby having not only high lithium ion conductivity but also high electron conductivity, thereby improving the power characteristics of the positive electrode including the positive electrode active material.

[0103] According to an exemplary embodiment, a method of preparing the positive active material is provided.

[0104] According to an exemplary embodiment, first, lithium-nickel metal composite oxide particles can be prepared. The lithium-nickel metal composite oxide particles can be in the form of secondary particles formed by the aggregation of multiple primary particles. The lithium-nickel metal composite oxide particles can be prepared by methods well known in the art. For example, lithium-nickel metal composite oxide particles can be prepared by reacting a transition metal precursor with a lithium raw material. The transition metal precursor (e.g., Ni-Co-Mn precursor) can be prepared by a coprecipitation reaction.

[0105] For example, the transition metal precursor can be prepared by a coprecipitation reaction of a metal salt, which can include a nickel salt, a manganese salt, and a cobalt salt.

[0106] Examples of the nickel salt include nickel sulfate, nickel hydroxide, nickel nitrate, nickel acetate, and hydrates thereof. Examples of the manganese salt include manganese sulfate, manganese acetate, and hydrates thereof.

[0107] Examples of the cobalt salt include cobalt sulfate, cobalt nitrate, cobalt carbonate, and hydrates thereof.

[0108] The aqueous solution may be prepared by mixing the metal salt with a precipitant and / or a chelating agent in a ratio satisfying the content or concentration ratio of each metal described with reference to Chemical Formula 1. The transition metal precursor may be prepared by coprecipitating the aqueous solution in a reactor.

[0109] The precipitant may include alkaline compounds such as sodium hydroxide (NaOH) and sodium carbonate (Na2CO3). The chelating agent may include, for example, aqueous ammonia, ammonium carbonate, and the like.

[0110] The temperature of the coprecipitation reaction can be adjusted within a range of about 40-60° C., for example. The reaction time can be adjusted within a range of about 24-72 hours.

[0111] The lithium raw material may include, for example, lithium-containing carbonates (e.g., lithium carbonate, etc.), hydrates (e.g., lithium hydroxide monohydrate (LiOH·H2O), etc.), hydroxides (e.g., lithium hydroxide, etc.), nitrates (e.g., lithium nitrate (LiNO3), etc.), chlorides (e.g., lithium chloride (LiCl), etc.), etc. These may be used alone or in combination of two or more.

[0112] According to an exemplary embodiment, the lithium-nickel metal composite oxide may be prepared by first calcining after preparing a mixture including a transition metal precursor and a lithium raw material. The mixture may further include a raw material containing a doping metal element or an auxiliary metal element.

[0113] In an exemplary embodiment, the first calcination may be performed at 600-1000° C., in some embodiments, the first calcination may be performed at 700-900° C. for 5-30 hours, and in some embodiments, the first calcination may be performed for 10-20 hours.

[0114] The prepared lithium-nickel metal composite oxide may be formed in the form of secondary particles having a structure in which a plurality of primary particles are aggregated.

[0115] Next, the secondary particles can be mixed with ammonium paratungstate (APT) and dry coated. The dry coating method is not particularly limited and can be a method known in the art. For example, the secondary particles and ammonium paratungstate can be dry mixed in a dry high-speed mixer.

[0116] The ammonium paratungstate may be mixed such that the content of the tungsten element is 500-10000 ppm or 1000-5000 ppm relative to the total weight of the secondary particles.

[0117] Next, the secondary particles dry-coated with APT are mixed with an aqueous solution containing a sulfonyl additive to prepare a mixture. The sulfonyl additive may be represented by the following structural formula 1.

[0118] [Structural Formula 1]

[0119]

[0120] In structural formula 1, n can be 0≤n<3, R1 and R2 can be O - , NH2, NH3 + , OH or a hydrocarbon group having 1 to 3 carbon atoms which may be substituted by a substituent, wherein the substituent may include a halogen, a cyano group, a hydroxyl group, a phosphoric acid group, a carboxyl group or a salt thereof.

[0121] In an exemplary embodiment, the aqueous solution may include a solvent and a sulfonyl additive, and the solvent may include deionized water.

[0122] In the process of preparing the secondary particles coated with APT by the dry method, in order to improve the yield of lithium metal oxide particles or the stability of the synthesis process, an excess of lithium raw material (lithium salt) may be used. In this case, lithium compounds including lithium hydroxide (LiOH) and lithium carbonate (Li2CO3) may remain on the surface of the secondary particles.

