A composite water treatment agent based on urban sewage and preparation method thereof
By preparing hyperbranched modified nano-ferric oxide and quaternary phosphonium salt modified chitosan, a composite water treatment agent with demulsification and flocculation properties was prepared, which solved the problem of low efficiency of traditional sewage treatment methods and achieved efficient flocculation sedimentation and COD removal.
Patent Information
- Application Number
- CN202410568744.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-05-09
AI Technical Summary
Traditional wastewater treatment methods have limitations in terms of treatment efficiency, energy consumption, and cost, and composite water treatment agents are not effective in demulsification and flocculation processes.
Hyperbranched modified nano-ferric oxide and quaternary phosphonium salt modified chitosan were prepared by Michael addition reaction. Through esterification and maleyl chitosan modification, a composite water treatment agent with demulsification and flocculation properties was prepared, which enhanced the floc removal ability under the action of magnetic field and gravity field.
It improves the efficiency of wastewater treatment and water purification, enhances flocculation and sedimentation, reduces suspension stability and hydration double layer stability, and achieves efficient COD removal.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite water treatment agents, in particular to a composite water treatment agent based on urban sewage and a preparation method thereof. Background Art
[0002] Urban sewage treatment has always been an important challenge for environmental protection and public health. Traditional sewage treatment methods have certain limitations in terms of treatment efficiency, energy consumption and cost. In order to solve these problems, in recent years, researchers have continuously tried to develop new water treatment agents and methods to improve sewage treatment efficiency, reduce treatment costs, and reduce environmental impact.
[0003] Composite water treatment agents have attracted much attention due to their versatility and synergistic effects. They are usually composed of multiple functional components such as adsorbents, demulsifiers, flocculants and precipitants, and can effectively remove multiple pollutants in sewage at the same time. In particular, composite water treatment agents play an important role in demulsification and flocculation processes, helping to aggregate tiny suspended matter and colloidal particles into large flocs, thereby facilitating subsequent sedimentation and separation.
[0004] The use of a suitable preparation method can make the composite water treatment agent have higher activity and stability, thereby improving its effect and durability in practical applications. Therefore, the invention of a composite water treatment agent based on urban sewage and its preparation method is of great significance for improving the efficiency of urban sewage treatment and the effect of water purification. Summary of the invention
[0005] The object of the present invention is to provide a composite water treatment agent based on urban sewage and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing a composite water treatment agent based on urban sewage, comprising the following steps:
[0007] S1: Add ethylenediamine to methanol, add methyl acrylate, react at room temperature for 24 hours, and distill under reduced pressure to obtain macromolecular polyamide-amine; add macromolecular polyamide-amine to methanol, add ethylenediamine, react at room temperature for 24 hours, and distill under reduced pressure to obtain polyamide-amine; add branched modified nano-ferroferric oxide to ethanol, add polyamide-amine, heat to 50-55°C and react for 12-14 hours to obtain hyperbranched modified nano-ferroferric oxide;
[0008] S2: adding quaternary phosphonium salt modified chitosan to acetic acid solution, adding biochar, heating to 40-45°C and stirring evenly, adding glutaraldehyde, continuing stirring, adjusting the pH of the reaction system to 9-10, keeping the temperature for 1-2h, filtering, washing, and drying to obtain modified biochar;
[0009] S3: Ultrasonic dispersion of hyperbranched modified nano-ferroferric oxide in deionized water, adding modified biochar and heating to 35-45°C for reaction for 3.5-4h to obtain a composite water treatment agent.
[0010] Furthermore, the preparation method of the branched modified nano-ferroferric oxide comprises the following steps:
[0011] Ultrasonic dispersion of nano-iron tetroxide in ethanol solution, adding ammonia water and tetraethyl silicate successively, reacting at room temperature for 6-7 hours, washing, and drying to obtain coated modified nano-iron tetroxide; pre-treating the coated modified nano-iron tetroxide, ultrasonically dispersing it in ethanol solution, heating it to 75-78°C, adding ammonia water and KH550 successively under constant temperature conditions, keeping the temperature for 6-7 hours, washing, and obtaining amino-modified nano-iron tetroxide; ultrasonically dispersing the amino-modified nano-iron tetroxide in methanol solution, adding methyl acrylate, reacting at room temperature for 24 hours, washing, and drying to obtain branched modified nano-iron tetroxide.
