A universal crosslinking agent and hydrogel that can be degraded by oxidation-reduction, and their preparation and application
Through the universal crosslinking agent synthesized by selenocycindihydrochloride and acrylic acid, the problem of degradation rate and biocompatibility of hydrogel crosslinking agents in biological applications is solved, and the biocompatibility and degradation rate are achieved. Controllability, suitable for drug release and tissue engineering, with wide application prospects.
Patent Information
- Application Number
- CN202410150409.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-02
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-02-02
AI Technical Summary
The existing hydrogel crosslinking agents are difficult to meet the requirements of versatility, good biocompatibility, controllable degradation speed, and mild degradation conditions at the same time, which limits their application in the medical and biotechnology fields.
Two general crosslinking agents with carbon-carbon double bonds synthesized by selenocycindamine dihydrochloride and acrylic acid in one step are used to control the mechanical properties and degradation time of the hydrogel by adjusting the crosslinking agent concentration, and through redox reaction Achieve hydrogel degradation.
It has achieved the non-toxic, good biocompatible and controllable degradation speed of hydrogel. It is suitable for in vivo drug release and tissue engineering, and has a wide market application prospect.
Smart Images

Figure CN118063366B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrogels, and in particular to a redox-degradable universal cross-linking agent, a hydrogel, and preparation and application thereof. Background Art
[0002] Hydrogel is a multifunctional polymer material with a unique three-dimensional network structure that can absorb and retain a large amount of water while still maintaining its solid form. This material can absorb water equivalent to tens to thousands of times its own weight, but still maintains structural stability and will not dissolve in water. Hydrogels are widely used in drug delivery systems, wound care, tissue engineering, etc. due to their good biocompatibility, adjustable physical and chemical properties, and characteristics similar to biological tissues. For example, hydrogels can be used as drug carriers and sustained-release systems to help drugs reach target sites more effectively and reduce side effects.
[0003] Stimuli-degradable hydrogels are a widely studied type of hydrogel with the unique ability to change their physical or chemical properties under specific stimuli (such as pH changes, temperature changes, light, electromagnetic fields, enzyme action, etc.), thereby causing the degradation of the material. These hydrogels are usually composed of cross-linked polymer networks that can absorb and retain large amounts of water while maintaining their structural integrity when not stimulated. The design of stimuli-degradable hydrogels enables them to respond precisely to environmental changes, a feature that is particularly important in the medical and biotechnology fields. For example, in drug delivery systems, such hydrogels can be designed to release drugs when they reach the disease site (such as the acidic environment of the tumor microenvironment). Similarly, in tissue engineering, they can serve as scaffolds for cell growth, gradually degrading and being replaced as new tissue is formed. The design and synthesis of such hydrogels involves precise control of their responsiveness, biocompatibility, mechanical strength, and degradation rate. In biomedical applications, these hydrogels must have good biocompatibility to ensure that they do not cause immune or toxic reactions. In addition, their degradation products should be non-toxic and can be safely absorbed or eliminated by the human body.
[0004] However, the development and application of stimulated degradable hydrogels face many challenges. First, the slow degradation and harsh degradation stimulus field conditions limit the application of most stimulus-responsive hydrogels in vivo. The degradation rate of the hydrogel must match the therapeutic needs to ensure effective drug release and tissue regeneration. Secondly, maintaining the mechanical stability of the hydrogel in vivo is also a major challenge, especially in dynamic and complex organisms. In addition, the current in vivo redox degradation is mainly based on hydrogels constructed based on disulfide bonds and boronic acid bonds, which limits the use of functional monomers. Therefore, it is particularly important to develop a universal cross-linker to prepare hydrogels with different functions, while meeting the requirements of non-toxicity, good biocompatibility, controllable degradation rate, mild degradation conditions, and controllable mechanical properties. Summary of the invention
[0005] The purpose of the present invention is to provide a universal cross-linking agent capable of redox degradation, aiming to solve the problem that the existing hydrogel cross-linking agents cannot simultaneously meet the requirements of versatility, good biocompatibility, controllable degradation rate, mild degradation conditions, etc.
[0006] Another object of the present invention is to provide a method for preparing the cross-linking agent for the degradable hydrogel.
