A test device and test method for quickly testing the microwave absorption performance of asphalt mortar
By designing a test device containing a trapezoidal sheet and a semicircular sheet, the height change and crack filling rate of the asphalt glue specimen are measured after microwave heating, the existing technology cannot test the asphalt glue absorbs microwave after the asphalt glue absorbs the microwave. The problem of flow characteristics and self-healing characteristics enables fast and accurate testing, simplifying operation and reducing costs.
Patent Information
- Application Number
- CN202410414619.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-04-08
AI Technical Summary
The prior art cannot simultaneously test the flow characteristics and self-healing characteristics of asphalt glue after microwave absorption, and the equipment is expensive, cumbersome and time-consuming.
A test device and method for quickly testing the microwave absorption performance of asphalt glue is designed, including trapezoidal sheet body, semicircular sheet body, round table groove and fixed ply plate. After microwave heating, the height change of the test piece and the preset crack are measured. fill rate to evaluate flow characteristics and self-healing characteristics.
It realizes rapid and accurate evaluation of the microwave absorption performance of asphalt slurry, simplifies operation, reduces equipment costs, can simultaneously determine flow characteristics and self-healing characteristics, and guides large-scale maintenance and maintenance of asphalt pavements.
Smart Images

Figure CN118169373B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a test device and a test method, in particular to a test device and a test method for quickly testing the microwave absorption performance of asphalt mortar, and belongs to the field of road engineering. Background Art
[0002] Asphalt pavement cracking refers to the occurrence of transverse, longitudinal, and reticular cracks on asphalt pavement under the coupling of complex factors such as vehicle load and service environment. Asphalt pavement cracks seriously affect the integrity and continuity of the pavement, while allowing water to penetrate into the lower layer of the pavement structure, affecting the stability of the road structure, seriously deteriorating the pavement performance and shortening its service life.
[0003] Asphalt is a petroleum-based medium-polymer material with good viscosity and fluidity. At the appropriate temperature, asphalt can flow to the damaged interface, fill small cracks and tiny damage, and show a certain degree of self-healing. However, in the actual service environment, due to the influence of complex factors such as vehicle load and environment, the self-healing ability of asphalt is very limited. Therefore, timely heating can be used to repair asphalt pavement defects such as transverse, longitudinal, and reticular cracks caused by the coupling of complex factors such as vehicle load and service environment, thereby ensuring the performance of the pavement and extending its service life.
[0004] Using microwave heating technology to heat asphalt materials and using the flow characteristics and self-healing properties of asphalt materials at higher temperatures to repair asphalt pavement cracks is a new method for preventing and treating asphalt pavement diseases. Microwave heating has the advantages of efficient and uniform heating and high energy efficiency. In practice, it is common practice to mix iron powder, steel slag, carbon materials, silicon carbide and other fillers into asphalt to form asphalt mortar with high microwave absorption capacity, thereby improving the microwave absorption performance of asphalt mixture. It is not difficult to see that the microwave absorption capacity of asphalt mortar directly determines the repair effect of microwave heating on asphalt pavement.
[0005] At present, the experimental methods for studying the wave-absorbing properties of asphalt mortar can be divided into direct and indirect methods: the direct method is to use a vector network analyzer to test the electromagnetic parameters such as the dielectric constant and magnetic permeability of the absorbing filler in the asphalt mortar; the indirect method is to add the absorbing filler to the asphalt to prepare the mortar, and then test the heating effect of the asphalt mortar under microwave radiation and the self-healing performance test based on the dynamic shear rheometer (such as fatigue-healing-fatigue test, fracture-healing-fracture test), etc.
[0006] It is not difficult to find that the above test method for the microwave absorption capacity of asphalt mortar requires specific professional and expensive equipment, and the operation is cumbersome, time-consuming and labor-intensive. In particular, it is impossible to simultaneously test the flow characteristics and self-healing characteristics of the asphalt mortar after absorbing microwaves, which are two properties directly related to the repair of asphalt pavement cracks. Considering the background of the future asphalt pavement from rapid construction to large-scale maintenance, it is very important to study the microwave absorption capacity of asphalt mortar and accurately evaluate its flow characteristics and self-healing characteristics after microwave heating.
