Copper-based scintillator-microporous template, dual-energy X-ray detector and preparation method

By combining the copper-based scintillator-microporous template and the manganese ion-doped copper-based scintillator, the problems of scintillator self-absorption and layer thickness limitation are solved, and a high-resolution dual-energy X-ray detector is realized, which is suitable for medicine. , safety inspection and other fields.

CN118501924BActive Publication Date: 2024-10-29UNIV OF SCI & TECH OF CHINA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410955287.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-29
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

The scintillator in existing scintillation detectors has limited application in the field of dual-energy detection due to self-absorption phenomenon and layer thickness limitations. For example, the half-peak width of the luminescence of CsI:Tl scintillator limits its application in the field of dual-energy detection. limit.

Method used

Using a copper-based scintillator-microporous template, the microporous template is filled with copper-based scintillator and manganese ion-doped copper-based scintillator, and an X-ray hardened layer is introduced between the two, combined with a visible light detector to form a double Energy X-ray detector uses micropore structure to reduce photon lateral diffusion and improve spatial resolution.

Benefits of technology

It achieves high light yield and small luminescence half-peak width, avoids self-absorption, improves the spatial resolution and imaging clarity of dual-energy X-ray detectors, and is suitable for high-resolution imaging and material composition differentiation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118501924B_ABST
    Figure CN118501924B_ABST
Patent Text Reader

Abstract

The present invention provides a copper-based scintillator-microporous template, a dual-energy X-ray detector and a preparation method. The copper-based scintillator-microporous template comprises: a microporous template, a copper-based scintillator crystal, and a copper-based scintillator crystal doped with manganese ions; wherein the microporous template comprises a plurality of evenly distributed holes, each of the plurality of holes is used to fill the copper-based scintillator crystal and the copper-based scintillator crystal doped with manganese ions, respectively, and each of the plurality of holes after filling is the same, the copper-based scintillator crystal is prepared based on copper-based halide powder, and the copper-based scintillator crystal doped with manganese ions is obtained by doping manganese ions in the copper-based halide powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of photoelectric detection technology, in particular to the field of indirect detection in radiation detection, and more particularly to a copper-based scintillator-microporous template, a dual-energy X-ray detector and a preparation method thereof. Background Art

[0002] X-ray detectors are widely used in medical diagnosis, radiotherapy, safety inspection, industrial non-destructive testing and other fields. In traditional X-ray imaging technology, the imaging results are displayed by grayscale values. The grayscale values ​​are distinguished based on the different attenuation coefficients of different objects to X-rays, which depends on their atomic number, physical density and beam energy. This method of distinguishing the internal material distribution or element composition of an object by relying on the attenuation coefficient distribution is prone to misjudgment and image artifacts of varying degrees in application. With the increasing requirements for X-ray imaging, there is an urgent need for an imaging technology that can more accurately reflect the internal information distribution of an object.

[0003] Dual-energy X-ray detection technology is one of the effective methods to achieve energy resolution and density resolution. Thanks to the development of radiation source and detector technology and the progress of image reconstruction theory, dual-energy X-ray detectors have been widely used in many fields. For example, in the field of medical diagnosis, dual-energy X-ray detectors are mainly used for separation between bones and soft tissues, measurement of bone density and iron content in the liver, etc.; in radiotherapy, dual-energy X-ray detectors are mainly used to delineate lesion areas and calculate radiation doses, etc.; in the field of security inspection, dual-energy X-ray detectors are mainly used to inspect low atomic number substances, such as alcohol and other contraband.

[0004] In the process of realizing the concept of the present invention, the inventors found that the scintillators in the current scintillation detectors, such as lead-based perovskite scintillators, are limited in their application in the field of dual-energy detection due to the widespread self-absorption phenomenon that leads to light yield loss and the thickness of the scintillator layer. For example, the half-peak width of the luminescence of CsI:Tl scintillator is as high as 200nm, which limits the application of CsI:Tl scintillator in the field of dual-energy detection. Summary of the invention

[0005] In view of this, the present invention provides a copper-based scintillator-microporous template, a dual-energy X-ray detector and a preparation method.

[0006] The first aspect of the present invention provides a copper-based scintillator-microporous template, comprising: a microporous template, a copper-based scintillator crystal, and a copper-based scintillator crystal doped with manganese ions; wherein the microporous template comprises a plurality of evenly distributed holes, each of the plurality of holes is used to fill the copper-based scintillator crystal and the copper-based scintillator crystal doped with manganese ions, respectively, and each of the plurality of holes after filling is the same, the copper-based scintillator crystal is prepared based on copper-based halide powder, and the copper-based scintillator crystal doped with manganese ions is obtained by doping manganese ions in the copper-based halide powder.

[0007] According to an embodiment of the present invention, the copper-based scintillator-microporous template also includes an X-ray hardening layer; wherein the X-ray hardening layer is located between the copper-based scintillator crystal and the copper-based scintillator crystal doped with manganese ions, and is used to separate the X-rays absorbed by the copper-based scintillator crystal and the copper-based scintillator crystal doped with manganese ions.

[0008] According to an embodiment of the present invention, the height of the X-ray hardening layer is 500 μm to 2 mm, and the X-ray hardening layer is prepared based on polydimethylsiloxane.

[0009] According to an embodiment of the present invention, the diameter of each of the multiple holes is 500nm~100μm, the height of each of the multiple holes is 10μm~10mm, and the microporous template includes at least one of the following: anodized aluminum, aluminum capillary, silicon, silicon oxide.