[0012] Furthermore, in the coated modified nano ferroferric oxide, the mass ratio of nano ferroferric oxide to tetraethyl silicate is 1:(4-5); in the amino modified nano ferroferric oxide, the pretreatment step includes heating the coated modified nano ferroferric oxide to 190-200°C and vacuum drying; the mass ratio of coated modified nano ferroferric oxide to KH550 is 1:(4-5); in the branched modified nano ferroferric oxide, the mass ratio of amino modified nano ferroferric oxide to methyl acrylate is 1:(0.02-0.03).
[0013] Furthermore, the preparation method of the quaternary phosphonium salt modified chitosan comprises the following steps:
[0014] The maleic anhydride grafted polymer modified chitosan was ultrasonically dispersed in deionized water, and sodium hydroxide solution and sodium hypochlorite solution were added under ice bath conditions. The mixture was sealed and shaken for 20-30 minutes, and naturally returned to room temperature. Under a nitrogen atmosphere, 1-hydroxybenzotriazole and (3-propylcarboxyl)triphenylphosphonium bromide were added, and the mixture was heated to 80-85° C. for reaction for 24 hours, purified, and dried to obtain quaternary phosphonium salt modified chitosan.
[0015] Furthermore, in the reaction system of chitosan modified by maleic anhydride grafted polymer, sodium hydroxide solution and sodium hypochlorite solution, -CONH2, OH - , ClO -The molar ratio is 1:(0.6-2.4):(0.25-0.95); the concentration of the sodium hydroxide solution is 4-5M; the concentration of the sodium hypochlorite solution is 1.5-2M; the volume ratio of the maleic anhydride grafted polymer modified chitosan: sodium hydroxide solution: sodium hypochlorite solution is 2:1:1; the mass ratio of the maleic anhydride grafted polymer: (3-propylcarboxyl)triphenylphosphonium bromide is 1:(0.3-0.6).
[0016] Furthermore, the preparation method of the maleic anhydride grafted polymer modified chitosan comprises the following steps:
[0017] The carboxymethyl chitosan is ultrasonically dispersed in a deacetic acid solution, maleic anhydride is added, heated to 30-35°C for reaction for 5-6 hours, purified, and dried to obtain maleyl chitosan; acrylamide and maleyl chitosan are added to deionized water, ammonium persulfate solution is added under a nitrogen atmosphere, heated to 45-50°C for reaction for 6-7 hours, maleic anhydride solution is added, the reaction is kept warm for 40-60 minutes, purified, and dried to obtain maleic anhydride grafted polymer modified chitosan.
[0018] Furthermore, in the maleyl chitosan, the mass ratio of carboxymethyl chitosan: maleic anhydride is 1:(2-3); in the maleic anhydride grafted polymer modified chitosan, the mass ratio of maleyl chitosan: acrylamide: maleic anhydride is (30-35):(30-35):(0.6-0.7).
[0019] Furthermore, in the macromolecular polyamide-amine, the mass ratio of ethylenediamine: methyl acrylate is 9: (77.4-86); in the polyamide-amine, the mass ratio of macromolecular polyamide-amine: ethylenediamine is (32.32-36.36): 60; in the hyperbranched modified nano-ferroferric oxide, the mass ratio of branched modified nano-ferroferric oxide: polyamide-amine is (0.15-0.2): (4-5).
[0020] Furthermore, in the modified biochar, the mass ratio of quaternary phosphonium salt modified chitosan:biochar is 1:1;
[0021] Furthermore, in the composite treatment agent, the mass ratio of the hyperbranched modified nano-ferroferric oxide to the modified biochar is (0.8-1.2): (0.8-1.2)
[0022] The concentration of the acetic acid solution is 2% v / v.