[0007] Another object of the present invention is to provide a redox-degradable hydrogel based on the above cross-linking agent.
[0008] Another object of the present invention is to provide a method for preparing a redox-degradable hydrogel based on the crosslinking agent.
[0009] Another object of the present invention is to provide an application of a redox-degradable hydrogel based on the cross-linking agent.
[0010] To this end, the first technical solution of the present invention is: a redox-degradable universal cross-linking agent, which is composed of 0.75-1.5 parts of selenocystamine dihydrochloride and 3 equivalents of acrylic acid.
[0011] The second technical scheme of the present invention is: a method for preparing the above-mentioned crosslinking agent for degradable hydrogel, the steps of which are as follows: adding selenocystamine dihydrochloride and acrylic acid to a mixed solution of 1 water: 4-8 dimethylformamide (DMF); adding 3-9 equivalents of N, N-diisopropylethylamine and 1-5 equivalents of azodimethoxytriphenylphosphine hydrochloride in sequence, stirring and reacting at room temperature for 30 minutes; after removing the solvent by rotary evaporation under reduced pressure, passing the silica gel column with a developing agent of dichloromethane: methanol = 15-30:1, and removing the solvent by rotary evaporation of the eluent to obtain a redox-degradable universal crosslinking agent.
[0012] The third technical solution of the present invention is: a redox-degradable hydrogel based on the above crosslinking agent, comprising 0.2-1 parts of hydrogel monomer, 1.8-5 parts of water, 0.002-0.01 parts of initiator and 0.002-0.02 parts of crosslinking agent in parts by weight.
[0013] On the basis of the above scheme and as a preferred scheme of the above scheme: the hydrogel monomer includes a mixture of one or more of acrylamide monomer, acrylic acid monomer, N-isopropylacrylamide monomer and N, N-dimethylacrylamide monomer.
[0014] On the basis of the above scheme and as a preferred scheme of the above scheme: the initiator includes a thermal initiator and a photoinitiator.
[0015] On the basis of the above scheme and as a preferred scheme of the above scheme: the thermal initiator includes azobisisobutylamidine hydrochloride, azobisisobutylimidazoline hydrochloride, azobiscyanovaleric acid, azobisisopropylimidazoline or azobisisobutyronitrile.
[0016] On the basis of the above scheme and as a preferred scheme of the above scheme: the photoinitiator includes phenyl (2,4,6-trimethylbenzoyl) lithium phosphate (LAP), diphenyl-(2,4,6-trimethylbenzoyl) phosphine oxide (TPO) or dibenzoyl peroxide (BPO).
[0017] The fourth technical solution of the present invention is: a method for preparing a redox-degradable hydrogel based on the above-mentioned crosslinking agent, the steps are as follows: adding a hydrogel monomer to water and stirring evenly, then adding an initiator and the above-mentioned crosslinking agent in sequence, stirring evenly, and removing bubbles in vacuo; placing the mixed solution at 50-70°C for 2-5h, or placing it under UV light for 5-10min to obtain a redox-degradable hydrogel, or using a DLP printer to print a complex structure hydrogel.
[0018] The fifth technical solution of the present invention is: a redox-degradable hydrogel based on the above cross-linking agent is used for catheter coating and drug release.
[0019] The present invention synthesizes two sections of universal crosslinking agents with carbon-carbon double bonds in one step by utilizing selenocystamine dihydrochloride and acrylic acid, thereby being able to achieve chemical crosslinking, and by adding crosslinking agents of different concentrations into the gel system, the mechanical properties and degradation time of the final hydrogel can be changed.
[0020] The degradation of crosslinking agent is because it contains diselenide bond, the bond energy of which is 172, which is relatively small. It can react with hydrogen peroxide to break, and the reaction speed is fast. According to the reaction kinetics, the degradation speed is related to the concentration of reactants, that is, the concentration of crosslinking agent and hydrogen peroxide, that is, the higher the concentration, the faster the reaction.
[0021] The preparation method of the cross-linking agent of the present invention is simple and easy to control, and can realize large-scale production. The prepared cross-linking agent is non-toxic and has good biocompatibility and biodegradability.