[0123] In the case of washing with substantially the same amount of water as the positive electrode active material to remove (water washing treatment) the residual lithium, although the residual lithium can be removed, it may cause oxidation of the surface of the secondary particles and side reactions with water, which may cause damage or collapse of the layered structure of the primary particles. In addition, the layered structure is transformed into a face-centered cubic structure, a spinel structure and / or a rock salt structure instead of a close-packed hexagonal structure due to water, so that the lithium-nickel-based oxide may be hydrolyzed to generate nickel impurities such as NiO. In this case, since the structure of the transformation is an irreversible structure, the movement of lithium may be hindered during charging and discharging. Therefore, the initial capacity and capacity retention rate of the secondary battery may be reduced.

[0124] However, according to some embodiments, when the aqueous solution and the secondary particles dry-coated with APT are mixed, the sulfonyl compound can react with the residual lithium present on the surface of the secondary particles to form lithium sulfate. The lithium sulfate can passivate the surface of the secondary particles, for example, a lithium-sulfur containing portion having a monoclinic crystal structure in which lithium and sulfur are combined can be formed between the primary particles including a close-packed hexagonal structure.

[0125] In addition, since no water washing treatment is performed, for example, the lithium-transition metal composite oxide particles do not contain primary particles of a face-centered cubic structure, thereby preventing oxidation of the particle surface caused by water and damage to the layered structure, and simultaneously effectively removing residual lithium.

[0126] The ammonium ions contained in the sulfonyl compound are ions composed only of non-metallic elements and can be removed by being gasified in the second calcination process described below.

[0127] In an exemplary embodiment, the amount of the solvent in the aqueous solution may be 2-20% by weight relative to the total weight of the secondary particles. In this case, a lithium-sulfur portion may be formed at a position where residual lithium exists on the surface of the secondary particles to have an appropriate lithium / sulfur content, and the layered structure of the primary particles may be substantially prevented from being damaged or collapsed as in the case of a water washing process.

[0128] In an exemplary embodiment, the amount of the sulfonyl compound added to the solvent may be 0.5-2.5 parts by weight relative to 100 parts by weight of the positive electrode active material. In this case, an appropriate amount of the sulfonyl compound sufficient to react with the residual lithium is added, so that the lithium-sulfur portion can be uniformly formed on the surface of the positive electrode active material, while preventing the sulfur content in the positive electrode active material from becoming too high. Therefore, the life characteristics of the battery can be improved while maintaining the power characteristics.

[0129] Next, a mixture including the secondary particles dry-coated with APT and an aqueous solution may be dried and second-calcined to obtain a positive active material.

[0130] Since the mixture contains a solvent contained in an aqueous solution, such as deionized water, the solvent may be removed by a drying process before the second calcination. The drying may be performed under a vacuum state and at a temperature of 100-200° C. for about 8-20 hours to remove the solvent and other volatile impurities.

[0131] The dried mixture can be placed in a calcining furnace for secondary calcination. During the second calcination, the ammonium paratungstate coated on the surface of the secondary particles melts at a high temperature above the melting point and flows into the interior of the secondary particles, thereby penetrating into the interface of the primary particles.

[0132] The second calcination may be performed in an oxygen atmosphere at a temperature of 200-500° C. In this case, the ammonium paratungstate on the surface of the secondary particles is fully melted and fully penetrates into the interface of the primary particles inside the secondary particles, thereby forming a lithium-tungsten compound.

[0133] According to an exemplary embodiment, a lithium secondary battery is provided, including: a positive electrode for a lithium secondary battery, the positive electrode for a lithium secondary battery including the positive electrode active material; and a negative electrode, the negative electrode being disposed opposite to the positive electrode.

[0134] Below, refer to Figure 1 and Figure 2 , a lithium secondary battery including a positive electrode including the above-mentioned positive electrode active material for lithium secondary battery is described.

[0135] Reference Figure 1 and Figure 2 The lithium secondary battery may include a positive electrode 100 and a negative electrode 130 , wherein the positive electrode 100 includes the positive electrode active material, and the negative electrode 130 is disposed opposite to the positive electrode 100 .

[0136] The positive electrode 100 may include a positive active material layer 110 formed by coating a slurry including the above-mentioned positive active material on a positive current collector 105 .

[0137] For example, the positive electrode slurry may be prepared by mixing and stirring the positive electrode active material with a binder, a conductive material and / or a dispersing material in a solvent. The positive electrode 100 may be manufactured by coating the positive electrode slurry on at least one side of the positive electrode collector 105, drying and rolling the positive electrode 100.

[0138] The positive electrode current collector 105 may include stainless steel, nickel, aluminum, titanium, or alloys thereof. The positive electrode current collector 105 may also include aluminum or stainless steel surface-treated with carbon, nickel, titanium, or silver.

[0139] The binder may include an organic binder such as polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, or a water-based binder such as styrene-butadiene rubber (SBR), and may be used together with a thickener such as carboxymethyl cellulose (CMC).