[0023] Furthermore, the method for preparing biochar comprises the following steps:
[0024] The macadamia nut shell was washed, dried at 80°C for 24 hours, crushed, and sieved to obtain macadamia nut shell powder; the macadamia nut shell powder was heated to 800°C under a nitrogen atmosphere at a heating rate of 10°C / min, and calcined for 2 hours to obtain biochar.
[0025] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0026] The invention adopts Michael addition reaction, takes ethylenediamine as an initiating core to react with methyl acrylate, and then takes the reaction product as a raw material to continue to react with ethylenediamine to prepare polyamide-amine; uses tetraethyl silicate to coat and modify nano ferroferric oxide, forms a spherical silicon dioxide coating layer on the surface of magnetic nano ferroferric oxide under the catalytic action of ammonia water, controls the vacuum drying temperature at 190-200 DEG C to pre-treat the coated modified nano ferroferric oxide, changes the distribution of silanol groups on the surface, and then carries out two Michael additions with KH550 and methyl acrylate to prepare modified nano ferroferric oxide containing methyl acrylate functional groups, and finally undergoes ester amidation with polyamide-amine to prepare hyperbranched modified nano ferroferric oxide.
[0027] The invention uses maleic chitosan, acrylamide and maleic anhydride to synthesize a cationic polymer with a flocculation effect, controls the addition of maleic anhydride at the end of the polymerization chain of maleic chitosan and acrylamide, caps and terminates the chain polymerization reaction (maleic anhydride is connected to the end of the molecular chain to serve as a "bridge" connected to the hyperbranched modified nano-iron tetroxide), then modifies the polymer containing an acrylamide group based on a Hofmann degradation reaction, and finally reacts with (3-propylcarboxyl) triphenylphosphonium bromide to prepare electronegative quaternary phosphonium salt modified chitosan.
[0028] Due to the previous pretreatment step for the coated modified nano ferroferric oxide, the surface silanol groups include highly active lateral hydroxyl groups and slightly less active para hydroxyl groups, which indirectly controls the number and distribution of acrylate on its surface, in order to facilitate the subsequent ester amidation with polyamide-amine, avoid the steric hindrance effect during the reaction process, and increase the grafting rate of polyamide-amine. The molecular terminal amino group of the hyperbranched modified nano ferroferric oxide is used to react with the maleic anhydride in the biochar modified by quaternary phosphonium salt modified chitosan (cationic polymer flocculant) to open the ring, so that the hyperbranched modified nano ferroferric oxide with demulsification and scale inhibition effects is loaded on the biochar modified by the cationic polymer flocculant, and a composite water treatment agent with both demulsification and flocculation properties is prepared.
[0029] The primary amine, secondary amine and amide groups in the polyamide-amine structure have the function of reducing the oil-water interfacial tension and improving the demulsification ability (depending on the strong polarity of the amide groups in polyamide-amine and quaternary phosphonium salt-modified chitosan, which exist in a hyperbranched structure with controlled quantity and distribution, have strong interfacial activity, can be rapidly adsorbed at the oil-water interface at multiple points, destroy the interfacial film strength, and achieve demulsification); synergistically with the electrical neutralization and adsorption bridging effects of quaternary phosphonium salt-modified chitosan, the purpose of degreasing and removing COD from sewage is achieved. Quaternary phosphonium salt-modified chitosan contains a large number of cationic groups, which reduce the Zeta potential and electrostatic repulsion through the oil-water interface and electrostatic adsorption, destroy the electrostatic stability between the colloid particles, and achieve demulsification. At the same time, combined with magnetic nano-ferroferric tetroxide, it can enhance the collision between particles under the action of magnetic field and gravity field, strengthen the cleaning ability of flocs, and enhance the demulsification effect.
[0030] The present invention uses quaternary phosphonium salt antimicrobial agents to replace traditional quaternary ammonium salt antimicrobial agents. Quaternary phosphonium salts are less likely to form nitrogen-containing disinfection byproducts with carcinogenic risks because the electronegativity of the P element is greater than that of the N element of the quaternary ammonium salt. At the same time, the relative molecular mass and charge of the flocculant are increased, and the flocculant has stronger electronegativity, thereby improving the bridging and electrical neutralization flocculation performance of the material. Hyperbranched-cationic segment.