[0007] In summary, the current test methods for testing the microwave absorption capacity of asphalt mortar require specific professional and expensive equipment, and the operation is cumbersome, time-consuming and labor-intensive. In particular, it is impossible to simultaneously test the flow characteristics and self-healing characteristics of the asphalt mortar after absorbing microwaves, which are two properties directly related to the repair of asphalt pavement cracks. Summary of the invention
[0008] The purpose of the present invention is to solve the problems of the existing asphalt mortar microwave absorption ability test technology, such as expensive test equipment, cumbersome operation, time-consuming and labor-intensive, and inability to simultaneously test the flow characteristics and self-healing characteristics of the asphalt mortar after absorbing microwaves. Further, a test device and test method for quickly testing the microwave absorption performance of asphalt mortar are provided.
[0009] The technical solution of the present invention is:
[0010] A test device for quickly testing the microwave absorption performance of asphalt mortar includes a trapezoidal sheet, a semicircular sheet, two truncated cone grooves, four fixing clamps and a plurality of butterfly bolts. A fixing clamp is respectively arranged on the left and right sides of the two truncated cone grooves and are made into one piece. After the two truncated cone grooves are buckled, they are connected to the fixing clamps by a plurality of butterfly bolts to form a conical truncated cone mold; the trapezoidal sheet is vertically arranged on the inner side wall of the upper part of a truncated cone groove, and the semicircular sheet is horizontally arranged on the inner side wall of the middle part of a truncated cone groove.
[0011] Furthermore, the semicircular diameter of the semicircular sheet is the diameter of the cross-sectional circle at half the height from the bottom of the conical truncated cone mold; the semicircular sheet is horizontally arranged on the inner side wall at half the height from the bottom of the conical truncated cone mold.
[0012] Furthermore, the thickness of the semicircular sheet is 0.1-5 mm, and is symmetrically distributed with the cross-section circle at half the height of the cone-shaped cone bottom as the center plane.
[0013] Furthermore, the trapezoidal sheet is an isosceles trapezoidal sheet; the lower base of the isosceles trapezoidal sheet is the lower base circle diameter of the conical truncated cone mold, the height is one-third of the height of the truncated cone of the conical truncated cone mold, and the upper base length is equal to the diameter of the cone at one-third of the height of the truncated cone top surface of the conical truncated cone mold.
[0014] Furthermore, the thickness of the trapezoidal sheet is 0.1-5 mm, and the sheet is symmetrically distributed with the plane where a pair of parallel diameters of the upper top surface and the lower bottom surface of the conical truncated cone mold are located as the center plane.
[0015] Furthermore, the thickness of the trapezoidal sheet is 1.5 mm, and the thickness of the semicircular sheet is 1.5 mm.
[0016] The present invention also provides a test method using a test device for quickly testing the microwave absorption performance of asphalt mortar, which comprises the following steps:
[0017] Step 1: First, turn the test device upside down and pour the asphalt mortar heated to a flowing state into the large diameter circle on the bottom surface of the test device;
[0018] Step 2: Scrape the surface of the asphalt mortar sample;
[0019] Step 3: Wait for the asphalt mortar to cool and solidify;
[0020] Step 4: demoulding the asphalt mortar after cooling and solidification. The asphalt mortar specimen after demoulding is in a truncated cone shape as a whole, and has two prefabricated cracks on the asphalt mortar specimen, namely a middle transverse crack and a lower vertical crack;
[0021] Step 5: inserting a transverse crack insert and a vertical crack insert into the middle transverse crack and the lower vertical crack respectively, and the transverse crack insert and the vertical crack insert fill the prefabricated cracks, wherein the transverse crack insert and the vertical crack insert both have a plurality of circular holes;
[0022] Step 6: Place the truncated cone-shaped asphalt mortar specimen with the large diameter circle facing downward into the center of the bottom of a scaled beaker, and record the scale value of the top surface of the truncated cone-shaped asphalt mortar specimen in the vertical height direction of the beaker; place the beaker and the truncated cone-shaped asphalt mortar specimen into a microwave heating device and start heating for 1-10 minutes;
[0023] Step 7: After the truncated cone asphalt mortar specimen is completely cooled, first record the scale value of the top surface of the truncated cone asphalt mortar specimen in the vertical height direction in the beaker, then take out the truncated cone asphalt mortar specimen, and measure the flow characteristics and self-healing characteristics of the test asphalt mortar after absorbing microwaves:
[0024] Flow characteristics: measured and characterized by the height change of the truncated cone asphalt mortar specimen before and after microwave heating;
[0025] Self-healing properties: The transverse crack inserts and vertical crack inserts in the two prefabricated cracks were taken out, and the self-healing characteristics of the asphalt mortar were quantitatively characterized by measuring the filling rate of the asphalt mortar in the circular holes on the transverse crack inserts and the vertical crack inserts. At this point, the flow characteristics and self-healing characteristics of the microwave absorption of the asphalt mortar were simultaneously measured and characterized.