[0010] The second aspect of the present invention provides a dual-energy X-ray detector based on a copper-based scintillator-micropore template, comprising: a copper-based scintillator-micropore template and a visible light detector; wherein the copper-based scintillator-micropore template is the above-mentioned copper-based scintillator-micropore template, the visible light detector is in contact with the copper-based scintillator-micropore template, and the visible light detector is located below the copper-based scintillator crystal, and is used to detect and convert the visible light photons generated when the X-ray photons interact with the copper-based scintillator crystal or the manganese ion-doped copper-based scintillator crystal into electrical signals.

[0011] According to an embodiment of the present invention, the dual-energy X-ray detector further comprises a packaging layer; wherein the packaging layer is used to package the surface of the copper-based scintillator-microporous template that is not in contact with the visible light detector.

[0012] The third aspect of the present invention provides a method for preparing a copper-based scintillator-microporous template, comprising: heating a copper-based halide powder covering the microporous template so that the copper-based halide powder reaches a molten state and is filled into the microporous template, and cooling so that the molten copper-based scintillator powder forms crystals in the microporous template to obtain a copper-based scintillator crystal layer, wherein the copper-based halide powder is obtained by grinding solid materials of AX and CuX, A represents an alkali metal element, and X represents a halogen element; heating a copper-based halide powder doped with manganese ions covering the microporous template so that the copper-based halide powder doped with manganese ions reaches a molten state and is filled into the microporous template, and cooling so that the molten copper-based scintillator powder doped with manganese ions forms crystals in the microporous template to obtain a copper-based scintillator crystal layer doped with manganese ions, wherein the copper-based scintillator powder doped with manganese ions is obtained by grinding solid materials of AX, CuX and MnX2; coupling the copper-based scintillator crystal layer with the copper-based scintillator crystal layer doped with manganese ions to obtain a copper-based scintillator-microporous template.

[0013] According to an embodiment of the present invention, the preparation method of the copper-based scintillator-microporous template also includes: pouring polydimethylsiloxane into the microporous template and curing it to form an X-ray hardening layer; sequentially superimposing and coupling the copper-based scintillator crystal layer, the X-ray hardening layer and the copper-based scintillator crystal layer doped with manganese ions to obtain the copper-based scintillator-microporous template.

[0014] The fourth aspect of the present invention provides a method for preparing a dual-energy X-ray detector based on a copper-based scintillator-microporous template, comprising: coupling the copper-based scintillator-microporous template with a visible light detector to obtain a dual-energy X-ray detector, wherein the copper-based scintillator-microporous template is obtained according to the above-mentioned method for preparing the copper-based scintillator-microporous template, and the visible light detector is located below the copper-based scintillator crystal.

[0015] According to an embodiment of the present invention, the method for preparing a dual-energy X-ray detector based on a copper-based scintillator-microporous template also includes: packaging the surface of the copper-based scintillator-microporous template that is not in contact with the visible light detector with optical glue to obtain a dual-energy X-ray detector.

[0016] According to an embodiment of the present invention, the copper-based scintillator crystal has a high light yield, no self-absorption phenomenon and a small luminescence half-width. In addition, by doping different elements, the luminescence wavelength of the copper-based scintillator crystal can be adjusted. Therefore, the preparation of a dual-energy X-ray detector can be achieved based on the copper-based scintillator crystal. The copper-based scintillator crystal has excellent light transmittance and can improve the extraction rate of photons, but due to the improvement of light transmittance, the lateral diffusion of photons in the scintillator will greatly reduce the spatial resolution of the detector. A microporous structure is introduced into the scintillator layer, which reduces the lateral diffusion of photons in the scintillator layer and the crosstalk between the scintillator layers. The copper-based scintillator-microporous template obtained in this way can be used in a dual-energy X-ray detector to improve the spatial resolution capability of the dual-energy X-ray detector. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The above and other objects, features and advantages of the present invention will become more apparent through the following description of the embodiments of the present invention with reference to the accompanying drawings, in which:

[0018] Figure 1 A schematic diagram of the structure of a copper-based scintillator-microporous template in an embodiment of the present invention is shown;

[0019] Figure 2a Schematic diagram of the propagation path of photons in copper-based scintillators;

[0020] Figure 2b Schematic diagram of the propagation path of photons in the copper-based scintillator-microporous template;

[0021] Figure 3 A schematic diagram of the structure of a dual-energy X-ray flat panel detector in an embodiment of the present invention is shown;

[0022] Figure 4 The luminous intensity of the copper-based scintillator powder and the manganese-ion-doped copper-based scintillator powder prepared in Example 1 of the present invention under X-rays is shown;

[0023] Figure 5 The imaging image of the dual-energy X-ray flat panel detector without microporous template prepared in Comparative Example 1 of the present invention on the line pair card is shown;

[0024] Figure 6 The imaging image of the dual-energy X-ray flat panel detector for line pair card prepared in Example 1 of the present invention is shown;

[0025] Figure 7 The Cs3Cu2I5 prepared by Example 2 of the present invention and the Cs3Cu2I5:15%Mn prepared by ball milling are shown. 2+ And Cs3Cu2I5:15%Mn prepared by melting method 2+ The luminous intensity of radiation under X-rays. DETAILED DESCRIPTION

[0026] Below, embodiments of the present invention will be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In the following detailed description, for ease of explanation, many specific details are set forth to provide a comprehensive understanding of embodiments of the present invention. However, it is apparent that one or more embodiments may also be implemented without these specific details. In addition, in the following description, descriptions of known structures and technologies are omitted to avoid unnecessary confusion of concepts of the present invention.