[0022] The hydrogel prepared by the above method is responsive to redox. When the hydrogel is immersed in hydrogen peroxide or ammonium persulfate solution, the crosslinking agent of the hydrogel breaks due to the redox reaction, thereby changing the morphology of the hydrogel.
[0023] In addition, the above hydrogels can be efficiently prepared into complex structures through 3D printing, and can also load hydrophilic or hydrophobic drugs as carriers for drug release. Due to the heterogeneous redox properties of the crosslinker, it can be used as a targeted drug carrier in high redox environments such as diabetic wounds, psoriasis, and cancer cell environments.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The cross-linking agent used in degradable hydrogels is universal, so the hydrogels can be given functionality by adding different monomers.
[0026] 2. The cross-linking agent can realize the preparation of degradable hydrogel by chemical cross-linking method, and the concentration of cross-linking agent and degradation liquid can be adjusted to achieve adjustable degradation time.
[0027] 3. The preparation method of the cross-linking agent and the hydrogel is simple, and the hydrogel is non-toxic, has good biocompatibility, controllable degradation rate, mild degradation conditions, and controllable mechanical properties. It can be used for in vivo drug release, wound care, and tissue engineering, and has good market application and promotion prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 Stress-strain diagram of the hydrogels prepared in Examples 1-3.
[0029] Figure 2 Actual pictures of the hydrogel prepared in Example 2 before and after degradation in pure water, 0.01%, 0.1% and 1% hydrogen peroxide for 5 hours; (a) pure water, (b) hydrogen peroxide concentration of 0.01%, (c) hydrogen peroxide concentration of 0.1%, (d) hydrogen peroxide concentration of 1%.
[0030] Figure 3 Actual pictures of the 3D printed complex structure hydrogel prepared in Example 4 before and after degradation in 0.1% hydrogen peroxide for 2h and 4h.
[0031] Figure 4 Actual pictures of the hydrogel prepared in Example 5 before and after degradation in 0.1% hydrogen peroxide and pure water for 4 hours; (a) pure water, (b) hydrogen peroxide concentration 0.1%.
[0032] Figure 5 Actual pictures of the hydrogel prepared in Example 6 before and after degradation in 0.1% hydrogen peroxide and pure water for 3h and 8h; (a) pure water, (b) hydrogen peroxide concentration 0.1%.
[0033] Figure 6 Actual pictures of the hydrogel prepared in Example 7 before and after degradation in 0.1% hydrogen peroxide and pure water for 3h and 8h; (a) pure water, (b) hydrogen peroxide concentration 0.1%.
[0034] Figure 7 This is a diagram showing the cytotoxicity test results of the hydrogel material prepared in Example 8. DETAILED DESCRIPTION
[0035] The following is a further detailed description in conjunction with the accompanying drawings and embodiments of the present invention.
[0036] Example 1
[0037] The preparation of redox-degradable polyacrylamide hydrogel comprises the following steps:
[0038] (1) Preparation of a redox-degradable cross-linking agent: 0.4 g of selenocystamine dihydrochloride and 3 equivalents of acrylic acid were added to a mixed solution of 1 ml of water and 4 ml of dimethylformamide, and 6 equivalents of N,N-diisopropylethylamine and 3 equivalents of azodimethoxytriphenylphosphine hydrochloride were added in sequence. The mixture was stirred at room temperature for 30 min, and the solvent was removed by rotary evaporation under reduced pressure. The mixture was passed through a silica gel column with a developing solvent of dichloromethane:methanol (20:1). The eluent was rotary evaporated to remove the solvent to obtain a redox-degradable universal cross-linking agent.
