Heat-resistant and salt-resistant polymer microsphere and preparation method thereof

The temperature-resistant and salt-resistant polymer microspheres prepared by silica compounding technology of different particle sizes solve the problem of unstable polymer microspheres under high temperature and high salt conditions, and realize the heat resistance and salt resistance of polymer microspheres. Improved performance and improved oilfield recovery.

CN118580443BActive Publication Date: 2024-11-29SUZHOU CHUXIN MOYI TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411067435.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-29
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The existing polymer microspheres are unstable under high temperature and high salt conditions, resulting in low water injection and mining efficiency in oil fields and it is difficult to effectively seal the micropores of the formation.

Method used

Using the silicon dioxide composite technology of different particle sizes, the temperature-resistant and salt-resistant resistance is prepared by dispersing small-particle and large-particle silicon dioxide particles and acrylamide, acrylic acid, N-methylenebisacrylamide and other materials. Polymer microspheres form multi-core structures to enhance the heat and salt resistance of the material.

Benefits of technology

It significantly improves the heat resistance and salt resistance of polymer microspheres, enhances its stability and sealing ability under high temperature and high salt conditions, can effectively enter the formation micropores and achieve dynamic sealing, and improves oil field recovery Rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118580443B_ABST
    Figure CN118580443B_ABST
Patent Text Reader

Abstract

The invention discloses a heat-resistant and salt-resistant polymer microsphere and a preparation method thereof, and belongs to the technical field of organic-inorganic composite materials. With acrylamide, acrylic acid, N, N-methylenebisacrylamide as reaction monomers and crosslinking agents, and silica of different particle sizes as reinforcing materials, the heat-resistant and salt-resistant polymer microspheres are prepared by dispersion polymerization. Compared with conventional inverse emulsion polymerization, it has the advantages of simple operation, mild reaction conditions, short reaction time, and stable reaction process. The use of silica of different particle sizes can effectively disperse stress, and the small-particle silica, large-particle silica and polymer matrix are cross-linked with each other, which can play a toughening role while playing the role of inorganic material reinforcement, and can significantly improve the heat resistance and salt resistance of the microspheres.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic-inorganic composite materials, and in particular relates to a temperature-resistant and salt-resistant polymer microsphere and a preparation method thereof. Background Art

[0002] With the rapid development of the global economy, the demand for crude oil in countries around the world is increasing. However, most of the old oil fields that have been developed to the late stage have gradually entered the high water content development stage due to long-term water injection and exploitation, and generally show serious water problems. In addition, long-term water flow scouring has greatly aggravated the heterogeneity of the reservoir, causing the injected water to break through the single layer in the formation, resulting in water cones, water channeling, fingering and other phenomena, greatly reducing the scope of water flow, greatly reducing the efficiency of water injection and exploitation, and the effectiveness of various displacement agents cannot be exerted. Therefore, it is very important to use profile adjustment and water plugging technology to block high-permeability formations, so that the injected water can be transferred to the unaffected area to displace the remaining oil, thereby improving the water drive recovery effect.

[0003] Among them, although polymer flooding has been widely used in tertiary oil recovery in major oil fields, there are also problems in the process of implementing polymer flooding in oil fields at this stage, such as instability under high temperature and high salt conditions in the formation. In recent years, in order to solve this problem, more and more companies have begun to turn their attention to the application of organic / inorganic composite materials in improving oil recovery. When inorganic particles are dispersed in polymer solutions, not only the rheological properties of the polymer solution are enhanced and the sweep efficiency is improved, but also the polymer / inorganic particle composite material exhibits good thermal stability and salt resistance. Among inorganic materials, silica has the characteristics of good thermal stability, low price, and environmental friendliness, and has gradually become an ideal material for application in the field of oil field improvement. In existing research, there are more studies on nanoparticles, and fewer studies on silica materials with different particle sizes. Compared with single nano-silicon dioxide, the composite of silica with different particle sizes has low surface activity and is not easy to agglomerate, and has the advantages of low cost and environmental protection. Summary of the invention

[0004] In order to solve the technical problems of low temperature and salt resistance and poor mechanical properties of polymer microspheres in the prior art, the present invention provides a heat-resistant and salt-resistant polymer microsphere and a preparation method thereof. The polymer microsphere can still play an excellent deep flooding effect under high temperature and high mineralization conditions.

