A non-deformable heat-resistant HIPS hot air blower shell material and preparation method thereof
Through the combination and optimization treatment of high-impact polystyrene, polyphenylene sulfide, glass fiber and other materials, the problem of insufficient deformation and heat resistance of the hot air fan shell under high heat state is solved, and the heat resistance and machinery of the material are realized Improved performance and extended service life.
Patent Information
- Application Number
- CN202410366984.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-28
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-03-28
AI Technical Summary
The heater shell is prone to deformity, hardness, discoloration and bulging in a long-term high-heat state, resulting in a shortening of service life. The existing high-impact polystyrene materials lack heat resistance, bending strength and tensile strength.
Using a combination of high-impact polystyrene, polyphenylene sulfide, glass fiber, polyurethane resin, compatibility agent and stabilizer, the heat resistance and flexibility of the material are improved by adding polyphenylene sulfide and polyurethane resin, and through Glass fiber reinforces mechanical and mechanical properties, optimizes the dosage and treatment methods of nucleating agents and rubber ultrafine powder, and improves the compatibility and crystallization structure of materials.
It significantly improves the heat resistance, tensile strength and impact resistance of the hot air fan shell material, extends the service life, avoids deformation, discoloration and bulging, and enhances the mechanical and mechanical properties of the material.
Smart Images

Figure GDA0005083623550000051 
Figure GDA0005083623550000061 
Figure GDA0005083623550000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of high-impact polystyrene material processing, and in particular to a non-deformable and heat-resistant HIPS hot air blower housing material and a preparation method thereof. Background Art
[0002] The hot air blower can quickly heat up the cold air, causing the indoor temperature to rise rapidly, thus playing a role in heating. In order to increase the service life of the hot air blower and protect the internal structure of the hot air blower, a hot air blower shell with good impact resistance is required. HIPS is a two-phase system consisting of a rubber phase and a continuous polystyrene phase. It has the characteristics of easy processing, excellent dimensional stability, high impact strength and good rigidity. It is one of the good materials for preparing the shell. High-impact polystyrene formed by rubber-modified polystyrene has greatly improved impact resistance and toughness, but its heat resistance, bending strength and tensile strength are lower than those of polystyrene. The hot air blower needs to work under high heat conditions for a long time. If it returns to high heat for a long time, the shell of the hot air blower will deform, harden, discolor and bulge. Summary of the invention
[0003] In order to improve the heat resistance, bending strength and tensile strength of high impact polystyrene, the present application provides a non-deformable heat-resistant HIPS hot air blower housing material and a preparation method thereof.
[0004] In the first aspect, the present application provides a non-deformable heat-resistant HIPS hot air blower housing material, which adopts the following technical scheme: a non-deformable heat-resistant HIPS hot air blower housing material is prepared from raw materials including the following parts by weight:
[0005] High impact polystyrene 40-50 parts
[0006] Polyphenylene sulfide 5-9 parts
[0007] 4-5 parts white oil
[0008] Glass fiber 5-10 parts
[0009] 4-8 parts polyurethane resin
[0010] 1-2 parts of compatibilizer
[0011] 1-3 parts of stabilizer.
[0012] By adopting the above technical scheme, the heat resistance, tensile strength and flexibility of the HIPS hot air blower shell material are improved, and the original state can be maintained after long-term use, without deformation, discoloration and bulging, thereby extending the service life of the hot air blower shell. In this application, polyphenylene sulfide is added and used in conjunction with high-impact polystyrene to improve the heat resistance of the hot air blower shell material. Polyphenylene sulfide has good heat resistance and is fully mixed with high-impact polystyrene to further improve the heat resistance of the hot air blower shell material, while not affecting the high impact strength, easy processing and rigidity of high-impact polystyrene. Polyphenylene sulfide has poor lubricity and high brittleness, and is difficult to fully mix with high-impact polystyrene. The mixing degree of polyphenylene sulfide with high-impact polystyrene and polyurethane resin is improved by the action of white oil, and then the compatibility of polyphenylene sulfide with high-impact polystyrene and polyurethane resin is increased in combination with the action of compatibilizer, thereby improving the structural uniformity of the hot air blower shell material, so that the hot air blower shell has good heat resistance and mechanical strength. Polyurethane resin has good flexibility and is used to prepare the shell material of the hot air blower. It can reduce the brittleness of polyphenylene sulfide, improve the flexibility of the hot air blower shell material, and effectively avoid the breakage or cracking of the hot air blower shell.