[0039] In this embodiment, two universal cross-linking agents with carbon-carbon double bonds are synthesized in one step by using selenocystamine dihydrochloride and acrylic acid (AAC+), so chemical cross-linking can be achieved, and the mechanical properties and degradation time of the final hydrogel can be changed by adding different concentrations of cross-linking agents in the gel system. The cross-linking agent degradation is because the cross-linking agent contains diselenide bonds, and the bond energy of the diselenide bonds is 172kJ / mol, which is relatively small, and can react and break with hydrogen peroxide, and the reaction speed is fast. According to the reaction kinetics, the degradation speed is related to the concentration of the reactants, that is, the concentration of the cross-linking agent and the concentration of hydrogen peroxide, that is, the more concentrated the reaction, the faster the reaction. The following is the synthesis and degradation principle of the cross-linking agent:
[0040]
[0041] Se-Se+H 2 O 2 →-SeOOH+H 2 O
[0042] (2) Preparation of redox hydrogel: 1.42 g acrylamide monomer was added to 5 ml water and stirred evenly, then 200 μl 2.5% LAP solution and 5 mg crosslinker prepared in step (1) were added in sequence, the molar ratio of crosslinker to monomer was 0.0007, stirred evenly, and air bubbles were removed by vacuum, and then irradiated with 385 nm ultraviolet light for 5 min to obtain a hydrogel with redox-stimulated degradation. The tensile properties were tested as follows: Figure 1 Middle curve 1.
[0043] Example 2
[0044] The preparation and degradation of redox-degradable polyacrylamide hydrogels include the following steps:
[0045] (1) Same as step (1) in Example 1.
[0046] (2) Add 1.42 g of acrylamide monomer to 5 ml of water and stir evenly, then add 200 μl of 2.5% LAP solution and 10 mg of the crosslinker prepared in step (1) in sequence, the molar ratio of the crosslinker to the monomer is 0.0014, stir evenly, remove bubbles in vacuum, and then irradiate with 385 nm ultraviolet light for 5 min to obtain a hydrogel with redox-stimulated degradation. Test the tensile properties as follows Figure 1 Middle curve 2.
[0047] Redox degradation test of hydrogel materials: Prepare 5 ml of hydrogen peroxide solution with concentrations of 0, 0.01%, 0.1% and 1%, add it to the bottle containing the above hydrogel, react for 5 hours at room temperature of 20 degrees, and then turn the bottle upside down to observe the degradation of the hydrogel. Figure 2 It can be seen that the hydrogel only swelled in pure water (a), but degraded under the oxidation of hydrogen peroxide, and the degree of degradation of the hydrogel increased with the increase of hydrogen peroxide concentration. Therefore, it is shown that the hydrogel prepared by this method has redox-stimulated degradation characteristics.
[0048] Example 3
[0049] The preparation of redox-degradable polyacrylamide hydrogel comprises the following steps:
[0050] (1) Same as step (1) in Example 1.
[0051] (2) Add 1.42 g of acrylamide monomer to 5 ml of water and stir evenly, then add 200 μl of 2.5% LAP solution and 20 mg of the crosslinker prepared in step (1) in sequence, the molar ratio of the crosslinker to the monomer is 0.0028, stir evenly, remove bubbles in vacuum, and then irradiate with 385 nm ultraviolet light for 5 min to obtain a hydrogel with redox-stimulated degradation. Test the tensile properties as follows Figure 1Middle curve 3.
[0052] Example 4
[0053] 3D printing redox degradable polyacrylamide hydrogel preparation and degradation, including the following steps:
[0054] (1) Same as step (1) in Example 1.
[0055] (2) Preparation of 3D printing precursor solution: 2 g of acrylamide monomer was added to 5 ml of water and stirred evenly, and then 800 μl of 2.5% LAP solution and 20 mg of the above cross-linking agent were added in sequence, stirred evenly, and the bubbles were removed by vacuum. Then, a complex structure hydrogel was printed using a DLP printer to obtain a hydrogel with redox-stimulated degradation.
[0056] (3) Redox degradation test of 3D printed hydrogel materials: The above 3D printed hydrogel was placed in a glass dish, 10 ml of 0.1% hydrogen peroxide was added, and the degradation of the hydrogel was observed at intervals of 0 h, 2 h, and 4 h. Figure 3 It can be seen that after 4 hours, the hydrogel could no longer support its own shape and collapsed and degraded.
[0057] Example 5
[0058] The preparation of redox-degradable polyacrylic acid hydrogel comprises the following steps:
[0059] (1) Same as step (1) in Example 1.