[0026] Furthermore, both the transverse crack insert and the vertical crack insert are provided with a handheld inserting portion.
[0027] Furthermore, the transverse crack inserts and the vertical crack inserts are made of materials that do not absorb microwaves.
[0028] Preferably, the transverse crack inserts and the vertical crack inserts are made of polytetrafluoroethylene, polypropylene or polyethylene.
[0029] Compared with the prior art, the present invention has the following effects:
[0030] 1. The wave absorption flow characteristics of asphalt mortar tested by the present invention are mainly characterized by testing the macroscopic deformation of the asphalt mortar specimen after absorbing microwaves. The specimen is in the shape of a truncated cone as a whole, with a smaller circular radius on the top surface of the truncated cone and a larger circular radius on the bottom surface. This design method enables the mortar specimen with microwave absorption ability to produce flow deformation after microwave heating, thereby reducing the overall height of the specimen. The wave absorption flow characteristics of the asphalt mortar can be evaluated by the height change amplitude. To achieve this purpose, the present invention designs a test device, the internal shape of the mold (referring to the test device) is a truncated cone shape, and for the convenience of demoulding, the mold takes the plane where a pair of parallel diameters on the upper and lower top surfaces of the truncated cone are located as the center plane, and half a groove is formed on each side. When preparing the sample, the molds on both sides are fixed together by bolts, and the lower top surface is not sealed for casting the sample. When demoulding, the bolts are loosened, and the molds on both sides are removed to obtain a truncated cone-shaped specimen.
[0031] 2. The microwave absorption and self-healing properties of asphalt mortar tested in the present invention are mainly characterized by testing the recovery of preset cracks after the asphalt mortar specimen absorbs microwaves. By designing a protruding part on the inner side of the above-mentioned mold (the protruding part mainly refers to the trapezoidal sheet 4 and the semicircular sheet 5), the preset cracks in the asphalt mortar specimen are realized. In order to explore the self-healing properties of asphalt materials in both horizontal and vertical directions, the preset cracks include two parts:
[0032] ① The transverse cracks are formed by adding a semicircular sheet protrusion at a height of half the cone from the bottom of the mold. With this arrangement, after the asphalt mortar is poured into the mold and cooled and demoulded, a transverse preset crack will be formed on the protruding semicircular sheet part of the mold. The size of the semicircular sheet is described as follows: the semicircular diameter is the diameter of the cross-sectional circle at half the height of the bottom of the cone, the arc is a semicircular arc of the cross-sectional circle at half the height of the bottom of the cone, the thickness of the semicircular sheet is 0.1 to 5 mm, and it is symmetrically distributed with the cross-sectional circle at half the height of the cone from the bottom of the mold as the center plane.
[0033] ② The vertical cracks are formed by adding an isosceles trapezoidal sheet protrusion vertically upward at the bottom diameter of the mold. With this arrangement, after the asphalt mortar is poured into the mold and cooled and demolded, a vertical preset crack will be formed on the protruding isosceles trapezoidal sheet part of the mold. The size of the isosceles trapezoidal sheet is described as follows: the lower base of the protruding trapezoidal surface of the isosceles trapezoidal sheet is the circular diameter of the lower base of the truncated cone, the height is one-third of the height of the truncated cone, the length of the upper base is equal to the diameter of the truncated cone at one-third of the height of the truncated cone bottom surface, the thickness of the protruding part of the isosceles trapezoidal sheet is 0.1 to 5 mm, and it is symmetrically distributed with the plane where a pair of parallel diameters of the top surface and the lower base of the truncated cone are located as the center plane.
[0034] 3. The test method of the present invention. The flow characteristics of the asphalt mortar after absorbing microwaves are reflected by the height change of the mortar specimen before and after microwave heating. After the demoulding truncated cone specimen is placed in a microwave heating device for heating, the high-temperature viscosity decreases and the flow deformation occurs, resulting in a change in the specimen height. Therefore, the microwave absorption flow characteristics of the asphalt mortar can be evaluated by the change in the specimen height.