[0031] The composite water treatment agent can effectively reduce the negative charge of suspended particles by adsorption and electrostatic adsorption to the surface of suspended particles, thereby directly promoting the flocculation of suspended particles formed by solid particles and anionic polymers. This process can not only reduce the suspension stability of sewage, but also destroy the stability of the hydrated double layer. With the collision and aggregation of multiple suspended particles, long-chain floccules are formed, which produces an effective net capture effect during the sedimentation process, further enhancing the flocculation and sedimentation effect. Under the action of the external magnetic field, the sedimentation effect is directly enhanced, which helps to promote the sedimentation of suspended particles, strengthen the net capture sedimentation effect, further enhance the flocculation effect, and has excellent COD removal ability. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] In the following examples, nano-ferroferric oxide has a specification of 50 nm and was purchased from Aladdin Reagent (Shanghai) Co., Ltd.; carboxymethyl chitosan has a specification of carboxylation degree ≥ 80% and was purchased from Shanghai Yuanye Biotechnology Co., Ltd.; (3-propylcarboxyl) triphenylphosphonium bromide was purchased from Shanghai McLean Biochemical Technology Co., Ltd.; and the remaining raw materials are commercially available.
[0034] In the following examples, the preparation method of polyamidoamine comprises the following steps:
[0035] 9 g of ethylenediamine was added to methanol, and 77.4 g of methyl acrylate was added, and the reaction was carried out at room temperature for 24 hours, and the reaction was distilled under reduced pressure to obtain a macromolecular polyamide-amine; 32.32 g of macromolecular polyamide-amine was added to methanol, and 60 g of ethylenediamine was added, and the reaction was carried out at room temperature for 24 hours, and the reaction was distilled under reduced pressure to obtain a polyamide-amine.
[0036] Embodiment 1: A preparation method of a composite water treatment agent based on urban sewage: S1: ultrasonically disperse 1g of nano-ferroferric oxide in an ethanol solution, add 5mL of ammonia water and 4g of tetraethyl silicate successively, react at room temperature for 6h, wash, and dry to obtain coated modified nano-ferroferric oxide; heat 1g of coated modified nano-ferroferric oxide to 190°C for vacuum drying pretreatment, ultrasonically disperse in an ethanol solution, heat to 75°C, add 5mL of ammonia water and 4g of KH550 successively under constant temperature conditions, keep warm for 6h, wash, and obtain amino-modified nano-ferroferric oxide; ultrasonically disperse 1g of amino-modified nano-ferroferric oxide in a methanol solution, add 0.02g of methyl acrylate, react at room temperature for 24h, wash, and dry to obtain branched modified nano-ferroferric oxide; add 0.15g of branched modified nano-ferroferric oxide to ethanol, add 4g of polyamide-amine, heat to 50°C for reaction for 12h, and obtain hyperbranched modified nano-ferroferric oxide;
[0037] S2: 1 g of carboxymethyl chitosan was ultrasonically dispersed in a deacetic acid solution, 2 g of maleic anhydride was added, the mixture was heated to 30°C for reaction for 5 h, purified, and dried to obtain maleyl chitosan; 30 g of acrylamide and 30 g of maleyl chitosan were added to deionized water, and an ammonium persulfate solution was added under a nitrogen atmosphere, the mixture was heated to 45°C for reaction for 6 h, a maleic anhydride solution containing 0.6 g of maleic anhydride was added, the mixture was kept warm for reaction for 40 min, purified, and dried to obtain maleic anhydride grafted polymer modified chitosan;
[0038] S3: 1g of maleic anhydride grafted polymer modified chitosan was ultrasonically dispersed in deionized water, sodium hydroxide solution and sodium hypochlorite solution were added under ice bath conditions, sealed and shaken for 20 minutes, and naturally restored to room temperature. Under nitrogen atmosphere, 0.2g of 1-hydroxybenzotriazole and 0.3g of (3-propylcarboxyl) triphenylphosphonium bromide were added, and the mixture was heated to 80°C for 24 hours, purified, and dried to obtain quaternary phosphonium salt modified chitosan; wherein -CONH2, OH in the reaction system of maleic anhydride grafted polymer modified chitosan, sodium hydroxide solution, and sodium hypochlorite solution - , ClO - The molar ratio is 1:1.2:0.65;
[0039] S4: Add 1 g of quaternary phosphonium salt-modified chitosan to the acetic acid solution, add 1 g of biochar, heat to 40 °C and stir evenly, add 1 g of glutaraldehyde, continue stirring, adjust the pH of the reaction system to 9, keep the reaction at this temperature for 1 h, filter, wash, and dry to obtain modified biochar;
[0040] S5: 0.8 g of hyperbranched modified nano-ferroferric oxide was ultrasonically dispersed in deionized water, 1.2 g of modified biochar was added, heated to 35° C. and reacted for 3.5 h to obtain a composite water treatment agent.