[0060] (2) Preparation of redox hydrogel: 1.44 g of acrylic acid monomer was added to 3.5 ml of water and stirred evenly, and then 200 μl of 2.5% LAP solution and 5 mg of the cross-linking agent prepared in step (1) were added in sequence, with the molar ratio of the cross-linking agent to the monomer being 0.0007. The mixture was stirred evenly, and bubbles were removed by vacuum. The mixture was then irradiated with 385 nm ultraviolet light for 5 min to obtain a hydrogel with redox-stimulated degradation.
[0061] Redox degradation test of hydrogel materials: Prepare 3 ml of hydrogen peroxide solution with concentrations of 0 and 0.1%, add it to the bottle with hydrogel, react at room temperature 20℃ for 4 hours, then turn the bottle upside down to observe the degradation of hydrogel. Figure 4 It can be seen that the hydrogel only swelled in pure water, but degraded under the oxidation of hydrogen peroxide. This shows the versatility of the above crosslinking agents and their responsiveness to oxidative degradation stimuli.
[0062] Example 6
[0063] The preparation and degradation of redox-degradable poly (N-isopropylacrylamide) hydrogel comprises the following steps:
[0064] (1) Same as Example 1(1).
[0065] (2) Preparation of redox hydrogel: 0.565 g of N-isopropylacrylamide monomer was added to 5 ml of water and stirred evenly, and then 200 μl of 2.5% LAP solution and 10 mg of the above cross-linking agent were added in sequence and stirred evenly. The bubbles were removed by vacuum, and then irradiated with 385 nm ultraviolet light for 5 min to obtain a hydrogel with redox-stimulated degradation.
[0066] (3) Redox degradation test of hydrogel materials: Prepare 3 ml of hydrogen peroxide solution with concentrations of 0 and 0.1%, add it to the bottle containing hydrogel, react at room temperature 20°C for 4 hours, then turn the bottle upside down to observe the degradation of hydrogel. Figure 5 It can be seen that the hydrogel only swelled in pure water, but degraded under the oxidation of hydrogen peroxide. This shows the versatility of the above crosslinking agent and the responsiveness of poly (N-isopropylacrylamide) hydrogel to oxidative degradation stimulus.
[0067] Example 7
[0068] Preparation and degradation of thermal polymerization redox degradable polyacrylamide hydrogel
[0069] (1) Same as Example 1(1).
[0070] (2) Preparation of thermally polymerized hydrogel: 1.42 g of acrylamide monomer was added to 5 ml of water and stirred evenly. Then 7 mg of azobiscyanovaleric acid and 10 mg of the above cross-linking agent were added in sequence and stirred evenly. The bubbles were removed by vacuum and then thermally polymerized in an oven at 70 °C for 4 h to obtain a hydrogel with redox-stimulated degradation.
[0071] (3) Redox degradation test of hydrogel materials: Prepare 5 ml of hydrogen peroxide solution with concentrations of 0 and 0.1%, add it to the bottle containing hydrogel, react at room temperature 20°C for 4 hours, then turn the bottle upside down to observe the degradation of hydrogel. Figure 6 It can be seen that the hydrogel only swelled in pure water, but degraded under the oxidation of hydrogen peroxide. This shows that the above crosslinking agent can not only photopolymerize the hydrogel but also thermally polymerize the hydrogel, and the obtained hydrogel has good mechanical properties and degradability.
[0072] Example 8
[0073] Cytotoxicity experiments of hydrogel materials
[0074] (1) Preparation of hydrogel network: Prepare 5 ml of an aqueous solution of 15% acrylic acid and 1% succinimidyl acrylate, add 150 μl of 2.5% LAP solution and 20 mg of a cross-linking agent, stir evenly, remove bubbles by vacuum, and then irradiate with 385 nm ultraviolet light for 8 min to obtain a single network hydrogel. Prepare 100 ml of an aqueous solution of 30% acrylic acid and 1% succinimidyl acrylate, add 3000 μl of 2.5% LAP solution and 80 mg of a cross-linking agent, stir evenly, and remove bubbles by vacuum. Then soak the single network hydrogel in the above solution for 24 h to fully swell, and then irradiate with 385 nm ultraviolet light for 8 min to obtain a double network hydrogel. The double network hydrogel was soaked in pure water for 3 days to remove unreacted monomers, with the water being changed every 24 h.