[0013] On the one hand, the glass fiber improves the mechanical strength of the hot air blower housing; on the other hand, it promotes the crystallization of polyphenylene sulfide, refines the grains of polyphenylene sulfide, makes the spherulites of polyphenylene sulfide more compact, and thus improves the heat resistance of the hot air blower housing.
[0014] Through the effect of stability, the durability of the hot air blower shell material is improved, the aging and oxidation of high-impact polystyrene and polyphenylene sulfide are effectively delayed, and the service life of the hot air blower shell is increased.
[0015] Preferably, the polyphenylene sulfide is modified polyphenylene sulfide, which is prepared by the following preparation method:
[0016] A: mixing a nucleating agent and polyphenylene sulfide to obtain a mixture A;
[0017] B: The mixture, glycidyl methacrylate, superfine rubber powder and antioxidant are then mixed, melt-extruded and granulated in a screw extruder to obtain modified polyphenylene sulfide.
[0018] Polyphenylene sulfide can greatly improve the heat resistance and tensile strength of high-impact polystyrene, but polyphenylene sulfide is very brittle. By adding polyurethane resin in combination with polyphenylene sulfide, the brittleness of polyphenylene sulfide can be reduced, but the degree of reduction is limited. The technical solution in this application can greatly reduce the brittleness of polyphenylene sulfide without affecting the heat resistance, tensile strength, and bending strength of polyphenylene sulfide. The addition of a nucleating agent in this application increases the crystallization density of polyphenylene sulfide during the melting process, thereby improving the heat resistance of high-impact polystyrene.
[0019] Glycidyl methacrylate can reduce the internal stress of polyphenylene sulfide. Glycidyl methacrylate has acrylate double bonds and epoxy groups, and can be grafted to polyphenylene sulfide, so that the internal stress of polyphenylene sulfide is reduced, and the brittleness of polyphenylene sulfide is greatly reduced. At the same time, under the action of glycidyl methacrylate and toughening agent, polyphenylene sulfide and rubber ultrafine powder are fully mixed, and the compatibility of the obtained product with high-impact polystyrene is greatly improved. After adding rubber ultrafine powder, rubber has certain elasticity and softness, which further improves the flexibility of polyphenylene sulfide, making the hot air blower shell not easy to break or crack. At the same time, due to the addition of rubber ultrafine powder, the compatibility of modified polyphenylene sulfide with high-impact polystyrene is further improved, thereby improving the mechanical properties of the hot air blower shell material.
[0020] Preferably, the nucleating agent is at least one of diformyl zinc oxide, sodium p-phenolsulfonate, sodium stearate and calcium p-phenolsulfonate.
[0021] Preferably, the weight parts of the raw materials used to prepare the modified polyphenylene sulfide are as follows:
[0022] Nucleating agent 0.1-0.2 parts
[0023] Polyphenylene sulfide 20-30 parts
[0024] Glycidyl methacrylate 5-10 parts
[0025] 5-9 parts of superfine rubber powder
[0026] 1-2 servings of antioxidants.
[0027] By adopting the above technical scheme, the amount of raw materials used in the preparation of modified polyphenylene sulfide is optimized, the brittleness of polyphenylene sulfide is greatly reduced, and the toughness of polyphenylene sulfide is greatly improved, which effectively prevents the hot air blower casing from cracking or breaking, and also improves the mechanical properties of the hot air blower casing material.
[0028] Preferably, the average particle size of the ultrafine rubber powder is 100-500 microns.
[0029] By adopting the above technical solution, the average particle size of the rubber superfine powder is optimized, so that the rubber superfine powder and polyphenylene sulfide are fully mixed, the brittleness of polyphenylene sulfide is effectively improved, and the flexibility of the modified polyphenylene sulfide is increased.
[0030] Preferably, the rubber ultrafine powder includes at least one of polybutadiene rubber, nitrile rubber, EPDM rubber, butyl rubber, styrene-butadiene rubber and toluene rubber.