[0027] The terms used herein are only for describing specific embodiments and are not intended to limit the present invention. The terms "comprise", "include", etc. used herein indicate the existence of features, steps, operations and / or components, but do not exclude the existence or addition of one or more other features, steps, operations or components.

[0028] All terms (including technical and scientific terms) used herein have the meanings commonly understood by those skilled in the art unless otherwise defined. It should be noted that the terms used herein should be interpreted as having a meaning consistent with the context of this specification and should not be interpreted in an idealized or overly rigid manner.

[0029] When using expressions such as "at least one of A, B, and C, etc.", they should generally be interpreted according to the meaning of the expression commonly understood by those skilled in the art (for example, "a system having at least one of A, B, and C" should include but is not limited to a system having A alone, B alone, C alone, A and B, A and C, B and C, and / or A, B, C, etc.).

[0030] In the process of realizing the concept of the present invention, the inventors found that the scintillators in the current scintillation detectors, such as lead-based perovskite scintillators, are limited in their application in the field of dual-energy detection due to the widespread self-absorption phenomenon that leads to light yield loss and the thickness of the scintillator layer. For example, the half-peak width of the luminescence of CsI:Tl scintillator is as high as 200nm, which limits the application of CsI:Tl scintillator in the field of dual-energy detection.

[0031] Based on this, the present invention provides a copper-based scintillator-microporous template, a dual-energy X-ray detector and a preparation method.

[0032] The following will be passed Figure 1 to Figure 7 The embodiments of the present invention are described in detail.

[0033] Figure 1 A schematic structural diagram of a copper-based scintillator-microporous template in an embodiment of the present invention is shown.

[0034] like Figure 1 As shown, the copper-based scintillator-microporous template 100 may include: a microporous template 101 , a copper-based scintillator crystal 102 and a copper-based scintillator crystal 103 doped with manganese ions.

[0035] The microporous template 101 may include a plurality of evenly distributed holes A, each of which may be used to fill a copper-based scintillator crystal 102 and a copper-based scintillator crystal 103 doped with manganese ions, respectively. After being filled, each of the plurality of holes A is identical. The copper-based scintillator crystal 102 is prepared based on a copper-based halide powder, and the copper-based scintillator crystal 103 doped with manganese ions is obtained by doping manganese ions in the copper-based halide powder.

[0036] According to an embodiment of the present invention, chemical constituent elements of the copper-based halide powder may include alkali metal elements, copper elements, and halogen elements.

[0037] Optionally, the chemical composition formula of the copper-based halide powder may include: m Cu n X m+n ; Wherein, A represents an alkali metal element, X represents a halogen element, and m and n are both real numbers.

[0038] Optionally, the alkali metal element may include at least one of the following: Cs + 、Na + , K + , Rb + .

[0039] Optionally, the halogen element may include at least one of the following: - Br - , Cl - .

[0040] According to the embodiment of the present invention, since the luminescence mechanism of the copper-based halide powder is the self-trapped exciton luminescence generated by the lattice distortion caused by the electron-phonon coupling, the copper-based halide powder has the advantages of high light yield, no self-absorption, and narrow half-peak width of luminescence. These advantages enable the preparation of copper-based scintillator crystals that meet the preset requirements based on the copper-based halide powder. The preset requirements may be the requirements of having sufficient thickness to fully absorb X-rays and having high light yield, and being able to meet the requirements of dual-energy detection that the scintillator needs to have a small half-peak width of luminescence to facilitate the distinction of different scintillator luminescence wavelengths. For example, the copper-based scintillator crystal 101 has high light yield, no self-absorption, and a luminescence half-peak width of about 50nm.

[0041] According to an embodiment of the present invention, the copper-based halide powder is doped with manganese ions (Mn 2+ ) can be achieved by adding MnX2; wherein Mn is manganese element and X represents a halogen element.

[0042] According to an embodiment of the present invention, Mn 2+ The emission wavelength of the doped copper-based scintillator crystal has an obvious red shift compared to the copper-based scintillator crystal, and can red shift the emission wavelength from 450nm to 550nm while maintaining a high light yield.

[0043] According to an embodiment of the present invention, the copper-based scintillator crystal has a high light yield, no self-absorption phenomenon and a small half-peak width of luminescence. In addition, by doping different elements, the luminescence wavelength of the copper-based scintillator crystal can be adjusted because the self-trapped excitons generated in the copper-based halide powder can be transferred to the manganese ions to emit light. Therefore, the preparation of a dual-energy X-ray detector can be achieved based on the copper-based scintillator crystal. The copper-based scintillator crystal has excellent light transmittance and can improve the extraction rate of photons, but due to the improvement of light transmittance, the lateral diffusion of photons in the scintillator will greatly reduce the spatial resolution of the detector. A microporous structure is introduced into the scintillator layer to reduce the lateral diffusion of photons in the scintillator layer and the crosstalk between the scintillator layers. The copper-based scintillator-microporous template obtained in this way can be used in a dual-energy X-ray detector to improve the spatial resolution of the dual-energy X-ray detector.

[0044] According to an embodiment of the present invention, the diameter of each hole in the plurality of holes A may be 500nm-100μm, for example, including but not limited to: 500nm, 1μm, 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm.