[0035] The self-healing properties of the test mortar are evaluated by the degree of recovery of the preset cracks in the truncated cone mortar specimen before and after heating. Considering that the self-healing degree of the cracks is difficult to test directly or observe with the naked eye, the present invention proposes to use crack inserts with the same size and thickness as the preset cracks to fill the cracks after the mortar specimen is demolded and before heating. In order to quantify the self-healing degree of the asphalt mortar, a plurality of circular holes with a diameter of 0.5mm-3mm are prefabricated on the crack insert. Due to the self-healing properties of the asphalt material, after the asphalt mortar absorbs microwave energy and is heated, the asphalt mortar will automatically fill the circular holes in these crack inserts. The self-healing properties of the asphalt mortar can be further evaluated by the filling rate of the circular holes in the crack inserts with asphalt mortar.
[0036] Place the truncated cone-shaped asphalt mortar specimen with the larger radius facing downward in the center of the bottom of a beaker with a precise scale. The beaker scale is required to measure vertically upward from the bottom of the beaker. The scale range is the height of the truncated cone specimen, and the scale is accurate to 1mm. Then put the beaker and the specimen into the microwave heating device and start heating. The heating time is 1-10 minutes. The asphalt mortar will produce flow deformation due to the increase in temperature. The test operator will keep his sight horizontal and observe the scale changes on the top of the specimen through the beaker scale line to quantify the wave absorption flow characteristics of the asphalt mortar. At the same time, due to the self-healing characteristics of the asphalt material, the asphalt mortar will fill the circular holes in the crack insert after heating. After the specimen is cooled after heating, the crack inserts in the two prefabricated cracks are taken out, and the self-healing characteristics of the asphalt mortar are quantified by measuring the hole filling rate of the asphalt mortar in the crack insert.
[0037] In summary, the present invention can realize rapid testing of the microwave absorption performance of asphalt mortar with the help of simple test operations, accurately evaluate the flow characteristics and self-healing characteristics of asphalt mortar after microwave heating, indirectly predict the repair effect of corresponding asphalt pavement crack diseases, guide and promote the application of microwave thermal induced self-healing technology in large-scale maintenance and repair of asphalt pavements, and solve the problems of the existing asphalt mortar microwave absorption ability test technology that cannot simultaneously measure the flow characteristics and self-healing characteristics, and has the problems of expensive equipment, cumbersome operation, time-consuming and labor-intensive. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 is a front view of the test device of the present invention;
[0039] Figure 2 is a top view of the test device of the present invention;
[0040] Figure 3 It is a left side view of the test device of the present invention;
[0041] Figure 4 is a front view of a transverse crack filling crack insert;
[0042] Figure 5 is a front view of a vertical crack filling crack insert;
[0043] In the figure: 1. truncated cone groove, 2. fixed splint, 3. butterfly bolt, 4. trapezoidal sheet, 5. semicircular sheet, 6. transverse crack insert, 7. vertical crack insert, 8. hand-held insertion part. DETAILED DESCRIPTION
[0044] Specific implementation method 1: Combination Figures 1 to 3 The present embodiment is described. A test device for quickly testing the microwave absorption performance of asphalt mortar in the present embodiment includes a trapezoidal sheet 4, a semicircular sheet 5, two truncated cone-shaped grooves 1, four fixed clamps 2 and a plurality of butterfly bolts 3. A fixed clamp 2 is respectively arranged on the left and right sides of the two truncated cone-shaped grooves 1 and are made into one piece. After the two truncated cone-shaped grooves 1 are buckled, they are connected to the fixed clamps 2 through a plurality of butterfly bolts 3 to form a conical truncated cone mold; the trapezoidal sheet 4 is vertically arranged on the inner side wall of the upper part of a truncated cone-shaped groove 1, and the semicircular sheet 5 is horizontally arranged on the inner side wall of the middle part of a truncated cone-shaped groove 1.
[0045] Specific implementation method 2: Combination Figures 1 to 3To explain this embodiment, the semicircular diameter of the semicircular sheet 5 of this embodiment is the diameter of the cross-sectional circle at a height of one-half of the bottom of the conical truncated cone mold; the semicircular sheet 5 is horizontally arranged on the inner side wall at a height of one-half of the bottom of the conical truncated cone mold. In this way, the size of the transverse preset cracks formed by the semicircular sheet 5 and the vertical preset cracks formed by the trapezoidal sheet 4 can be increased as much as possible, while avoiding the connection and mutual influence between the transverse preset cracks formed by the semicircular sheet 5 and the vertical preset cracks formed by the trapezoidal sheet 4, thereby improving the test effect of the self-healing characteristics of the transverse preset cracks of the asphalt mortar. The other components and connection relationships are the same as those of the first specific embodiment.
[0046] Specific implementation method three: Combination Figures 1 to 3 To explain this embodiment, the semicircular sheet 5 of this embodiment has a thickness of 0.1-5 mm and is symmetrically distributed with the cross-section circle at half the height of the cone-shaped cone bottom as the center plane.