[0140] For example, a PVDF-based binder may be used as a binder for forming a positive electrode. In this case, the amount of the binder used to form the positive active material layer 110 may be reduced, and the amount of the positive active material may be relatively increased, thereby improving the power and capacity of the secondary battery.

[0141] The conductive material may be included to promote electron migration between active material particles. For example, the conductive material may include carbon-based conductive materials such as graphite, carbon black, graphene, and carbon nanotubes and / or metal-based conductive materials such as perovskite materials such as tin, tin oxide, titanium oxide, LaSrCoO3, and LaSrMnO3.

[0142] The negative electrode 130 may include a negative electrode collector 125 and a negative electrode active material layer 120 formed by coating a negative electrode active material on at least one side of the negative electrode collector 125 .

[0143] The negative electrode active material can be used without particular limitation as long as it is a material known in the technical field that can embed and de-embed lithium ions. For example, carbon-based materials such as crystalline carbon, amorphous carbon, carbon composites, and carbon fibers; lithium alloys; silicon or tin, etc. can be used. Examples of amorphous carbon include hard carbon, coke, mesocarbon microbeads (MCMB) calcined below 1500°C, and mesophase pitch-based carbon fibers (MPCF). Examples of crystalline carbon include graphite-based carbons such as natural graphite, graphitized coke, graphitized mesophase carbon microbeads, and graphitized mesophase pitch-based carbon fibers. Elements contained in the lithium alloy can include aluminum, zinc, bismuth, cadmium, antimony, silicon, lead, tin, gallium, or indium, etc.

[0144] The negative electrode current collector 125 may include, for example, gold, stainless steel, nickel, aluminum, titanium, copper, or alloys thereof, for example, copper or a copper alloy.

[0145] In some embodiments, the slurry may be prepared by mixing and stirring the negative active material with a binder, a conductive material and / or a dispersing material in a solvent. The negative electrode 130 may be manufactured by coating the slurry on the negative current collector, followed by drying and rolling.

[0146] The binder and the conductive material may use materials substantially the same as or similar to the above-mentioned materials. In some embodiments, for compatibility with the carbon-based active material, the binder used to form the negative electrode may include a water-based binder such as styrene-butadiene rubber (SBR), and may be used together with a thickener such as carboxymethyl cellulose (CMC).

[0147] In some embodiments, a separator 140 may be inserted between the positive electrode 100 and the negative electrode 130. The separator 140 may include a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, an ethylene / methacrylate copolymer, etc. The separator 140 may also include a non-woven fabric formed of a high melting point glass fiber, a polyethylene terephthalate fiber, etc.

[0148] According to an exemplary embodiment, a battery cell is defined by a positive electrode 100, a negative electrode 130, and a separator 140, and a plurality of the battery cells may be stacked to form, for example, an electrode assembly 150 in the form of a jelly roll. For example, the electrode assembly 150 may be formed by winding, laminating, folding, etc., of the separator 140.

[0149] The electrode assembly is housed in the case 160 together with an electrolyte, thereby defining a lithium secondary battery. According to an exemplary embodiment, the electrolyte may use a non-aqueous electrolyte.

[0150] The non-aqueous electrolyte may include a lithium salt as an electrolyte and an organic solvent. The lithium salt may be, for example, Li + X - Indicates that, as the anion of the lithium salt (X - ), we can exemplify F - , Cl - Br - ,I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - PF6 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - CF3SO3 - CF3CF2SO3 - 、(CF3SO2)2N - 、(FSO2)2N - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - 、(SF5)3C - 、(CF3SO2)3C - CF3(CF2)7SO3- CF3CO2 - 、CH3CO2 - 、SCN - and (CF3CF2SO2)2N - wait.

[0151] The organic solvent may be, for example, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), methyl propyl carbonate, dipropyl carbonate, dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, vinylene carbonate, cyclopentane, γ-butyrolactone, propylene sulfite, tetrahydrofuran, etc. These may be used alone or in combination of two or more.

[0152] like Figure 1 As shown, the tabs (positive tabs and negative tabs) may protrude from the positive current collector 105 and the negative current collector 125 belonging to each battery cell and extend to one side of the shell 160. The tabs may be fused with the one side of the shell 160 and form electrode leads (positive lead 107 and negative lead 127) extending to the outside of the shell 160 or exposed to the outside of the shell 160.

[0153] The lithium secondary battery may be manufactured in, for example, a cylindrical shape using a can, a prismatic shape, a pouch type, a coin shape, or the like.