[0041] Example 2: A method for preparing a composite water treatment agent based on urban sewage: S3: 1g of maleic anhydride grafted polymer modified chitosan is ultrasonically dispersed in deionized water, sodium hydroxide solution and sodium hypochlorite solution are added under ice bath conditions, sealed and shaken for 20 minutes, and naturally restored to room temperature, 0.2g of 1-hydroxybenzotriazole and 0.6g of (3-propylcarboxyl) triphenylphosphonium bromide are added under nitrogen atmosphere, heated to 80°C for reaction for 24 hours, purified, and dried to obtain quaternary phosphonium salt modified chitosan; wherein, -CONH2, OH in the reaction system of maleic anhydride grafted polymer modified chitosan, sodium hydroxide solution, and sodium hypochlorite solution - , ClO - The molar ratio is 1:1.2:0.65;
[0042] S5: 0.8 g of hyperbranched modified nano-ferroferric oxide was ultrasonically dispersed in deionized water, 1.2 g of modified biochar was added, and the mixture was heated to 35° C. and reacted for 3.5 h to obtain a composite water treatment agent;
[0043] The remaining steps are the same as those in Example 1.
[0044] Example 3: A method for preparing a composite water treatment agent based on urban sewage: S3: 1g of maleic anhydride grafted polymer modified chitosan is ultrasonically dispersed in deionized water, sodium hydroxide solution and sodium hypochlorite solution are added under ice bath conditions, sealed and shaken for 20 minutes, and naturally restored to room temperature, 0.2g of 1-hydroxybenzotriazole and 0.6g of (3-propylcarboxyl) triphenylphosphonium bromide are added under nitrogen atmosphere, heated to 80°C for reaction for 24 hours, purified, and dried to obtain quaternary phosphonium salt modified chitosan; wherein, -CONH2, OH in the reaction system of maleic anhydride grafted polymer modified chitosan, sodium hydroxide solution, and sodium hypochlorite solution - , ClO - The molar ratio is 1:1.2:0.65;
[0045] S5: 1 g of hyperbranched modified nano-ferroferric oxide was ultrasonically dispersed in deionized water, 1 g of modified biochar was added, and the mixture was heated to 35°C and reacted for 3.5 h to obtain a composite water treatment agent;
[0046] The remaining steps are the same as those in Example 1.
[0047] Example 4: A method for preparing a composite water treatment agent based on urban sewage: S3: 1g of maleic anhydride grafted polymer modified chitosan is ultrasonically dispersed in deionized water, sodium hydroxide solution and sodium hypochlorite solution are added under ice bath conditions, sealed and shaken for 20 minutes, and naturally restored to room temperature, 0.2g of 1-hydroxybenzotriazole and 0.6g of (3-propylcarboxyl) triphenylphosphonium bromide are added under nitrogen atmosphere, heated to 80°C for reaction for 24 hours, purified, and dried to obtain quaternary phosphonium salt modified chitosan; wherein -CONH2, OH in the reaction system of maleic anhydride grafted polymer modified chitosan, sodium hydroxide solution, and sodium hypochlorite solution - , ClO - The molar ratio is 1:1.2:0.65;
[0048] S5: 1.2 g of hyperbranched modified nano-ferroferric oxide was ultrasonically dispersed in deionized water, 0.8 g of modified biochar was added, and the mixture was heated to 35° C. and reacted for 3.5 h to obtain a composite water treatment agent;
[0049] The remaining steps are the same as those in Example 1.