[0031] By adopting the above-mentioned rubber ultrafine powder, the toughness of the modified polyphenylene sulfide is further improved, and the compatibility of polyphenylene sulfide and high-impact polystyrene is improved. The above-mentioned rubber ultrafine powder has good toughness and elasticity and can effectively improve the flexibility of the modified polyphenylene sulfide.
[0032] Preferably, the high impact polystyrene is a copolymer of styrene and polybutadiene rubber, and the number average molecular weight of the high impact polystyrene is 15000-40000.
[0033] By adopting the above technical solution, the parameters of high-impact polystyrene are optimized, which is beneficial to improving the mechanical strength of the hot air blower shell material.
[0034] Preferably, the glass fiber is pretreated, and the pretreatment steps are as follows:
[0035] The glass fiber is heated to 200-250°C, then added to a sodium hydroxide solution, soaked for 20-30 minutes, filtered, rinsed with water, and then ground with a mercaptosilane coupling agent to obtain a pretreated glass fiber.
[0036] The compatibility and bonding strength of glass fiber with high-impact polystyrene and polyphenylene sulfide are poor. By pretreating the glass fiber, the surface properties of the glass fiber are changed, the compatibility and bonding strength of the glass fiber with high-impact polystyrene and polyphenylene sulfide are improved, thereby further improving the heat resistance and mechanical properties of the hot air blower shell material.
[0037] By first heating and then placing it in a sodium hydroxide solution, the surface of the glass fiber becomes rough and the surface area is increased, and then it is ground with a mercaptosilane coupling agent to change the surface properties of the glass fiber. The mercaptosilane coupling agent contains a thiol group, which can improve the compatibility and bonding between the glass fiber and high-impact polystyrene and polyphenylene sulfide, thereby improving the heat resistance, tensile strength and strength of HIPS.
[0038] Preferably, the compatibilizer is composed of ethylene-octene copolymer grafted maleic anhydride, polyethylene grafted maleic anhydride and styrene-isoprene copolymer grafted maleic anhydride in a weight ratio of (1-3): (2-5): 6.
[0039] By adopting the above technical solution, the compatibility of high-impact polystyrene and polyphenylene sulfide is greatly improved, thereby improving the heat resistance, impact resistance, hardness, tensile strength and other mechanical properties of the hot air blower casing.
[0040] Preferably, the stabilizer is obtained by mixing an ultraviolet absorber and an organic antimony in a weight ratio of (0.1-0.5):1.
[0041] By adopting the above technical solution, the light aging resistance of the shell material of the hot air blower is improved, and the degradation of high-impact polystyrene caused during the processing is prevented.
[0042] In the second aspect, the present application provides a method for preparing a non-deformable heat-resistant HIPS hot air blower housing material, using the following technical solution:
[0043] A method for preparing a heat-resistant HIPS hot air blower housing material that is not easily deformed comprises the following steps:
[0044] S1. According to parts by weight, polyphenylene sulfide, white oil and glass fiber are dispersed by high-speed stirring to obtain a mixture;
[0045] S2. High-impact polystyrene, the mixture, the compatibilizer, the polyurethane resin and the stabilizer are mixed, and the mixture is extruded and granulated by an extruder to obtain a heat-resistant HIPS hot air blower housing material that is not easily deformed.
[0046] By adopting the above technical solution, the prepared non-deformable heat-resistant HIPS hot air blower shell material has good heat resistance and mechanical properties, can be used for a long time under high temperature conditions without deformation, discoloration or bulging.
[0047] In summary, this application has the following beneficial effects:
[0048] 1. The present application prepares a non-deformable heat-resistant HIPS hot air blower shell material by mixing high-impact polystyrene, polyphenylene sulfide, white oil, glass fiber, polyurethane resin, compatibilizer and stabilizer, thereby improving the heat resistance, tensile strength, flexibility and impact resistance of the hot air blower shell material. After being used in a heated state for a long time, it can still maintain its original state without deformation, discoloration or bulging, thereby reducing the possibility of breakage or cracking of the hot air blower shell material and extending its service life.