[0045] According to an embodiment of the present invention, the diameter of each hole in the plurality of holes A is less than 500 nm, which may affect the difficulty of preparation or require high resolution of the visible light detector when preparing a dual-energy X-ray detector using a copper-based scintillator-micropore template. The diameter of each hole in the plurality of holes is greater than 100 μm, which may reduce the spatial resolution.

[0046] According to an embodiment of the present invention, the height of each hole in the multiple holes A can be 10μm~10mm, for example, it can include but is not limited to: 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 500μm, 1mm, 5mm, 10mm.

[0047] According to an embodiment of the present invention, the height of each hole in the plurality of holes A is less than 10 μm, which will affect the attenuation of X-rays. The height of each hole in the plurality of holes A is greater than 10 mm, which will waste the material of the microporous template.

[0048] According to an embodiment of the present invention, the microporous template 101 may include at least one of the following: anodized aluminum, aluminum capillary, silicon, silicon oxide.

[0049] According to another embodiment of the present invention, Figure 1 As shown, the copper-based scintillator-microporous template 100 may also include an X-ray hardening layer 104; wherein the X-ray hardening layer 104 is located between the copper-based scintillator crystals 102 and the manganese ion-doped copper-based scintillator crystals 103, and is used to separate the X-ray energy spectra absorbed by the copper-based scintillator crystals 102 and the manganese ion-doped copper-based scintillator crystals 103.

[0050] According to an embodiment of the present invention, the height of the X-ray hardening layer 104 may be 500 μm to 2 mm, for example, may include but is not limited to: 500 μm, 750 μm, 1 mm, 1.5 mm, 1 mm, 1.5 mm, 2 mm.

[0051] According to an embodiment of the present invention, the X-ray hardening layer 104 may be glass or a material with high transparency and significant attenuation of X-rays. For example, the X-ray hardening layer 104 may be prepared based on polydimethylsiloxane.

[0052] According to an embodiment of the present invention, since the absorption rate of copper-based scintillator crystals for X-rays is extremely close, an X-ray hardening layer is introduced between two layers of scintillator crystals for further optimization, which has a separation effect on the X-ray energy spectra absorbed by the two layers of scintillator crystals. Therefore, the dual-energy X-ray flat-panel detector prepared using the above-mentioned copper-based scintillator-microporous template containing the X-ray hardening layer has high energy resolution.

[0053] Figure 2a Schematic diagram of the propagation path of photons in copper-based scintillators; Figure 2b Schematic diagram of the propagation path of photons in the copper-based scintillator-microporous template.

[0054] It should be noted that Figure 2 a and Figure 2b All of them are taken as examples including an X-ray hardened layer.

[0055] Figure 2a Herein, the copper-based scintillator refers to a copper-based scintillator without a microporous template compared to a copper-based scintillator-microporous template.

[0056] The photons generated by the copper-based scintillator undergo a scattering process, such as Figure 2a As shown in Figure 1, due to the lateral propagation of photons, the imaging spatial resolution of the detector will be reduced. By introducing the micro-hole template, the photons of the detector will be confined to the vertical micro-hole channel, as shown in Figure 1. Figure 2b As shown, the lateral propagation of photons can be reduced, greatly improving the spatial resolution.

[0057] Based on the copper-based scintillator-microporous template provided by the present invention, the present invention also provides a dual-energy X-ray detector based on the copper-based scintillator-microporous template.

[0058] Figure 3 A schematic structural diagram of a dual-energy X-ray flat panel detector in an embodiment of the present invention is shown.

[0059] like Figure 3 As shown, in this embodiment, the dual-energy X-ray flat panel detector 300 may include: a copper-based scintillator-microporous template 100 and a visible light detector 301 .

[0060] The copper-based scintillator-microporous template 100 can be the copper-based scintillator-microporous template provided above, and the visible light detector 301 is in contact with the copper-based scintillator-microporous template 100. The visible light detector 301 is located below the copper-based scintillator crystal 102, and is used to detect and convert the visible light photons generated when the X-ray photons interact with the copper-based scintillator crystal 102 or the manganese ion-doped copper-based scintillator crystal 103 into electrical signals.

[0061] According to the embodiment of the present invention, the two layers of scintillator crystals of the dual-energy X-ray flat panel detector are both composed of copper-based scintillators, and the only difference is that one layer of the scintillator crystal is doped with manganese, which changes the luminescent wavelength and narrows the luminescent half-peak width, which can meet the dual-energy detector's requirement that the scintillator has a smaller luminescent half-peak width to facilitate the distinction of different scintillator luminescent wavelengths. In addition, since copper-based halide powder has the advantages of high light yield and no self-absorption, copper-based scintillator crystals with sufficient thickness that can fully absorb X-rays and have high light yield can be prepared, so the dual-energy X-ray flat panel detector has high spatial resolution.

[0062] According to the embodiments of the present invention, the high-resolution dual-energy X-ray flat-panel detector provided by the present invention can achieve high-resolution imaging while distinguishing the composition of materials, compared with the scintillators (such as CsI: Tl, GOS: Tb) currently widely used in commercial X-ray flat-panel detectors, and has an obvious auxiliary effect on security inspections and medical imaging.

[0063] According to an embodiment of the present invention, the dual-energy X-ray detector 300 may further include a packaging layer 302 ; wherein the packaging layer 302 is used to package the surface of the copper-based scintillator-microporous template 100 that is not in contact with the visible light detector 301 .