[0050] Comparative Example 1: A method for preparing a composite water treatment agent based on urban sewage: S1: ultrasonically disperse 1g of nano-ferroferric oxide in an ethanol solution, add 5mL of ammonia water and 4g of tetraethyl silicate successively, react at room temperature for 6h, wash, and dry to obtain coated modified nano-ferroferric oxide; ultrasonically disperse 1g of coated modified nano-ferroferric oxide in an ethanol solution, heat to 75°C, add 5mL of ammonia water and 4g of KH550 successively under constant temperature conditions, keep warm for 6h, wash, and obtain amino-modified nano-ferroferric oxide; ultrasonically disperse 1g of amino-modified nano-ferroferric oxide in a methanol solution, add 0.02g of methyl acrylate, react at room temperature for 24h, wash, and dry to obtain branched modified nano-ferroferric oxide; add 0.15g of branched modified nano-ferroferric oxide to ethanol, add 4g of polyamide-amine, heat to 50°C and react for 12h to obtain hyperbranched modified nano-ferroferric oxide;
[0051] The remaining steps are the same as those in Example 1.
[0052] Comparative Example 2: A method for preparing a composite water treatment agent based on urban sewage: S1: ultrasonically disperse 1g of nano-iron tetroxide in an ethanol solution, add 5mL of ammonia water and 4g of tetraethyl silicate successively, react at room temperature for 6h, wash, and dry to obtain coated modified nano-iron tetroxide; heat 1g of coated modified nano-iron tetroxide to 400℃ for vacuum drying pretreatment, ultrasonically disperse it in an ethanol solution, heat it to 75℃, add 5mL of ammonia water and 4g of KH550 successively under constant temperature conditions, keep warm for 6h, wash, and obtain amino-modified nano-iron tetroxide; ultrasonically disperse 1g of amino-modified nano-iron tetroxide in a methanol solution, add 0.02g of methyl acrylate, react at room temperature for 24h, wash, and dry to obtain branched modified nano-iron tetroxide; add 0.15g of branched modified nano-iron tetroxide to ethanol, add 4g of polyamide-amine, heat to 50℃ for reaction for 12h, and obtain hyperbranched modified nano-iron tetroxide;
[0053] The remaining steps are the same as those in Example 1.
[0054] Comparative Example 3: A method for preparing a composite water treatment agent based on urban sewage: S3: 1g of maleic anhydride grafted polymer modified chitosan is ultrasonically dispersed in deionized water, sodium hydroxide solution and sodium hypochlorite solution are added under ice bath conditions, sealed and shaken for 20 minutes, naturally restored to room temperature, 0.2g of 1-hydroxybenzotriazole and 0.3g of acryloyloxyethyl trimethylammonium chloride are added under nitrogen atmosphere, heated to 80°C for reaction for 24 hours, purified, and dried to obtain quaternary phosphonium salt modified chitosan; wherein, -CONH2, OH in the reaction system of maleic anhydride grafted polymer modified chitosan, sodium hydroxide solution, and sodium hypochlorite solution - , ClO - The molar ratio is 1:1.2:0.65;
[0055] The remaining steps are the same as those in Example 1.
[0056] Comparative Example 4: A method for preparing a composite water treatment agent based on urban sewage: S2: 1 g of carboxymethyl chitosan was ultrasonically dispersed in a deacetic acid solution, 2 g of maleic anhydride was added, heated to 30°C for reaction for 5 h, purified, and dried to obtain maleyl chitosan; 30 g of acrylamide and 30 g of maleyl chitosan were added to deionized water, and ammonium persulfate solution was added under a nitrogen atmosphere, heated to 45°C for reaction for 3 h, maleic anhydride solution containing 0.6 g of maleic anhydride was added, and the reaction was kept warm for 40 min, purified, and dried to obtain maleic anhydride grafted polymer modified chitosan;
[0057] The remaining steps are the same as those in Example 1.