[0154] The embodiments of the present invention are further described below with reference to specific experimental examples. The embodiments and comparative examples included in the experimental examples are only used to illustrate the present invention and are not used to limit the claims. Various modifications and variations can be made to the embodiments within the scope of the present invention and the technical concept, which is obvious to those skilled in the art, and it is natural that such modifications and variations belong to the scope of the claims.

[0155] Example 1

[0156] Preparation of positive electrode active material

[0157] Using distilled water that had been bubbling N2 for 24 hours to remove dissolved oxygen, NiSO4, CoSO4, and MnSO4 were mixed in a ratio of 0.885:0.090:0.025. The above solution was added to a reactor at 50°C, and a coprecipitation reaction was performed for 48 hours using NaOH and NH3·H2O as a precipitant and a chelating agent to obtain Ni as a transition metal precursor.0.885 Co 0.09 Mn 0.025 The obtained precursor was dried at 80°C for 12 hours and then dried again at 110°C for 12 hours.

[0158] Lithium hydroxide and the transition metal precursor were added to a dry high-speed mixer at a ratio of 1.01:1 and mixed uniformly for 5 minutes.

[0159] The mixture is placed in a calcining furnace, heated to 730-750°C at a rate of 2°C / min, and maintained at 730-750°C for 10 hours. During the heating and maintaining process, oxygen is continuously introduced at a flow rate of 20 L / min. After the calcination, the mixture is naturally cooled to room temperature, and crushed and classified to obtain lithium-nickel metal composite oxide particles.

[0160] Relative to the total weight of the lithium-nickel metal composite oxide particles, ammonium paratungstate (APT) is added to make the tungsten content reach 1000ppm, and aluminum oxide is added to make the aluminum content reach 1000ppm, mixed with a high-speed mixer for 5 minutes, and dry-coated on the lithium-nickel metal composite oxide particles.

[0161] To pure water (deionized water (DIW)) accounting for 5 wt % relative to the total weight of the dry-coated lithium-nickel metal composite oxide particles, 1.2 wt % of ammonium sulfate ((NH4)2SO4) powder is added relative to the total weight of the lithium-transition metal composite oxide particles, followed by stirring to allow the ammonium sulfate to fully dissolve in the pure water, thereby preparing an aqueous solution of a sulfonyl compound.

[0162] The dry-coated lithium-nickel metal composite oxide particles and the sulfonyl compound aqueous solution are mixed to prepare a mixture. The prepared mixture is dried in a vacuum oven at a temperature of 100-200°C for about 10 hours to remove moisture including the solvent. After drying, it is placed in a calcining furnace, oxygen is supplied at a flow rate of 20L / min, and the temperature is raised to 400°C at a heating rate of 2°C / min, and maintained at the raised temperature for 10 hours. After calcination, it is graded with 325 meshes to obtain positive electrode active material particles with D50=16μm or less.

[0163] Fabrication of coin-type half-cell

[0164] The coin-type half-cell was manufactured using the positive electrode active material. Specifically, the positive electrode active material, graphite as a conductive material, and PVDF as a binder were mixed in a composition of a mass ratio of 93:5:2 to prepare a positive electrode mixture, which was then coated on an aluminum current collector and dried. After that, rolling was performed so that the electrode density reached 3.0 g / cubic centimeter (g / cc), thereby manufacturing a positive electrode.

[0165] Lithium metal was used as the negative electrode.

[0166] The positive electrode and negative electrode manufactured as described above are notched into circles with diameters of Φ14 and Φ16, respectively, and stacked, and a separator (polyethylene, 13 μm thick) cut into Φ19 is inserted between the positive electrode and the negative electrode to form a battery cell. The battery cell is assembled by placing the battery cell in a coin battery outer material with a diameter of 20 mm and a height of 1.6 mm and injecting an electrolyte, and aging for more than 12 hours so that the electrolyte is impregnated into the electrode.

[0167] The electrolyte used was a solution prepared by dissolving 1 M LiPF6 in a mixed solvent of EC / EMC (30 / 70; volume ratio).

[0168] The coin-type half-cell manufactured as described above was subjected to formation charge and discharge (charge condition: CC-CV 0.1C 4.3V 0.005C CUT-OFF, discharge condition: CC 0.1C 3V CUT-OFF).

[0169] Example 2

[0170] A positive electrode active material and a coin-type half-cell were prepared by the same method as in Example 1, except that in Example 1, ammonium paratungstate (APT) was added relative to the total weight of the lithium-nickel metal composite oxide particles to achieve a tungsten content of 3000 ppm.

[0171] Example 3

[0172] A positive electrode active material and a coin-type half-cell were prepared by the same method as in Example 1, except that in Example 1, ammonium paratungstate (APT) was added relative to the total weight of the lithium-nickel metal composite oxide particles so that the tungsten content reached 10,000 ppm.