[0064] According to the embodiment of the present invention, the surface of the copper-based scintillator-microporous template that is not in contact with the visible light detector is encapsulated by the encapsulation layer, so that the two layers of scintillator crystals can be protected and the service life can be extended.

[0065] Based on the copper-based scintillator-microporous template provided by the present invention, the present invention also provides a method for preparing a copper-based scintillator-microporous template, which may include operations S1 to S3.

[0066] In operation S1, the copper-based halide powder covering the microporous template is heated to make the copper-based halide powder molten and filled into the microporous template, and then cooled to make the molten copper-based scintillator powder form crystals in the microporous template to obtain a copper-based scintillator crystal layer.

[0067] In operation S2, the copper-based halide powder doped with manganese ions covering the microporous template is heated so that the copper-based halide powder doped with manganese ions reaches a molten state and is filled into the microporous template, and the temperature is lowered so that the molten copper-based scintillator powder doped with manganese ions forms crystals in the microporous template to obtain a copper-based scintillator crystal layer doped with manganese ions.

[0068] In operation S3 , a copper-based scintillator crystal layer is coupled with a copper-based scintillator crystal layer doped with manganese ions to obtain a copper-based scintillator-micropore template.

[0069] According to an embodiment of the present invention, the copper-based halide powder is obtained by grinding solid materials of AX and CuX, where A represents an alkali metal element and X represents a halogen element.

[0070] Optionally, the molar ratio of AX to CuX may be 0.5: 1 to 1.7: 1. Preferably, the molar ratio of AX to CuX may be 3:2.

[0071] Optionally, the chemical composition of the copper-based halide powder may include but is not limited to at least one of the following: Cs3Cu2I5, Cs3Cu2Br5, Cs3Cu2Cl5, CsCu2I3, Cs5Cu3I8, Cs5Cu3Cl6I2, etc.

[0072] Optionally, grinding can be achieved by a ball mill using a grinding method. The grinding method can include dry grinding and wet grinding. The grinding time can be 3 to 12 hours. The grinding speed can be 500 to 2000 r / min. For example, the raw materials AX, CuX and agate balls can be placed in a ball mill, and the raw materials can be ground by a ball mill (including dry grinding and wet grinding) to obtain a copper-based halide powder.

[0073] According to an embodiment of the present invention, the copper-based scintillator powder doped with manganese ions is obtained by grinding solid materials of AX, CuX and MnX2.

[0074] Optionally, the molar ratio of MnX2 to the copper-based halide powder may be in the range of 0.001% to 100%.

[0075] For example, raw materials AX, CuX and a certain proportion of MnX2 solid powder and agate balls are placed in a ball mill, and the raw materials are ground by dry grinding or wet grinding to obtain copper-based scintillator powder doped with manganese ions.

[0076] According to an embodiment of the present invention, Mn is doped 2+ The emission wavelength of the copper-based scintillator crystal has an obvious red shift, which can red-shift the emission wavelength from 450 nm to 550 nm and maintain a high light yield.

[0077] According to an embodiment of the present invention, the heating mentioned in operations S1 and S2 can be implemented in a muffle furnace. For example, the microporous template and the copper-based scintillator powder or the copper-based scintillator powder doped with manganese ions can be placed in a muffle furnace, the copper-based scintillator powder or the copper-based scintillator powder doped with manganese ions can be covered on the microporous template, and the scintillator powder is heated so that it reaches a molten state and is filled into the microporous template; after a slow cooling process, the molten copper-based scintillator powder or the copper-based scintillator powder doped with manganese ions can form crystals in the microporous template.

[0078] Optionally, the heating temperature may be 300°C to 1000°C, for example but not limited to: 300°C, 400°C, 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C.

[0079] According to an embodiment of the present invention, the cooling rate mentioned in operations S1 and S2 can be 1°C / h~400°C / h, for example, but not limited to: 1°C / h, 50°C / h, 100°C / h, 150°C / h, 200°C / h, 250°C / h, 300°C / h, 350°C / h, 400°C / h.

[0080] According to an embodiment of the present invention, the coupling mentioned in operation S3 may be coupling by means of optical adhesive. Optionally, the optical adhesive may include but is not limited to at least one of the following: epoxy resin, silicone oil, acrylate optical adhesive, silicone optical adhesive, etc.

[0081] According to the embodiment of the present invention, the two scintillator crystals prepared by the melting method have excellent light transmittance, which can improve the photon extraction rate. In addition, the preparation process of the melting method allows the doping ions to be better and more uniformly doped into the lattice, which is unmatched by other preparation methods.

[0082] According to another embodiment of the present invention, before operation S3, the operation may also be included: cutting, polishing, and grinding the copper-based scintillator crystal layer obtained by operation S1 and the copper-based scintillator crystal layer doped with manganese ions obtained by operation S2 to obtain a copper-based scintillator crystal layer and a copper-based scintillator crystal layer doped with manganese ions of a certain thickness, respectively.

[0083] According to yet another embodiment of the present invention, the method for preparing a copper-based scintillator-microporous template may further include operations S4 to S5 in addition to the above operations S1 to S2.

[0084] In operation S4, polydimethylsiloxane is poured into the microporous template and cured to form an X-ray hardening layer.

[0085] In operation S5 , the copper-based scintillator crystal layer, the X-ray hardening layer, and the copper-based scintillator crystal layer doped with manganese ions are sequentially stacked and coupled to obtain a copper-based scintillator-microporous template.