[0047] By setting the thickness range of the semicircular sheet in this way, different cracking grades of asphalt mixture can be effectively simulated, and the mold design is carried out for the self-healing characteristics of asphalt mortar under different cracking grades. The other components and connection relationships are the same as those of the first or second specific implementation mode.
[0048] Specific implementation method four: Combination Figures 1 to 3 To explain this embodiment, the trapezoidal sheet 4 of this embodiment is an isosceles trapezoidal sheet; the lower base of the isosceles trapezoidal sheet is the lower base circle diameter of the conical truncated cone mold, the height is one-third of the height of the truncated cone of the conical truncated cone mold, and the length of the upper base is equal to the diameter of the truncated cone at one-third of the height of the truncated cone of the conical truncated cone mold. In this way, the size of the vertical preset cracks formed by the trapezoidal sheet 4 and the horizontal preset cracks formed by the semicircular sheet 5 can be increased as much as possible, and the test effect of the self-healing characteristics of the vertical preset cracks of the asphalt mortar can be improved. The other components and connection relationships are the same as those of the first, second or third specific embodiments.
[0049] Specific implementation method five: Combination Figures 1 to 3 This embodiment is described. The thickness of the trapezoidal sheet 4 of this embodiment is 0.1-5 mm, and is symmetrically distributed with the plane where a pair of parallel diameters of the upper top surface and the lower bottom surface of the conical truncated cone mold are located as the center plane. In this way, the thickness range of the trapezoidal sheet is set, which can effectively simulate different crack cracking levels of asphalt mixture, and design the mold for the self-healing characteristics of asphalt mortar under different cracking conditions. The other components and connection relationships are the same as any one of the specific embodiments one to four.
[0050] Specific implementation method six: Combination Figures 1 to 3To illustrate this embodiment, the thickness of the trapezoidal sheet 4 is 1.5 mm, and the thickness of the semicircular sheet 5 is 1.5 mm. This arrangement can effectively simulate the self-healing effect of asphalt mortar on a slight 1.5 mm wide crack under microwave heating conditions. The other components and connection relationships are the same as any one of the specific embodiments 1 to 5.
[0051] Specific implementation method seven: Combination Figures 1 to 5 The test method of this embodiment is characterized in that it includes the following steps:
[0052] Step 1: First, turn the test device upside down and pour the asphalt mortar heated to a flowing state into the large diameter circle on the bottom surface of the test device;
[0053] Step 2: Scrape the surface of the asphalt mortar sample;
[0054] Step 3: Wait for the asphalt mortar to cool and solidify;
[0055] Step 4: demoulding the asphalt mortar after cooling and solidification. The asphalt mortar specimen after demoulding is in a truncated cone shape as a whole, and has two prefabricated cracks on the asphalt mortar specimen, namely a middle transverse crack and a lower vertical crack;
[0056] Step 5: inserting the transverse crack insert 6 and the vertical crack insert 7 into the middle transverse crack and the lower vertical crack respectively, and the transverse crack insert 6 and the vertical crack insert 7 fill the prefabricated cracks, wherein the transverse crack insert 6 and the vertical crack insert 7 both have a plurality of circular holes;
[0057] Step 6: Place the truncated cone-shaped asphalt mortar specimen with the large diameter circle facing downward into the center of the bottom of a scaled beaker, and record the scale value of the top surface of the truncated cone-shaped asphalt mortar specimen in the vertical height direction of the beaker; place the beaker and the truncated cone-shaped asphalt mortar specimen into a microwave heating device and start heating for 1-10 minutes;
[0058] Step 7: After the truncated cone asphalt mortar specimen is completely cooled, first record the scale value of the vertical height direction of the truncated cone asphalt mortar specimen in the beaker, then take out the truncated cone asphalt mortar specimen, and measure the flow characteristics and self-healing characteristics of the test asphalt mortar after absorbing microwaves:
[0059] Flow characteristics: measured and characterized by the height change of the truncated cone asphalt mortar specimen before and after microwave heating;
[0060] Self-healing characteristics: Take out the transverse crack insert 6 and the vertical crack insert 7 from the two prefabricated cracks, and quantitatively characterize the self-healing characteristics of the asphalt mortar by measuring the filling rate of the asphalt mortar in the circular holes on the transverse crack insert 6 and the vertical crack insert 7. At this point, the simultaneous determination of the flow characteristics and self-healing characteristics of the asphalt mortar after absorbing microwaves is completed.