[0058] Experiment: Test environment: Under magnetic field, adjust the magnetic field direction vertically downward by permanent magnet, use N35 neodymium iron boron permanent magnet, the maximum magnetic energy product is 35MGOe, that is, 270KA / m 3 ;
[0059] Performance test: Take urban sewage (not degreased) as the treatment object, set the addition amount of composite treatment agent at 30mg / L, the experimental temperature at 25℃, shake well and let it stand for 30min, take the middle layer clear liquid to determine the oil content, and calculate the oil removal rate; use the same method, test according to GB11901-1989 and GB11914-1989, and calculate the suspended solids removal rate and COD removal rate.
[0060] Table 1 Composite water treatment agent performance test data table
[0061] Oil removal rate / % Suspended matter removal rate / % COD removal rate / % Example 1 83.93 88.78 89.18 Example 2 85.15 90.12 91.11 Example 3 90.22 93.32 94.08 Example 4 88.13 91.87 92.10 Comparative Example 1 72.57 75.08 75.98 Comparative Example 2 68.54 69.68 71.06 Comparative Example 3 78.98 84.45 85.15 Comparative Example 4 74.18 82.83 83.20
[0062] Conclusion: The composite water treatment agent prepared in this application has excellent demulsification and flocculation properties.
[0063] In Comparative Example 1, the coated modified nano-ferroferric oxide was not subjected to heating treatment, resulting in a disordered distribution of hydroxyl groups on its surface. The silicon hydroxyl groups and water molecules were combined with hydrogen bonds to form multi-layer bound water. The number of active hydroxyl groups was small, and the demulsification and flocculation performance of the composite water treatment agent was reduced.
[0064] In Comparative Example 2, the coated modified nano-ferroferric oxide was heated at 400° C., so that the internal hydrogen bonds of the surface silanol groups were basically broken and all adjacent hydroxyl groups were lost, resulting in a decrease in the grafting rate, and the demulsification and flocculation performance of the composite water treatment agent was reduced.
[0065] Comparative Example 3 uses acryloyloxyethyl trimethyl ammonium chloride to replace (3-propylcarboxyl) triphenylphosphonium bromide, resulting in a decrease in the electronegativity of the quaternary phosphonium salt-modified chitosan and a decrease in the flocculation performance of the composite water treatment agent.
[0066] In Comparative Example 4, maleic anhydride was added too early, and the polymerization reaction of the chain ended prematurely, resulting in a decrease in the number of amide groups in the chain segment and a decrease in the number of (3-propylcarboxyl)triphenylphosphonium bromide grafts, resulting in a decrease in the electronegativity of the quaternary phosphonium salt-modified chitosan and a decrease in the flocculation performance of the composite water treatment agent.
[0067] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a composite water treatment agent based on urban sewage, characterized in that: The following steps are involved: S1: Add ethylenediamine to methanol, add methyl acrylate, react at room temperature, and distill under reduced pressure to obtain macromolecular polyamide-amine; add macromolecular polyamide-amine to methanol, add ethylenediamine, react at room temperature, and distill under reduced pressure to obtain polyamide-amine; add branched modified nano-ferroferric oxide to ethanol, add polyamide-amine, heat to 50-55°C and react for 12-14h to obtain hyperbranched modified nano-ferroferric oxide; S2: adding quaternary phosphonium salt modified chitosan to acetic acid solution, adding biochar, heating to 40-45°C and stirring evenly, adding glutaraldehyde, continuing stirring, adjusting the pH of the reaction system to 9-10, keeping the temperature for 1-2h, filtering, washing, and drying to obtain modified biochar; S3: Ultrasonic dispersion of hyperbranched modified nano-ferroferric oxide in deionized water, adding modified biochar and heating to 35-45° C. for reaction for 3.5-4 hours to obtain a composite water treatment agent; The preparation method of the branched modified nano-ferroferric oxide comprises the following steps: Ultrasonic dispersion of nano-iron tetroxide in an ethanol