[0049] 2. In the present application, modified polyphenylene sulfide is prepared by using a nucleating agent, polyphenylene sulfide, glycidyl acrylate, rubber ultrafine powder and an antioxidant, so that the brittleness of polyphenylene sulfide is greatly reduced and the flexibility is improved, thereby effectively improving the heat resistance of the hot air blower housing material and preventing the hot air blower housing material from breaking or cracking. DETAILED DESCRIPTION
[0050] Example
[0051] Example 1
[0052] A non-deformable heat-resistant HIPS hot air blower housing material is prepared by the following method:
[0053] S1, 50 g of polyphenylene sulfide, 40 g of white oil and 50 g of glass fiber are dispersed by high-speed stirring to obtain a mixture;
[0054] S2. Mix 400 g of high-impact polystyrene, the mixture, 10 g of a compatibilizer (polyethylene grafted maleic anhydride), 40 g of a polyurethane resin and 10 g of a stabilizer (anti-ultraviolet absorber), and extrude and granulate them through an extruder to obtain a non-deformable and heat-resistant HIPS hot air blower housing material.
[0055] The molecular weight of polyphenylene sulfide is 10,000.
[0056] The average diameter of the glass fibers is 25 microns.
[0057] High impact polystyrene is a copolymer of styrene and polybutadiene rubber, and the number average molecular weight of high impact polystyrene is 15,000.
[0058] The molecular weight of the polyurethane resin is 20,000.
[0059] The grafting rate of polyethylene grafted with maleic anhydride is 1.5%.
[0060] The difference between Example 2-3 and Example 1 is that the raw material types, amounts and experimental parameters for preparing the non-deformable heat-resistant HIPS hot air blower housing material are partially different. The specific differences are shown in Table 1:
[0061] Table 1: Types of raw materials, amounts and experimental parameters for preparing heat-resistant HIPS hot air blower housing materials that are not easily deformed in Examples 1-3
[0062]
[0063] The grafting rate of the styrene-isoprene copolymer grafted with maleic anhydride was 1.5%.
[0064] Example 4
[0065] A heat-resistant HIPS hot air blower housing material that is not easily deformed. The difference between this embodiment and embodiment 1 is that the polyphenylene sulfide is modified polyphenylene sulfide, which is prepared by the following method:
[0066] A: 2 g of a nucleating agent (zinc diformyl oxide) and 400 g of polyphenylene sulfide were mixed to obtain a mixture A;
[0067] B: The mixture, 100 g of glycidyl methacrylate, 100 g of superfine rubber powder and 20 g of antioxidant (antioxidant 1024) were mixed, melt-extruded and granulated in a screw extruder to obtain modified polyphenylene sulfide.
[0068] The molecular weight of polyphenylene sulfide is 10,000.
[0069] The rubber ultrafine powder is polybutadiene rubber with an average particle size of 100 microns and a number average molecular weight of 124,000.
[0070] The difference between Example 5-6 and Example 4 is that the types of raw materials, amounts and experimental parameters for preparing modified polyphenylene sulfide are partially different. The specific differences are shown in Table 2:
[0071] Table 2 Raw material types, amounts and experimental parameters for preparing modified polyphenylene sulfide in Examples 4-6
[0072]
[0073] The average particle size of nitrile rubber is 300 microns and the number average molecular weight is 100,000.
[0074] The average particle size of EPDM rubber is 500 microns and the number average molecular weight is 90,000.
[0075] Example 7
[0076] A heat-resistant HIPS hot air blower shell material that is not easily deformed. The difference between this embodiment and embodiment 4 is that diformyl zinc oxide is not used, and the other experimental raw material types, amounts and experimental parameters are consistent with those of embodiment 4.
[0077] Example 8
[0078] A heat-resistant HIPS hot air blower shell material that is not easy to deform. The difference between this embodiment and embodiment 4 is that stearic acid is used instead of glycidyl methacrylate, and the other experimental raw material types, amounts and experimental parameters are consistent with those of embodiment 4.
[0079] Example 9
[0080] A non-deformable and heat-resistant HIPS hot air blower shell material. The difference between this embodiment and embodiment 4 is that polyurethane resin is used instead of rubber ultrafine powder, and the other experimental raw material types, amounts and experimental parameters are consistent with those of embodiment 4.