[0061] In step seven of this embodiment, in order to avoid the asphalt mortar around the crack plug affecting the number of connected holes when the crack plug is pulled out, the crack plug should be taken out after the asphalt mortar specimen is completely cooled, and then the self-healing properties of the asphalt mortar are evaluated by the filling rate of the asphalt mortar holes on the crack plug.
[0062] In order to more objectively quantify the self-healing effect of asphalt mortar, the more circular holes there are on the transverse crack insert 6 and the vertical crack insert 7, the better. The more circular holes there are, the more accurately the self-healing properties of asphalt mortar can be characterized and quantified, and more accurate test results can be obtained.
[0063] Specific implementation method eight: Combination Figures 4 to 5 To explain this embodiment, both the transverse crack insert 6 and the vertical crack insert 7 of this embodiment are provided with a hand-held insertion and removal portion 8. With this arrangement, under the premise that the internal volume of the crack insert inserted into the specimen is consistent with the preset crack volume of the specimen, a hand-held insertion and removal portion 8 of a certain size should be added to the outside of the crack insert to facilitate the test operator to insert and remove the crack insert. The other components and connection relationships are the same as any one of the specific embodiments 1 to 7.
[0064] Specific implementation method nine: Combination Figures 4 to 5 To explain this embodiment, the transverse crack insert 6 and the vertical crack insert 7 of this embodiment are made of materials that do not absorb microwaves. This arrangement is to prevent the crack inserts from absorbing microwaves and heating the surrounding asphalt to cause asphalt rheology. Other components and connection relationships are the same as any one of the specific embodiments 1 to 8.
[0065] Specific implementation method ten: Combination Figures 4 to 5 This embodiment is described. The material of the transverse crack insert 6 and the vertical crack insert 7 of this embodiment is polytetrafluoroethylene, polypropylene or polyethylene. This arrangement can prevent the crack insert itself from absorbing microwaves to heat the surrounding asphalt and cause asphalt rheology. Other components and connection relationships are the same as any one of the specific embodiments 1 to 8.
[0066] Combination Figures 1 to 5 Describe the embodiments of the present invention:
[0067] Example 1
[0068] 1. Test piece mold design.
[0069] like Figure 1-3 , Figure 1 The front view of the structural schematic diagram of the test device of the present invention is shown, including a truncated cone groove 1, a fixing clamping plate 2, a butterfly bolt 3, a trapezoidal sheet 4, and a semicircular sheet 5. Figure 2 The schematic diagram of the structure of the test device of the present invention is shown in a top view, which includes a truncated cone groove 1, a fixing clamp 2, a butterfly bolt 3, a trapezoidal sheet 4, and a semicircular sheet 5. Figure 3 The left view of the structural schematic diagram of the test device of the present invention is shown, which includes a truncated cone groove 1, a fixed clamping plate 2, a butterfly bolt 3, and a semicircular sheet 5.
[0070] The mold wall thickness is 0.5mm, the diameter of the top circle of the cone formed inside is 20mm, the diameter of the bottom circle is 40mm, and the height of the cone is 600mm. In order to preset a horizontal crack in the middle of the cone, the size of the semicircular sheet part inside the model is: the diameter is the diameter of the cross-section circle at half the distance from the bottom of the cone, the arc is the arc of the cross-section circle at half the distance from the bottom edge of the cone, the thickness is 1.5mm, and it is symmetrically distributed with the cross-section circle at half the height of the cone at the bottom of the mold as the center plane. In order to preset a vertical crack in the lower part of the cone body, the size of the trapezoidal sheet part inside the mold is: the lower bottom edge is the diameter of the circle of the lower top of the cone, 40mm, the height is 20mm, one-third of the height of the cone, the upper bottom edge is the diameter of the circle at one-third of the height of the lower top of the cone, the thickness is 1.5mm, and it is symmetrically distributed with the plane where a pair of parallel diameters of the top and lower bottom of the cone are located as the center plane.
[0071] The butterfly bolts used in this case are M3 bolts, that is, the outer diameter of the bolt thread is 3mm.
[0072] 2. Experimental test methods.
[0073] First, heat the asphalt mortar to 155℃ until it flows, and then pour it into the test mold designed for the test device. Scrape off the excess asphalt at the opening of the mold with a shovel, then cool the specimen at room temperature for 4 hours, unscrew the butterfly bolts and demould the specimen. The overall outline of the specimen is a truncated cone with an upper top surface of a circle with a diameter of 20mm, a lower bottom surface of a circle with a diameter of 40mm, and a height of 600mm. There is a transverse crack at half the height of the lower bottom surface of the truncated cone. The volume of the transverse crack is the volume of the semicircular sheet described in the test device. The truncated cone has a vertical crack vertically upward from the diameter of the lower bottom circle. The volume of the vertical crack is the volume of the trapezoidal sheet described in the test device.