[0173] Comparative Example 1

[0174] A positive electrode active material and a coin-type half-cell were prepared by the same method as in Example 1, except that in Example 1, tungsten oxide (WO3) was added relative to the total weight of the lithium-nickel metal composite oxide particles so that the tungsten content reached 10000 ppm.

[0175] Comparative Example 2

[0176] A positive electrode active material and a coin-type half-cell were prepared by the same method as in Comparative Example 1, except that in Comparative Example 1, calcination was performed at a temperature of 500° C. after the mixture was dried.

[0177] Comparative Example 3

[0178] A positive electrode active material and a coin-type half-cell were prepared by the same method as in Comparative Example 1, except that in Comparative Example 1, calcination was performed at a temperature of 600° C. after drying the mixture.

[0179] Comparative Example 4

[0180] A positive electrode active material and a coin-type half-cell were prepared by the same method as in Comparative Example 1, except that in Comparative Example 1, calcination was performed at a temperature of 700° C. after the mixture was dried.

[0181] Reference example

[0182] A positive electrode active material and a coin-type half-cell were prepared by the same method as in Example 1, except that in Example 1, the lithium-nickel metal composite oxide particles were placed separately in a calcination furnace, oxygen was supplied at a flow rate of 20 L / min, and the temperature was increased to 400°C at a heating rate of 2°C / min, and the temperature was maintained at the increased temperature for 10 hours for calcination to prepare the positive electrode active material.

[0183] Experimental Example 1: TEM-EDS Analysis

[0184] Transmission Electron Microscope (TEM) images of the positive electrode active materials prepared in the examples and comparative examples were taken, and element mapping images and EDS spectra were obtained by energy dispersive X-ray spectroscopy (EDS). In the case of the EDS element mapping image, the energy regions of the tungsten element and the nickel element overlap (EDS spectrum, refer to Figures 8 to 12 ), so the tungsten energy area was partially changed, and corrections were made to reduce the background intensity effect to show the tungsten distribution.

[0185] Figures 3 to 7 TEM images and EDS tungsten element mapping images of the positive electrode active materials of Example 3 and Comparative Examples 1 to 4 are shown in FIG. Figure 3 The square-shaped portions 1, 2, and 3 of the upper left TEM image are enlarged and shown separately, and the EDS tungsten element mapping image is shown as an inset of each TEM image. Figures 4 to 7 The portion indicated by a square in the left TEM image is enlarged and shown on the right, and an EDS tungsten element mapping image is shown as an inset.

[0186] Figures 8 to 10 , which shows the EDS spectra of the surface and the interior of the positive electrode active material of Example 3, Fig.11 and Fig.12 , the EDS spectra of the surface and internal positions of the positive electrode active material of Comparative Example 1 are shown. Specifically, Figures 8 to 12 In the figure, the EDS spectrum of the portion indicated by the square in the left TEM image is shown on the right. Figures 8 to 12 The tungsten contents at the corresponding positions analyzed are shown in Table 1 below.

[0187] [Table 1]

[0188]

[0189] Reference Figure 3 It can be confirmed that the positive electrode active material of Example 3 is a secondary particle structure in the form of a plurality of primary particles aggregated, and it can be confirmed that tungsten exists at the primary particle interface at the positions of the square-shaped portions 1 and 2 as the surface portions of the secondary particles. In addition, it can be confirmed that tungsten also exists at an internal position at a depth of about 4.07 μm (about 50.9% of the radius) from the surface of the secondary particles in the positive electrode active material of Example 3.

[0190] Reference Figures 4 to 7 It can be confirmed that in the positive electrode active material of the comparative example, tungsten is distributed only on the surface of the particles, and there is no tungsten at a position closer to the inside than a depth of about 500 nm or more from the particle surface. In addition, it is confirmed that in the positive electrode active material of the comparative example, tungsten does not penetrate into the inside even if the calcination temperature is increased during the preparation process.

[0191] Reference Figures 8 to 10 It can be confirmed that tungsten exists on the surface and inside of the positive electrode active material of Example 3.

[0192] Reference Fig.11 , Fig.12From Table 1, it can be confirmed that in the positive electrode active material of Comparative Example 1, the tungsten content at a position inside the particle at a depth of 1 μm from the particle surface is about 0.93 wt %. Fig.12 From the EDS spectrum on the right, it can be confirmed that there is a high-intensity nickel peak at about 7.5 keV on the horizontal axis, and the tungsten peak is located nearby.

[0193] However, since the energy regions of tungsten and nickel overlap, the tungsten content of 0.93 wt% can be qualitatively explained as interference between the nickel peak and the tungsten peak. Considering that the resolution limit is 0.5 wt%, the tungsten content value is within the error range, so it is explained that there is almost no tungsten element.