[0081] The molecular weight of the polyurethane resin is 20,000.
[0082] Example 10
[0083] A heat-resistant HIPS hot air blower housing material that is not easily deformed. The difference between this embodiment and embodiment 1 is that the glass fiber is pretreated, and the pretreatment steps are as follows:
[0084] The glass fiber was heated to 200° C., added into a sodium hydroxide solution (mass fraction of 10%), soaked for 20 minutes, filtered, rinsed with water, and then ground with a mercaptosilane coupling agent (3-mercaptopropyltrimethoxysilane) to obtain a pretreated glass fiber.
[0085] Embodiment 11
[0086] A heat-resistant HIPS hot air blower housing material that is not easily deformed. The difference between this embodiment and embodiment 4 is that the glass fiber is pretreated, and the pretreatment steps are as follows:
[0087] The glass fiber was heated to 250° C., added into a sodium hydroxide solution (mass fraction of 10%), soaked for 30 minutes, filtered, rinsed with water, and then ground with a mercaptosilane coupling agent (3-mercaptopropyltriethoxysilane) to obtain a pretreated glass fiber.
[0088] Example 12
[0089] A heat-resistant HIPS hot air blower shell material that is not easy to deform. The difference between this embodiment and Example 10 is that 3-mercaptopropyltrimethoxysilane is replaced with an equal amount of 3-aminopropyltriethoxysilane, and the remaining experimental raw material types, amounts and experimental parameters are consistent with Example 10.
[0090] Example 13
[0091] A heat-resistant HIPS hot air blower shell material that is not easy to deform. The difference between this embodiment and Example 1 is that the compatibilizer is composed of 1.1g of ethylene-octene copolymer grafted maleic anhydride, 2.2g of polyethylene grafted maleic anhydride and 6.7g of styrene-isoprene copolymer grafted maleic anhydride in a weight ratio of 1:2:6, and the remaining experimental raw material types, amounts and experimental parameters are consistent with Example 1.
[0092] The grafting rate of polyethylene grafted with maleic anhydride is 1.5%.
[0093] The grafting rate of maleic anhydride grafted onto the ethylene-octene copolymer was 1%.
[0094] The grafting rate of the styrene-isoprene copolymer grafted with maleic anhydride was 1.5%.
[0095] Embodiment 14
[0096] A heat-resistant HIPS hot air blower shell material that is not easy to deform. The difference between this embodiment and Example 4 is that the compatibilizer is composed of 2.1g of ethylene-octene copolymer grafted maleic anhydride, 3.6g of polyethylene grafted maleic anhydride and 4.3g of styrene-isoprene copolymer grafted maleic anhydride in a weight ratio of 3:5:6, and the remaining experimental raw material types, amounts and experimental parameters are consistent with Example 4.
[0097] The grafting rate of polyethylene grafted with maleic anhydride is 1.5%.
[0098] The grafting rate of maleic anhydride grafted onto the ethylene-octene copolymer was 1%.
[0099] The grafting rate of the styrene-isoprene copolymer grafted with maleic anhydride was 1.5%.
[0100] Comparative Example
[0101] Comparative Example 1
[0102] A HIPS hot air blower shell material. The difference between this comparative example and Example 1 is that polyamide is used instead of an equal amount of polyphenylene sulfide, and the other experimental raw material types, amounts and experimental parameters are consistent with Example 1.
[0103] The molecular weight of the polyamide is 10,000.
[0104] Comparative Example 2
[0105] A HIPS hot air blower shell material. The difference between this comparative example and Example 1 is that melamine polyphosphate is used instead of an equal amount of polyphenylene sulfide, and the other experimental raw material types, amounts and experimental parameters are consistent with Example 1.
[0106] Comparative Example 3
[0107] A HIPS hot air blower shell material. The difference between this comparative example and Example 1 is that ABS resin is used instead of polyurethane resin, and the other experimental raw material types, amounts and experimental parameters are consistent with those in Example 1.
[0108] The molecular weight of ABS resin is 20,000, the content of acrylonitrile is 30%, the content of butadiene is 30%, and the content of styrene is 40%.