[0086] According to the embodiment of the present invention, the coupling manner in operation S5 is similar to that in the above operation S3, and will not be described in detail herein.

[0087] Based on the dual-energy X-ray detector based on the copper-based scintillator-microporous template provided by the present invention, the present invention also provides a method for preparing a dual-energy X-ray detector based on the copper-based scintillator-microporous template, which may include the following operations: coupling the copper-based scintillator-microporous template with a visible light detector to obtain a dual-energy X-ray detector.

[0088] According to an embodiment of the present invention, the copper-based scintillator-microporous template may be obtained according to the above-mentioned method for preparing the copper-based scintillator-microporous template, or may be the above-mentioned copper-based scintillator-microporous template 100. The visible light detector is located below the copper-based scintillator crystal.

[0089] For example, one side of the copper-based scintillator crystal of the copper-based scintillator-microporous template is superimposed on a visible light detector, and a dual-energy X-ray detector is formed through optical glue coupling.

[0090] According to an embodiment of the present invention, the method for preparing a dual-energy X-ray detector based on a copper-based scintillator-microporous template may also include the operation of: encapsulating the surface of the copper-based scintillator-microporous template that is not in contact with the visible light detector with optical glue to obtain a dual-energy X-ray detector.

[0091] According to the embodiment of the present invention, the optical adhesive encapsulates the non-contact surface of the copper-based scintillator-microporous template and the visible light detector, which can protect the two layers of scintillator crystals and extend the service life.

[0092] The copper-based scintillator-microporous template, dual-energy X-ray detector and preparation method are described below by more specific examples. It should be noted that the examples are only specific embodiments of the present invention and cannot limit the protection scope of the present invention.

[0093] Embodiment 1:

[0094] S11, placing the raw materials CsI and CuI in a ball mill according to a molar ratio of 3:2 with agate balls, and grinding the raw materials by dry grinding to obtain copper-based scintillator powder (Cs3Cu2I5), with a ball milling speed of 1000 r / min and a ball milling time of 10 h;

[0095] S12, placing raw materials CsI, CuI, MnCl2 in a ratio of 3:2:0.15 and agate balls in a ball mill, grinding the raw materials by dry grinding or wet grinding to obtain manganese ion-doped copper-based scintillator powder (Cs3Cu2I5:15%Mn 2+ ), ball milling speed 1000 r / min, ball milling time 10h;

[0096] S13, placing an anodized aluminum microporous template with a thickness of 200 μm and a copper-based scintillator powder and a copper-based scintillator powder doped with manganese ions in a muffle furnace, respectively, with the copper-based scintillator powder and the copper-based scintillator powder doped with manganese ions both covering the microporous template, heating to 400°C, and keeping the temperature for 5 hours so that the two scintillator powders reach a molten state and are filled into the anodized aluminum microporous template; after a slow cooling process of 20°C / min, the molten scintillator powder is able to form high-quality crystals in the microporous template, and a copper-based scintillator crystal layer and a manganese-ion-doped copper-based scintillator crystal layer are obtained respectively;

[0097] S14, cutting, polishing and grinding the copper-based scintillator crystal layer and the manganese ion-doped copper-based scintillator crystal layer respectively to obtain a flat and smooth copper-based scintillator crystal layer and a manganese ion-doped copper-based scintillator crystal layer of a certain thickness;

[0098] S15, pouring polydimethylsiloxane (liquid PDMS) into an anodized aluminum microporous template with a thickness of 500 μm, and curing it at room temperature for 12 hours to form an X-ray hardening layer;

[0099] S16, sequentially stacking a copper-based scintillator crystal layer, an X-ray hardening layer, a manganese ion-doped copper-based scintillator crystal layer, and a flat-panel visible light detector and coupling them through optical glue to form a dual-energy X-ray flat-panel detector;

[0100] S17, encapsulate the dual-energy X-ray flat panel detector using optical adhesive.

[0101] Figure 4 The radiation luminescence intensity of the copper-based scintillator powder prepared in Example 1 of the present invention and the copper-based scintillator powder doped with manganese ions under X-rays is shown.

[0102] like Figure 4 As shown, after doping with manganese ions, the luminescence wavelength is red-shifted from about 450nm to about 550nm, which not only meets the requirements for preparing dual-energy X-ray detectors, but also maintains the copper-based scintillator powder with high light yield, no self-absorption and a small luminescence half-width.

[0103] Comparative Example 1:

[0104] S21, placing the raw materials CsI and CuI in a ball mill according to a molar ratio of 3:2 with agate balls, and grinding the raw materials by dry grinding to obtain copper-based scintillator powder (Cs3Cu2I5), with a ball milling speed of 1000 r / min and a ball milling time of 10 h;

[0105] S22, placing raw materials CsI, CuI, and MnCl2 in a ratio of 3:2:0.15 and agate balls in a ball mill, grinding the raw materials by dry grinding or wet grinding to obtain manganese ion-doped copper-based scintillator powder (Cs3Cu2I5:15%Mn 2+ ), ball milling speed 1000 r / min, ball milling time 10h;

[0106] S23, placing the copper-based scintillator powder and the copper-based scintillator powder doped with manganese ions in a muffle furnace, heating them to 400° C., and keeping them warm for 5 hours so that the two scintillator powders reach a molten state; after a slow cooling process at 20° C. / min, the molten scintillator powder is able to form high-quality crystals, and a copper-based scintillator crystal layer without a microporous template and a copper-based scintillator crystal layer doped with manganese ions without a microporous template are obtained respectively;