[0194] That is, it can be confirmed that the positive electrode active material of the embodiment includes a permeation region, which is distributed from the surface of the secondary particles to the inside and contains a tungsten compound at the interface between the primary particles. On the other hand, it can be confirmed that in the positive electrode active material of the comparative example, tungsten exists only in the surface of the secondary particles, for example, in the region within a depth of about 10 nm from the surface, and tungsten does not exist in the interior of the particles.

[0195] Experimental Example 2: TEM-SAED Analysis

[0196] In order to analyze the crystal phase of the primary particles of the positive active material of Example 3 and Comparative Example 1, TEM-SAED (selected area electron diffraction) analysis was performed. The positive active material particles of Example 3 and Comparative Example 1 were FIB processed to make samples, and then the selected area aperture was specified for the cross section using TEM, and then the diffraction mode was entered to obtain a diffraction image. The layered structure was fitted with the zone axis

[010] , and the rock salt phase structure was fitted with the zone axis

[110] to confirm the SAED image.

[0197] Fig.13 and Fig.14 TEM images and SAED images (insets) of Example 3 and Comparative Example 1 are shown in FIG.

[0198] Reference Fig.13 In the positive electrode active material of Example 3, it was confirmed that the primary particles contained a layered structure and a rock salt phase, and it was confirmed that the rock salt phase was formed in a region with a thickness of about 8.93 nm.

[0199] Reference Fig.14 It can be confirmed that in the positive electrode active material of Comparative Example 1, the primary particles also contain a layered structure and a rock salt phase, and the rock salt phase is formed in a region with a thickness of about 10.8 nm.

[0200] Experimental Example 3: XPS Surface Analysis

[0201] The components of the positive electrode active materials of Example 3 and Comparative Example at a depth of 10 nm from the particle surface were analyzed by X-ray photoelectron spectroscopy. The XPS analysis conditions were as follows.

[0202] - Equipment used: ESCALAB 250Xi (Thermo Fisher Scientific)

[0203] 1) X-ray type: Source - Al kα, 1486.68 eV, beam size 900 μm

[0204] 2) Scanning conditions (including Al2p, Na1s):

[0205] Number of scans: 20 to 50

[0206] Pass energy: 20eV

[0207] Dwell time: 50-100ms

[0208] Energy level: 0.1eV

[0209] The XPS etching depth was 10 nm, and the W 4f ... 7 / 2 The content data of tungsten element was obtained by calculating the regional integral value of the peak, and the relative standard deviation (RSD) was obtained by dividing the standard deviation of the data by the average value, and is shown in Table 2 below.

[0210] [Table 2]

[0211] Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 RSD(%) 23.5 8.7 5.9 9.9 5.4

[0212] Referring to Table 2, it can be confirmed that the positive electrode active material of Example 3 has a high RSD value of 23.5%. On the other hand, in the case of Comparative Examples 1 to 4, it can be confirmed that the RSD values ​​are less than 10%.

[0213] In the preparation process of the positive active material of Example 3, a part of the tungsten located on the outer surface of the particle can penetrate into the inside. However, tungsten penetrates into the interface between the primary particles, and tungsten can penetrate into the inside of the secondary particles in different amounts and at different depths depending on the positions of the outer surface of the secondary particles. Therefore, the distribution of tungsten on the surface of the positive active material particles of Example 3 may be uneven.

[0214] On the other hand, in the case of the positive electrode active material of the comparative example, tungsten does not penetrate into the positive electrode active material particles, but remains on the surface of the positive electrode active material as it is present on the particle surface by dry coating during the preparation process.

[0215] Therefore, a similar level of distribution amount of tungsten is detected at any position on the surface of the positive electrode active material particle, and thus a low RSD value of 10% or less is shown.

[0216] Experimental Example 4: Measurement and Evaluation of Resistivity

[0217] In order to measure the resistivity, the positive active materials prepared in the examples, comparative examples and reference examples were mixed with a binder (PVDF) and coated on an Al foil to prepare an electrode.

[0218] In order to analyze the inherent conductivity of the positive electrode active material and eliminate the effect of improving the conductivity brought about by the conductive material, the electrode is manufactured by mixing only the minimum content (1 weight %) of the binder, which is different from the components of ordinary electrodes.

[0219] The cut cross-section of the electrode was analyzed using AFM in SSRM mode to confirm the resistance distribution.

[0220] Specifically, the positive electrode manufactured in the embodiment, comparative example and reference example was cut, and a needle tip coated with a conductive material (contact area radius of 30 nm) was brought into contact with a 200nm×200nm area in the cross section using Bruker's AFM, a voltage of 3V was applied, and analysis was performed in SSRM mode to obtain an extended resistance distribution image.