[0074] The filler of the asphalt mortar in this embodiment adopts the mineral powder of 200 mesh of common aggregate, including steel slag, obsidian, limestone, amphibolite, iron tailings, calcium magnesium tourmaline, andesite, rhyolite, basalt, dolomite, diabase, granite, and iron series tourmaline 200 mesh mineral powder. The powder-to-binder mass ratio of the asphalt mortar (i.e. the ratio of filler to asphalt) is 1.1:1. Then, the prefabricated crack inserts are inserted into the preset cracks. The schematic diagrams of the prefabricated crack inserts at the horizontal cracks and vertical cracks are shown as follows: Figure 4 and Figure 5 As shown. The material used to prepare the crack insert in this example is polytetrafluoroethylene. The crack insert is prefabricated at the transverse crack. In order to facilitate the test operator to insert and remove the crack insert, an irregular crack insert with a portion of the upper bottom edge parallel to the diameter of the semicircular sheet body is added to the semicircular sheet body. The length of the upper bottom edge is half the diameter of the circle where the arc is located. The size of the semicircular sheet body is the size of the semicircular sheet body inside the mold in the test device. In order to quantify the self-healing degree of the material, 40 circular holes with a diameter of 1.5 mm are prefabricated on the crack insert. The overall outline of the prefabricated crack insert at the transverse crack is as shown in the figure. Figure 4 As shown, the thickness is 1.5mm. A part of the trapezoidal crack insert is added to the right side of the trapezoidal sheet. The trapezoidal crack insert is added with a hand-held part to form a right-angle trapezoid with the crack insert for inserting the specimen, which is used to facilitate the insertion and removal of the crack insert during the test operation. The size of the trapezoidal sheet is the size of the trapezoidal sheet inside the mold in the test device. In order to quantify the self-healing degree of the material, 77 circular holes with a diameter of 1.5mm are prefabricated on the crack insert. The overall outline of the prefabricated crack insert at the vertical crack is as follows: Figure 5 As shown, the thickness is 1.5 mm.
[0075] Place the truncated cone-shaped asphalt mortar specimen with the larger radius facing downward in the center of the bottom of a beaker with a precise scale. The beaker scale is required to measure vertically upward from the bottom of the beaker. The scale range is 60mm and the scale is accurate to 1mm. Then put the beaker and the specimen into a microwave oven and start heating. Further experiments verify that when the microwave heating power is 700W, the asphalt mortar specimen is heated for 6 minutes. The height changes of the thirteen asphalt mortar specimens and the number of holes filled with asphalt mortar and the filling rate of the crack inserts for filling the horizontal and vertical cracks are shown in Table 1:
[0076] Table 1 Test results of common mineral powder mortar test
[0077]
[0078] In this implementation case, asphalt mortar was prepared using aggregate mineral powder and asphalt. The microwave heating test verified that the microwave absorption efficiency of asphalt mortar prepared from steel slag, basalt, iron series tourmaline and 200 mesh diabase mineral powders after microwave heating was significantly improved compared with the asphalt mortar prepared from the commonly used filler limestone mineral powder. It is believed that the asphalt mortars prepared from these four mineral powders have better flow properties and self-healing properties, and the minimum height change of these four asphalt mortar specimens is 11.3mm. The hole filling rates of the asphalt mortar filled in the horizontal and vertical crack filling crack inserts are 72.50% and 64.94% respectively.
[0079] Therefore, when the method described in this implementation case is used to design the mortar specimens and the test method is used to test the flow characteristics and self-healing characteristics of the asphalt mortar after absorbing microwaves, the asphalt mortar specimens with a height change greater than 10 mm are qualified as mortars that absorb microwave flow deformation, and the hole filling rates of the asphalt mortar filled in the horizontal and vertical crack filling crack inserts are greater than 70% and 60%, respectively, which are qualified as mortars that absorb microwaves and have self-healing characteristics.