[0107] S24, cutting, polishing and grinding the copper-based scintillator crystal layer without microporous template and the copper-based scintillator crystal layer doped with manganese ions without microporous template respectively to obtain a flat and smooth copper-based scintillator crystal layer without microporous template and a copper-based scintillator crystal layer doped with manganese ions without microporous template of a certain thickness;

[0108] S25, curing polydimethylsiloxane (liquid PDMS) at room temperature for 12 hours to form an X-ray hardened layer with a thickness of 500 μm without a microporous template;

[0109] S26, sequentially stacking a copper-based scintillator crystal layer without a microporous template, an X-ray hardening layer without a microporous template, a copper-based scintillator crystal layer doped with manganese ions without a microporous template, and a flat-panel visible light detector, and coupling them through optical glue to form a dual-energy X-ray flat-panel detector without a microporous template;

[0110] S27, encapsulating the dual-energy X-ray flat panel detector without microporous template using optical adhesive.

[0111] Figure 5 The imaging image of the dual-energy X-ray flat panel detector without microporous template prepared in Comparative Example 1 of the present invention on the line pair card is shown; Figure 6 The imaging image of the dual-energy X-ray flat panel detector prepared in Example 1 of the present invention for line pair and card pair is shown.

[0112] From above Figure 5 and Figure 6From the clarity of the imaging image shown, it can be seen that the dual-energy X-ray flat-panel detector prepared in Example 1 of the present invention has clearer imaging of the line pair card, which can prove that the dual-energy X-ray flat-panel detector provided by the present invention, by introducing a micropore template, the photons of the dual-energy X-ray flat-panel detector will be confined to the vertical micropore channels, thereby reducing the lateral propagation of photons and improving the spatial resolution.

[0113] Embodiment 2:

[0114] S31, placing the raw materials CsI and CuI in a ball mill according to a molar ratio of 3:2 with agate balls, and grinding the raw materials by dry grinding to obtain copper-based scintillator powder Cs3Cu2I5, with a ball milling speed of 1000 r / min and a ball milling time of 10 h;

[0115] S32, placing the raw materials CsI, CuI, and MnCl2 in a ratio of 3:2:0.15 and agate balls in a ball mill, and grinding the raw materials by dry grinding or wet grinding to obtain manganese ion-doped copper-based scintillator powder Cs3Cu2I5:15%Mn 2+ , ball milling speed 1000 r / min, ball milling time 10h;

[0116] S33, heating the copper-based scintillator powder doped with manganese ions to 400°C in a muffle furnace, keeping the temperature for 5 hours to make the scintillator powder reach a molten state, and then slowly cooling the temperature at a rate of 20°C / min to obtain Cs3Cu2I5:15%Mn prepared by the melting method. 2+ Crystal.

[0117] Figure 7 The Cs3Cu2I5 prepared by Example 2 of the present invention and the Cs3Cu2I5:15%Mn prepared by ball milling are shown. 2+ And Cs3Cu2I5:15%Mn prepared by melting method 2+ The luminous intensity of radiation under X-rays.

[0118] like Figure 7 As shown, Cs3Cu2I5:15%Mn prepared by ball milling 2+ Compared with Cs3Cu2I5:15%Mn prepared by melting method 2+ The radiation luminescence intensity is weak, and the Cs3Cu2I5:15%Mn prepared by the melting method 2+ Compared with Cs3Cu2I5 and Cs3Cu2I5:15%Mn prepared by ball milling 2+ , all of which have undergone red shift. It can be seen that during the ball milling process, CsI and CuI can form Cs3Cu2I5 scintillator, but Mn 2+It is difficult for Mn to enter the Cs3Cu2I5 lattice in the solid phase reaction, resulting in the scintillator prepared by solid phase reaction such as ball milling method still mainly composed of Cs3Cu2I5 and free Mn 2+ However, in the melting process, all substances exist in the form of ions in the molten state, and can achieve ideal self-assembly during the crystallization process, thus forming a uniformly doped Cs3Cu2I5:15%Mn 2+ .

[0119] According to the embodiments of the present invention, the melting method used in the present invention can achieve more uniform doping compared to solid phase reaction methods such as ball milling, and can even complete ion doping that cannot be achieved by solid phase reaction.

[0120] It will be appreciated by those skilled in the art that the features described in the various embodiments of the present invention may be combined and / or combined in various ways, even if such combinations or combinations are not explicitly described in the present invention. In particular, without departing from the spirit and teachings of the present invention, the features described in the various embodiments of the present invention may be combined and / or combined in various ways. All of these combinations and / or combinations fall within the scope of the present invention.

[0121] The embodiments of the present invention are described above. However, these embodiments are only for the purpose of illustration, and are not intended to limit the scope of the present invention. Although each embodiment is described above, it does not mean that the measures in each embodiment cannot be used in combination. The scope of the present invention is defined by the attached claims and their equivalents. Without departing from the scope of the present invention, those skilled in the art may make various substitutions and modifications, which should all fall within the scope of the present invention.