[0221] Fig.15 SSRM extended resistance distribution images of the positive electrode cross sections of Examples 1 to 3, Comparative Examples 1 to 4, and the reference example are shown in FIG.

[0222] Reference Fig.15 , in the extended resistance distribution image, the darker the color, the lower the resistance, and it can be confirmed that the resistance of the surrounding area outside the positive electrode active material particles is very high, so it appears bright. In particular, in the case of Examples 1 to 3, it can be confirmed that each cross section presents a bright dark color. In the case of the comparative example, bright transverse scratches appear on the cross section of the active material. This is because there is a surface with an uneven thickness in the processed electrode cross section, and this part absorbs current, thereby showing high resistance. Therefore, in order to make an accurate comparison, this part is excluded, and only the clean surface part is added to the resistance average value and the value is calculated.

[0223] The average value of the spreading resistance value of the 200 nm×200 nm region in the cross section of each positive electrode active material particle was obtained from the spreading resistance distribution image, and the resistivity was calculated according to the following formula 1 and is shown in the following Table 3. In addition, Fig.16 The average values ​​of the spreading resistances of the positive electrode active materials of Examples 1 to 3, Comparative Example 1 and Reference Example are shown in FIG.

[0224] [Formula 1]

[0225] ρ=4×r×R sp

[0226] In the above formula 1, ρ is the resistivity, R sp is the average value of the spreading resistance of the positive electrode active material, r is the contact radius of the AFM tip (30nm = 30*10 -7 cm).

[0227] [Table 3]

[0228] Resistivity (Ω·cm) Example 1 <![CDATA[8.11×10 1 (81.1)]]> Example 2 <![CDATA[4.26×10 1 (42.6)]]> Example 3 <![CDATA[1.02×10 2 (102)]]> Comparative Example 1 <![CDATA[1.29×10 2 (129)]]> Comparative Example 2 <![CDATA[1.13×10 2 (113)]]> Comparative Example 3 <![CDATA[1.28×10 2 (128)]]> Comparative Example 4 <![CDATA[1.27×10 2 (127)]]> Reference example <![CDATA[2.18×10 1 (21.8)]]>

[0229] Refer to Table 3 and Fig.16 It can be confirmed that the resistivity of the positive electrode active material of the example is lower than the resistivity of the positive electrode active material of the comparative example.

[0230] In addition, it can be confirmed that the resistivity of the positive electrode of the reference example not containing tungsten is low. This seems to be because, as confirmed in Experimental Example 2, the positive electrode active materials of the examples and comparative examples contain a rock salt phase, and the rock salt phase is a non-conductor and increases the resistance of the positive electrode active material.

[0231] Experimental Example 5: Evaluation of Battery Characteristics

[0232] (1) Evaluation of initial capacity efficiency

[0233] The coin-type half-cells manufactured according to the examples and comparative examples were charged in a chamber at 25° C. (CC-CV 0.1C 4.3V 0.005C cutoff) and the battery capacity (initial charge capacity) was measured, and then discharged (CC 0.1C 3.0V cutoff) and the battery capacity (initial discharge capacity) was measured.

[0234] The initial capacity efficiency was evaluated by converting the value of the measured initial discharge capacity divided by the measured initial charge capacity into a percentage (%).

[0235] (2) Evaluation of life characteristics during repeated charge and discharge

[0236] The coin-type half-cells according to the examples and comparative examples were charged (CC / CV 0.5C 4.3V 0.05C cutoff) and discharged (CC 1.0C 3.0V cutoff) 300 times, and the capacity retention ratio was obtained by dividing the 300th discharge capacity by the 1st discharge capacity.

[0237] [Table 4]

[0238]

[0239]

[0240] Referring to Table 4, it can be confirmed that in the examples, as the tungsten content increases, the initial discharge capacity slightly decreases. This is because the rock salt phase formed by adding tungsten leads to a decrease in discharge capacity, which is an inevitable trade-off phenomenon.

[0241] In addition, it can be confirmed that in Examples 1 to 3, as the tungsten content increases, the difference in initial charge and discharge efficiency is within 1%, and compared with the reference example without tungsten, the initial efficiency is improved by 0.5-1.4%, and compared with the comparative example, the efficiency is more excellent.

[0242] In particular, in the case of the comparative example, the range of the optimal heat treatment temperature according to the transition metal composition used to form the crystal structure of the positive electrode active material was exceeded, and an unpreferable crystal phase (e.g., a rock salt phase such as NiO) was formed, resulting in a sharp decrease in charge and discharge efficiency and discharge capacity.