[0109] Comparative Example 4
[0110] A HIPS hot air blower shell material. The difference between this comparative example and Example 1 is that silicon dioxide is used instead of an equal amount of glass fiber, and the other experimental raw material types, amounts and experimental parameters are consistent with those in Example 1.
[0111] Comparative Example 5
[0112] A HIPS hot air blower shell material. The difference between this comparative example and Example 1 is that paraffin is used instead of white oil, and the other experimental raw material types, amounts and experimental parameters are consistent with those in Example 1.
[0113] Performance testing
[0114] The shell materials of the hot air blower prepared in Examples 1-14 and Comparative Examples 1-5 were prepared into sheet samples, and then the sheet samples were tested for tensile properties, Izod impact strength, and cracking and fracture properties.
[0115] Detection method / test method
[0116] Heat resistance test: first test the tensile properties and cantilever beam impact strength, then fold it in half to observe whether the hot air blower shell material is broken, cracked or cracked. Place the sheet sample in an environment with a temperature of 205℃, let it stand for 72 hours, take it out, test the tensile properties and cantilever beam impact strength, and then fold it in half to observe the heat.
[0117] Tensile properties: tested according to GB / T 1040-2006 standard.
[0118] Izod beam impact strength: tested according to GB / T 1843-2008 standard.
[0119] The experimental data are shown in Table 3:
[0120] Table 3 Experimental data of Examples 1-14 and Comparative Examples 1-5
[0121]
[0122] From Examples 1-14 and Comparative Examples 1-5 in combination with Table 3, it can be seen that the present application prepares a non-deformable heat-resistant HIPS hot air blower shell material by combining high-impact polystyrene, polyphenylene sulfide, white oil, glass fiber, polyurethane resin, compatibilizer and stabilizer, which can significantly improve the heat resistance, tensile strength, impact resistance and flexibility of the hot air blower shell material.
[0123] Compared with Example 1, the tensile strength and cantilever beam impact strength data of Example 1 before heating are not as good as those of Example 1, and the change in tensile strength and cantilever beam impact strength is much greater than that of Example 1, indicating that by adding polyphenylene sulfide in the present application, the heat resistance, tensile strength and impact resistance of the hot air blower housing material can be further improved.
[0124] Compared with Example 1 and Comparative Example 2, the changes in tensile strength and cantilever beam impact strength in Comparative Example 2 are basically the same as those in Example 1; however, the tensile strength and cantilever beam impact strength data before heating in Comparative Example 2 are not as good as those in Example 1, and cracking occurs in Comparative Example 2 after folding before heating, indicating that the heat resistance of the hot air blower shell material can be improved by adding melamine polyphosphate, but the tensile strength and impact resistance of the hot air blower shell material will be reduced, and the hot air blower shell will be easily broken.
[0125] Compared with Example 1 and Comparative Example 3, the tensile strength and cantilever beam impact strength of Comparative Example 3 before heating are basically the same. However, after heating, cracks are found in Comparative Example 3 when it is folded in half, indicating that the use of polyurethane resin in this application can significantly improve the flexibility of the hot air blower housing and reduce the possibility of cracking of the hot air blower housing.
[0126] Compared with Example 1 and Comparative Example 4, the tensile strength and cantilever beam impact strength data of Comparative Example 4 before heating are not as good as those of Example 1, and there are cracks in Comparative Example 4 when it is folded after heating, indicating that the use of glass fiber in the present application can significantly improve the flexibility, tensile strength and impact resistance of the hot air blower casing, and reduce the possibility of cracking of the hot air blower casing.
[0127] Compared with Example 1 and Comparative Example 5, the tensile strength and cantilever beam impact strength data of Comparative Example 5 before heating are slightly smaller than those of Example 1, and there are cracks in Comparative Example 5 when it is folded after heating, indicating that the use of glass fiber in the present application can significantly improve the flexibility of the hot air blower casing and reduce the possibility of cracking of the hot air blower casing.
[0128] Compared with Example 4, the tensile strength and cantilever beam impact strength data of Example 4 before heating are significantly higher than those of Example 1, and the changes in tensile strength and cantilever beam impact strength are much smaller than those of Example 1, and Example 1 has cracks after heating, indicating that by adding modified polyphenylene sulfide in the present application, the heat resistance, tensile strength and impact resistance of the hot air blower housing material can be further improved.