Claims

1. A dual-energy X-ray detector based on a copper-based scintillator-microporous template, characterized in that: The dual-energy X-ray detector comprises: a copper-based scintillator-microporous template and a visible light detector; Wherein, the copper-based scintillator-microporous template comprises: a microporous template, a copper-based scintillator crystal, and a copper-based scintillator crystal doped with manganese ions; Wherein, the microporous template comprises a plurality of evenly distributed holes, and the plurality of holes are used to fill the copper-based scintillator crystals and the copper-based scintillator crystals doped with manganese ions, and the holes of each of the holes after filling are the same; The copper-based scintillator-microporous template is obtained by the following operations: The copper-based halide powder covering the microporous template is heated to make the copper-based halide powder reach a molten state and fill the microporous template, and the temperature is lowered to make the molten copper-based halide powder form crystals in the microporous template to obtain a copper-based scintillator crystal layer, wherein the copper-based halide powder is obtained by grinding solid materials of AX and CuX, A represents an alkali metal element, and X represents a halogen element; The copper-based halide powder doped with manganese ions covering the microporous template is heated to make the copper-based halide powder doped with manganese ions reach a molten state and fill the microporous template, and the temperature is lowered to make the molten copper-based halide powder doped with manganese ions form crystals in the microporous template to obtain a copper-based scintillator crystal layer doped with manganese ions, wherein the copper-based halide powder doped with manganese ions is obtained by grinding solid materials of AX, CuX and MnX2; coupling the copper-based scintillator crystal layer with the copper-based scintillator crystal layer doped with manganese ions to obtain the copper-based scintillator-microporous template; The visible light detector is in contact with the copper-based scintillator-microporous template. The visible light detector is located below the copper-based scintillator crystal and is used to detect and convert visible light photons generated when X-ray photons interact with the copper-based scintillator crystal or the manganese ion-doped copper-based scintillator crystal into electrical signals.

2. The dual-energy X-ray detector according to claim 1, characterized in that: The copper-based scintillator-microporous template also includes an X-ray hardening layer; The X-ray hardening layer is located between the copper-based scintillator crystal and the manganese ion-doped copper-based scintillator crystal, and is used to separate the X-rays absorbed by the copper-based scintillator crystal and the manganese ion-doped copper-based scintillator crystal.

3. The dual-energy X-ray detector according to claim 2, characterized in that: The height of the X-ray hardening layer is 500 μm to 2 mm, and the X-ray hardening layer is prepared based on polydimethylsiloxane.

4. The dual-energy X-ray detector according to any one of claims 1 to 3, characterized in that: The diameter of each of the plurality of holes is 500nm~100μm, the height of each of the plurality of holes is 10μm~10mm, and the microporous template includes at least one of the following: anodized aluminum, aluminum capillary, silicon, silicon oxide.

5. The dual-energy X-ray detector according to claim 1, characterized in that: The dual-energy X-ray detector further includes a packaging layer; Wherein, the encapsulation layer is used to encapsulate the surface of the copper-based scintillator-microporous template that is not in contact with the visible light detector.

6. The dual-energy X-ray detector according to claim 1, characterized in that: The copper-based scintillator-microporous template is also obtained by the following operations: pouring polydimethylsiloxane into the microporous template and curing it to form an X-ray hardening layer; The copper-based scintillator crystal layer, the X-ray hardening layer and the copper-based scintillator crystal layer doped with manganese ions are sequentially stacked and coupled to obtain the copper-based scintillator-microporous template.

7. A method for preparing a dual-energy X-ray detector based on a copper-based scintillator-microporous template, characterized in that: The method comprises: A dual-energy X-ray detector is obtained by coupling a copper-based scintillator-microporous template with a visible light detector, wherein the copper-based scintillator-microporous template comprises: a microporous template, a copper-based scintillator crystal, and a copper-based scintillator crystal doped with manganese ions; Wherein, the microporous template comprises a plurality of evenly distributed holes, and the plurality of holes are used to fill the copper-based scintillator crystals and the copper-based scintillator crystals doped with manganese ions, and the holes of each of the holes after filling are the same; The copper-based scintillator-microporous template is obtained by the following operations: The copper-based halide powder covering the microporous template is heated to make the copper-based halide powder reach a molten state and fill the microporous template, and the temperature is lowered to make the molten copper-based halide powder form crystals in the microporous template to obtain a copper-based scintillator crystal layer, wherein the copper-based halide powder is obtained by grinding solid materials of AX and CuX, A represents an alkali metal element, and X represents a halogen element; The copper-based halide powder doped with manganese ions covering the microporous template is heated to make the copper-based halide powder doped with manganese ions reach a molten state and fill the microporous template, and the temperature is lowered to make the molten copper-based halide powder doped with manganese ions form crystals in the microporous template to obtain a copper-based scintillator crystal layer doped with manganese ions, wherein the copper-based halide powder doped with manganese ions is obtained by grinding solid materials of AX, CuX and MnX2; coupling the copper-based scintillator crystal layer with the copper-based scintillator crystal layer doped with manganese ions to obtain the copper-based scintillator-microporous template; The visible light detector is located below the copper-based scintillator crystal.

8. The method according to claim 7, characterized in that The method further comprises: The copper-based scintillator-microporous template and the surface not in contact with the visible light detector are packaged with optical glue to obtain the dual-energy X-ray detector.

Citation Information

Patent Citations

  • Manganese-doped Cs3Cu2I5 halide scintillator with high light yield

    CN111778017A

  • Disclosed are ray detector substrate and ray detector

    CN112117290A

  • Method for preparing lead-free perovskite pixelated scintillation film

    CN115636434A