[0243] Therefore, in the comparative example, as the heat treatment temperature increases, the capacity retention rate increases, thereby possibly showing that the life characteristics are improved, but since the discharge capacity of the battery is maintained at a low level, this is an unpreferable battery characteristic.

[0244] On the other hand, in the examples, the initial charge and discharge efficiency was equal to or better than that of the reference example and the comparative example, and the capacity retention rate after 300 cycles was about 1-3.8% higher, thus showing that the life characteristics were improved.

[0245] Furthermore, when the results of Example 3 and Comparative Example 1 having the same heat treatment temperature and the same tungsten content are compared, the initial charge and discharge efficiency and discharge capacity are at the same level, but the capacity retention rate differs by about 2%.

[0246] This can be explained by the fact that since APT penetrates into the active material, a tungsten penetration region exists at a maximum of 55% of the particle radius, thereby improving the structural stability of the positive electrode active material particles and thus improving the battery life characteristics.

Claims

1. A positive electrode active material for a lithium secondary battery, the positive electrode active material for a lithium secondary battery comprising lithium-nickel metal composite oxide particles, the lithium-nickel metal composite oxide particles having a secondary particle form of a plurality of primary particles aggregated, The lithium-nickel metal composite oxide particles include a permeation region formed in a region from a surface to a position of 70% or less of a radius in a central direction of the particles and containing a tungsten compound at an interface between the primary particles, The relative standard deviation (RSD) value of the results of measuring the tungsten content 10 times at positions different from each other at a depth of 10 nm from the surface of the secondary particles by X-ray photoelectron spectroscopy was 10-40%.

2. The positive electrode active material for lithium secondary battery according to claim 1, wherein The relative standard deviation value is 20-30%.

3. The positive electrode active material for lithium secondary battery according to claim 1, wherein The thickness of the permeable region corresponds to 10-55% of the radius of the secondary particle from the surface of the secondary particle to the center direction of the particle.

4. The positive electrode active material for lithium secondary battery according to claim 1, wherein The lithium-nickel metal composite oxide particles include a chemical structure represented by the following Chemical Formula 1: [Chemical formula 1] Li a [Ni b Co c Mr d X y ]O e In the chemical formula 1, X includes at least one of W, S, Al, Ti, Sr, Zr, P and K, 0.5 <a<1.5,0.8<b≤1,0<c<0.1,0<d<0.1,1.5<e<2.5,0<y<0.1。 5. The positive electrode active material for lithium secondary battery according to claim 1, wherein The tungsten compound includes lithium-tungsten oxide.

6. The positive electrode active material for lithium secondary battery according to claim 5, wherein The lithium-tungsten oxide is represented by the following chemical formula 2: [Chemical formula 2] Li x W y O z In the chemical formula 2, 0 <x≤3,0<y≤5,0<z≤8。 7. The positive electrode active material for lithium secondary battery according to claim 1, wherein The content of tungsten in the total weight of the lithium-nickel metal composite oxide particles is 500-10000 ppm.

8. The positive electrode active material for lithium secondary battery according to claim 1, wherein The content of tungsten in the total weight of the lithium-nickel metal composite oxide particles is 1000-5000 ppm.

9. The positive electrode active material for lithium secondary battery according to claim 1, wherein At least a portion of the plurality of primary particles in the permeation region includes a rock salt phase region formed from the surface along the center direction, and the thickness of the rock salt phase region is 5-10 nm from the surface of the primary particle to the center direction.

10. The positive electrode active material for lithium secondary battery according to claim 1, wherein The average particle size D50 of the lithium-nickel metal composite oxide particles is 10-30 μm.

11. The positive electrode active material for lithium secondary battery according to claim 1, wherein The resistivity of the positive electrode active material for lithium secondary battery is defined by the following formula 1: [Formula 1] 0ρ=4×r×Rsp In the above formula 1, ρ is the resistivity, Rs p is the average value of the spreading resistance of the lithium-nickel metal composite oxide particles measured from a spreading resistance distribution image, wherein the spreading resistance distribution image is obtained by contacting a needle tip coated with a conductive component of an atomic force microscope (AFM) to an area of ​​200 nm×200 nm in a cross section of a positive electrode containing the positive electrode active material and applying a voltage of 3 V and photographing in a scanning spreading resistance microscope (SSRM) mode, r is the contact radius of the needle tip.

12. The positive electrode active material for lithium secondary battery according to claim 11, wherein The resistivity is 40-105Ω·cm.

13. A lithium secondary battery comprising: A positive electrode for a lithium secondary battery, the positive electrode for a lithium secondary battery comprising the positive electrode active material according to claim 1; and A negative electrode is arranged opposite to the positive electrode.