solution, adding ammonia water and tetraethyl silicate successively, reacting at room temperature for 6-7 hours, washing, and drying to obtain coated modified nano-iron tetroxide; pre-treating the coated modified nano-iron tetroxide, ultrasonically dispersing it in an ethanol solution, heating it to 75-78°C, adding ammonia water and KH550 successively at a constant temperature, keeping the temperature for 6-7 hours, washing, and obtaining amino-modified nano-iron tetroxide; ultrasonically dispersing the amino-modified nano-iron tetroxide in a methanol solution, adding methyl acrylate, reacting at room temperature, washing, and drying to obtain branched modified nano-iron tetroxide; The preparation method of the quaternary phosphonium salt modified chitosan comprises the following steps: The maleic anhydride grafted polymer modified chitosan was ultrasonically dispersed in deionized water, sodium hydroxide solution and sodium hypochlorite solution were added under ice bath conditions, sealed and shaken for 20-30 minutes, and naturally restored to room temperature. Under nitrogen atmosphere, 1-hydroxybenzotriazole and (3-propylcarboxyl)triphenylphosphonium bromide were added, and the mixture was heated to 80-85°C for reaction for 24 hours, purified, and dried to obtain quaternary phosphonium salt modified chitosan; The method for preparing maleic anhydride grafted polymer modified chitosan comprises the following steps: The carboxymethyl chitosan is ultrasonically dispersed in a deacetic acid solution, maleic anhydride is added, heated to 30-35°C for reaction for 5-6 hours, purified, and dried to obtain maleyl chitosan; acrylamide and maleyl chitosan are added to deionized water, ammonium persulfate solution is added under a nitrogen atmosphere, heated to 45-50°C for reaction for 6-7 hours, maleic anhydride solution is added, the reaction is kept warm for 40-60 minutes, purified, and dried to obtain maleic anhydride grafted polymer modified chitosan.
2. The method for preparing a composite water treatment agent based on urban sewage according to claim 1, characterized in that: In the coated modified nano ferroferric oxide, the mass ratio of nano ferroferric oxide to tetraethyl silicate is 1:(4-5); in the amino modified nano ferroferric oxide, the pretreatment step includes heating the coated modified nano ferroferric oxide to 190-200° C. and vacuum drying; The mass ratio of coated modified nano-ferroferric oxide to KH550 is 1:(4-5); in the branched modified nano-ferroferric oxide, the mass ratio of amino-modified nano-ferroferric oxide to methyl acrylate is 1:(0.02-0.03).
3. The method for preparing a composite water treatment agent based on urban sewage according to claim 1, characterized in that: The mass ratio of the maleic anhydride grafted polymer to (3-propylcarboxyl)triphenylphosphonium bromide is 1:(0.3-0.6).
4. The method for preparing a composite water treatment agent based on urban sewage according to claim 1, characterized in that: In the maleyl chitosan, the mass ratio of carboxymethyl chitosan: maleic anhydride is 1:(2-3); in the maleic anhydride grafted polymer modified chitosan, the mass ratio of maleyl chitosan: acrylamide: maleic anhydride is (30-35):(30-35):(0.6-0.7).
5. The method for preparing a composite water treatment agent based on urban sewage according to claim 1, characterized in that: In the hyperbranched modified nano-ferroferric oxide, the mass ratio of branched modified nano-ferroferric oxide to polyamide-amine is (0.15-0.2):(4-5).
6. The method for preparing a composite water treatment agent based on urban sewage according to claim 1, characterized in that: In the modified biochar, the mass ratio of quaternary phosphonium salt modified chitosan:biochar is 1:1; in the composite water treatment agent, the mass ratio of hyperbranched modified nano-ferroferric oxide:modified biochar is (0.8-1.2):(0.8-1.2).
7. A composite water treatment agent prepared according to the method for preparing a composite water treatment agent based on urban sewage according to any one of claims 1 to 6.
Citation Information
Patent Citations
Preparation method of hyperbranched magnetic demulsification flocculant for oil field water treatment
CN113354049A
Sewage treatment flocculant and preparation method thereof
CN117069215A