[0129] Compared with Examples 7-9, the tensile strength and cantilever beam impact strength data of Example 4 before heating are significantly higher than those of Examples 7-9, and the changes in tensile strength and cantilever beam impact strength are much greater than those of Examples 7-9. There are cracks in Examples 8-9, indicating that the modified polyphenylene sulfide prepared by the method of the present application can further improve the heat resistance, tensile strength and impact resistance of the hot air blower housing material.
[0130] Compared with Example 1 and Example 10, and Example 1 and Example 12, the heat resistance, tensile strength and impact resistance of the high-temperature blower housing material can be further improved by treating the glass fiber with a mercaptosilane coupling agent according to the method of the present application.
[0131] Compared with Example 13, by using ethylene-octene copolymer grafted with maleic anhydride, polyethylene grafted with maleic anhydride and styrene-isoprene copolymer grafted with maleic anhydride as compatibilizers in a specific proportion, the compatibility of polyphenylene sulfide and high-impact polystyrene can be further improved, thereby improving the heat resistance, tensile strength and impact resistance of the hot air blower housing material.
[0132] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A non-deformable heat-resistant HIPS hot air blower housing material, characterized in that: Prepared from the following raw materials in parts by weight: High impact polystyrene 40-50 parts Polyphenylene sulfide 5-9 parts 4-5 parts white oil Glass fiber 5-10 parts Polyurethane resin 4-8 parts 1-2 parts of compatibilizer 1-3 parts of stabilizer; The polyphenylene sulfide is a modified polyphenylene sulfide, which is prepared by the following preparation method: A: mixing a nucleating agent and polyphenylene sulfide to obtain a mixture A; B: Mixing the mixture A, glycidyl methacrylate, rubber ultrafine powder and antioxidant, melt-extruding and granulating in a screw extruder to obtain modified polyphenylene sulfide; The weight parts of the raw materials used to prepare the modified polyphenylene sulfide are as follows: Nucleating agent 0.1-0.2 parts Polyphenylene sulfide 20-30 parts Glycidyl methacrylate 5-10 parts 5-9 parts of superfine rubber powder 1-2 parts of antioxidants; The average particle size of the rubber superfine powder is 100-500 microns; The rubber ultrafine powder includes at least one of polybutadiene rubber, nitrile rubber, EPDM rubber, butyl rubber, styrene butadiene rubber and toluene rubber.
2. The non-deformable heat-resistant HIPS hot air blower housing material according to claim 1, characterized in that: The high impact polystyrene is a copolymer of styrene and polybutadiene rubber, and the number average molecular weight of the high impact polystyrene is 15000-40000.
3. The non-deformable heat-resistant HIPS hot air blower housing material according to claim 1, characterized in that: The glass fiber is pretreated, and the pretreatment steps are as follows: The glass fiber is heated to 200-250° C., added into a sodium hydroxide solution, soaked for 20-30 minutes, filtered, rinsed with water, and then ground with a mercaptosilane coupling agent to obtain a pretreated glass fiber.
4. The non-deformable heat-resistant HIPS hot air blower housing material according to claim 1, characterized in that: The compatibilizer is composed of ethylene-octene copolymer grafted maleic anhydride, polyethylene grafted maleic anhydride and styrene-isoprene copolymer grafted maleic anhydride in a weight ratio of (1-3): (2-5):
6.
5. A method for preparing the non-deformable heat-resistant HIPS hot air blower housing material as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: S1. According to parts by weight, polyphenylene sulfide, white oil and glass fiber are dispersed by high-speed stirring to obtain a mixture; S2. High-impact polystyrene, the mixture, the compatibilizer, the polyurethane resin and the stabilizer are mixed, and the mixture is extruded and granulated by an extruder to obtain a heat-resistant HIPS hot air blower housing material that is not easily deformed.
Citation Information
Patent Citations
Polyphenylene sulfide / styrene alloy material and preparation method thereof
CN103173013A
PPS engineering plastic for NMT technology, and preparation method thereof
CN104910623A