[0075] (2) The double network hydrogel material was subjected to a NIH3T3 mouse fibroblast cytotoxicity test, and the experimental method was as follows:
[0076] The experiment was divided into a control group and an experimental group, with 5 replicate wells set up in a 24-well plate. The CCK-8 method was used to determine the toxic effects of the materials on NIH3T3 cells. The material samples were first sterilized by ultraviolet irradiation and placed in a 24-well plate. NIH3T3 cells in the logarithmic growth phase were taken for cell counting and cell concentration was adjusted to 5×10 4 Cells / well were seeded on the material, 5% CO 2 , and cultured overnight in a 37°C constant temperature incubator. Cultured for 24 h according to the above grouping treatment, and the culture medium was removed. Each well was washed three times with PBS, and a culture medium containing 10% CCK-8 was added at 500 μL / well, and 5% CO 2 , cultured in a 37°C constant temperature incubator for 2 hours. After taking out the material, the absorbance value at 450nm was detected by an enzyme marker to analyze the toxic effect of the material on NIH3T3 cells.
[0077] like Figure 7 The hydrogel has good biocompatibility, in that after 24 hours of cell co-culture, the cell survival rate can reach more than 98%, indicating that the hydrogel has great application prospects in vivo.
[0078] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A redox degradable hydrogel, characterized in that: The invention comprises, by weight, 0.2-1 parts of hydrogel monomer, 1.8-5 parts of water, 0.002-0.01 parts of initiator and 0.002-0.02 parts of crosslinking agent; The preparation method of the crosslinking agent is as follows: 0.75-1.5 parts of selenocystamine dihydrochloride and 3 equivalents of acrylic acid are added to a mixed solution of 1 water: 4-8 dimethylformamide; 3-9 equivalents of N, N-diisopropylethylamine and 1-5 equivalents of diethyl azodicarboxylate-triphenylphosphine are added in sequence, and the mixture is stirred at room temperature for 30 minutes to react; after the solvent is removed by rotary evaporation under reduced pressure, the mixture is passed through a silica gel column with a developing agent of dichloromethane: methanol = 15-30:1, and the eluent is rotary evaporated to remove the solvent, thereby obtaining a redox-degradable universal crosslinking agent; The preparation method of the hydrogel is as follows: adding the hydrogel monomer to water and stirring evenly, then adding the initiator and the above-mentioned cross-linking agent in sequence, stirring evenly, and removing bubbles by vacuum; placing the mixed solution at 50-70°C for 2-5 hours, or placing it under UV light for 5-10 minutes to obtain a redox-degradable hydrogel, or using a DLP printer to print a complex structure hydrogel.
2. The redox-degradable hydrogel according to claim 1, characterized in that: The hydrogel monomers include a mixture of one or more of acrylamide monomers, acrylic acid monomers, N-isopropylacrylamide monomers and N,N-dimethylacrylamide monomers.
3. The redox-degradable hydrogel according to claim 1, characterized in that: The initiator includes a thermal initiator and a photoinitiator.
4. The redox-degradable hydrogel according to claim 3, characterized in that: The thermal initiator includes azobisisobutylamidine hydrochloride, azobisisobutylimidazoline hydrochloride, azobiscyanovaleric acid, azobisisopropylimidazoline or azobisisobutyronitrile.
5. The redox-degradable hydrogel according to claim 3, characterized in that: The photoinitiator includes phenyl (2,4,6-trimethylbenzoyl) lithium phosphate, diphenyl-(2,4,6-trimethylbenzoyl) phosphine oxide or dibenzoyl peroxide.
Citation Information
Patent Citations
Dynamic polymer foam composite material[v]
CN111253610A
Energy absorption method and material based on hybrid cross-linked dynamic polymer
CN111378159A
Combined energy absorption method and application thereof
CN111378160A
Combined hybrid cross-linked dynamic polymer and application thereof
CN111378165A
Hydrogel coating with underwater stability and resistance reduction function for implantation / intervention medical apparatus and preparation method and application of hydrogel coating
CN117258044A