[0080] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A test method using a test device for rapidly testing the microwave absorption performance of asphalt mortar, characterized in that: It includes the following steps: Step 1: First, turn the test device upside down and pour the asphalt slurry heated to a flowing state into the large diameter circle on the bottom surface of the test device; The test device comprises a trapezoidal sheet (4), a semicircular sheet (5), two truncated cone-shaped grooves (1), four fixing clamps (2) and a plurality of butterfly bolts (3). A fixing clamping plate (2) is respectively arranged on the left and right sides of the two truncated cone-shaped grooves (1) and is made into an integral body. After the two truncated cone-shaped grooves (1) are buckled together, they are connected to the fixing clamping plate (2) through a plurality of butterfly bolts (3) to form a conical truncated cone mold; the trapezoidal sheet (4) is vertically arranged on the inner side wall of the upper part of a truncated cone-shaped groove (1), and the semicircular sheet (5) is horizontally arranged on the inner side wall of the middle part of a truncated cone-shaped groove (1); Step 2: Scrape the surface of the asphalt mortar sample; Step 3: Wait for the asphalt mortar to cool and solidify; Step 4: demoulding the asphalt mortar after cooling and solidification. The asphalt mortar specimen after demoulding is in a truncated cone shape as a whole, and has two prefabricated cracks on the asphalt mortar specimen, namely a middle transverse crack and a lower vertical crack; Step 5: inserting a transverse crack insert (6) and a vertical crack insert (7) into the middle transverse crack and the lower vertical crack respectively, and the transverse crack insert (6) and the vertical crack insert (7) fill the prefabricated cracks, wherein the transverse crack insert (6) and the vertical crack insert (7) both have a plurality of circular holes; Step 6: Place the truncated cone asphalt mortar specimen with the large diameter circle facing downward in the center of the bottom of a scaled beaker, and record the scale value of the vertical height direction of the truncated cone asphalt mortar specimen in the beaker; place the beaker and the truncated cone asphalt mortar specimen together in a microwave heating device and start heating for 1-10 minutes; Step 7: After the truncated cone asphalt mortar specimen is completely cooled, first record the scale value of the vertical height direction of the truncated cone asphalt mortar specimen in the beaker, then take out the truncated cone asphalt mortar specimen, and measure the flow characteristics and self-healing characteristics of the test asphalt mortar after absorbing microwaves: Flow characteristics: measured and characterized by the height change of the truncated cone asphalt mortar specimen before and after microwave heating; Self-healing properties: The transverse crack inserts (6) and the vertical crack inserts (7) in the two prefabricated cracks are taken out, and the self-healing characteristics of the asphalt mortar are quantitatively characterized by measuring the filling rate of the asphalt mortar in the circular holes on the transverse crack inserts (6) and the vertical crack inserts (7). At this point, the flow characteristics and self-healing characteristics of the microwave absorption of the asphalt mortar are simultaneously measured and characterized.
2. The test method according to claim 1, characterized in that: Both the transverse crack insert (6) and the vertical crack insert (7) are provided with a handheld inserting portion (8).
3. The test method according to claim 2, characterized in that: The transverse crack inserts (6) and the vertical crack inserts (7) are made of materials that do not absorb microwaves.
4. The test method according to claim 3, characterized in that: The material of the transverse crack insert (6) and the vertical crack insert (7) is polytetrafluoroethylene, polypropylene or polyethylene.
5. The test method according to claim 4, characterized in that: The semicircular diameter of the semicircular sheet (5) is the diameter of the cross-section circle at a height halfway from the bottom of the conical truncated cone mold; the semicircular sheet (5) is horizontally arranged on the inner side wall at a height halfway from the bottom of the conical truncated cone mold.
6. The test method according to claim 5, characterized in that: The thickness of the semicircular sheet (5) is 0.1-5 mm, and the semicircular sheet (5) is symmetrically distributed with the cross-section circle at half the height of the cone-shaped cone bottom as the center plane.
7. The test method according to claim 6, characterized in that: The trapezoidal sheet (4) is an isosceles trapezoidal sheet; the lower base of the isosceles trapezoidal sheet is the lower bottom surface circle diameter of the conical truncated cone mold, the height is one third of the height of the truncated cone of the conical truncated cone mold, and the upper base length is equal to the diameter of the truncated cone at one third of the height of the lower bottom surface of the truncated cone of the conical truncated cone mold.
8. The test method according to claim 7, characterized in that: The thickness of the trapezoidal sheet (4) is 0.1-5 mm, and the sheet is symmetrically distributed with the plane where a pair of parallel diameters of the upper top surface and the lower bottom surface of the conical truncated cone mold are located as the center plane.
9. The test method according to claim 8, characterized in that: The thickness of the trapezoidal sheet (4) is 1.5 mm, and the thickness of the semicircular sheet (5) is 1.5 mm.