[0005] The purpose of the present invention is achieved through the following technical solutions.

[0006] The first aspect of the present invention provides a method for preparing temperature-resistant and salt-resistant polymer microspheres, comprising the following steps:

[0007] (1) Weighing 0.1-0.2 parts of small-size silica particles and 1-2 parts of large-size silica particles respectively, dispersing them in a solvent, then adding 1-3 parts of a double-bond silane coupling agent, stirring for reaction, and post-treating to obtain mixed modified silica particles; wherein the small-size silica particles have a volume D50 of 10-20 nm as measured by laser scattering; and the large-size silica particles have a volume D50 of 70-300 nm as measured by laser scattering;

[0008] (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 1-4 parts of a surfactant, 8-16 parts of acrylamide, 8-16 parts of acrylic acid, 1-2 parts of N,N-methylenebisacrylamide, and 0.1-0.5 parts of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 55-75°C for 3-6 hours to obtain a mixed solution;

[0009] (3) The mixed solution is centrifuged, washed, and dried to obtain temperature-resistant and salt-resistant polymer microspheres.

[0010] The present invention uses acrylamide, acrylic acid, N, N-methylenebisacrylamide as reaction monomers and crosslinking agents, and silica of different particle sizes as reinforcing materials, and adopts a dispersion polymerization method to prepare heat-resistant and salt-resistant polymer microspheres. Compared with conventional reverse emulsion polymerization, it has the advantages of simple operation, mild reaction conditions, short reaction time, stable reaction process and uniform particle size. The prior art usually directly uses nano-silicon dioxide of a single particle size as the core. Although the performance of the composite microspheres is improved to a certain extent, in today's increasingly harsh oil reservoir environment, due to the influence of high temperature, high salt and high shear conditions, conventional chemical cross-linked silica-polymer microspheres are prone to degradation, fragmentation, flocculation and other problems and lose their plugging ability. The present invention uses silica of different particle sizes to effectively disperse stress, and compositely modify the polymer, which can play the role of inorganic material reinforcement while also serving the purpose of toughening, and can significantly improve the heat resistance and salt resistance of the material. The present invention adds a large amount of large-particle silica, supplemented by a small amount of small-particle silica. During the polymerization process, the addition of a small amount of small-particle silica improves the dispersion of silica in the organism, and can be evenly dispersed in the polymer matrix to play the role of inorganic filler, increase the stress required for the microsphere body to deform under force, enhance the viscoelasticity of the system, and can more easily enter the micropores of the formation under the action of the displacement pressure difference and achieve dynamic plugging.

[0011] Furthermore, in step (1), the solvent is a mixed solution of ethanol and water.

[0012] Furthermore, the double bond-containing silane coupling agent in step (1) is at least one of vinyl triethoxysilane, 3-(isobutyl acrylate) propyl trimethoxysilane, vinyl trimethoxysilane, and vinyl tri(β-methoxyethoxy) silane; and the large-size silica particles have a volume D50 of 100-200 nm as measured by laser scattering.

[0013] Furthermore, in step (1), the stirring rate is 400-700 r / min and the reaction temperature is 40-60°C.

[0014] Furthermore, the post-treatment in step (1) is a centrifugation, washing and drying process.

[0015] Furthermore, in step (2), the solvent is a mixed solution of ethanol and ethyl acetate.

[0016] Furthermore, in step (2), the surfactant is polyvinyl pyrrolidone.

[0017] Furthermore, in step (2), the initiator is azobisisobutyronitrile.

[0018] Furthermore, in step (2), the inert gas is nitrogen.

[0019] The second aspect of the present invention also provides a temperature-resistant and salt-resistant polymer microsphere.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention uses acrylamide, acrylic acid, N, N-methylenebisacrylamide as reaction monomers and crosslinking agents, and silica of different particle sizes as reinforcing materials, and adopts a dispersion polymerization method to prepare heat-resistant and salt-resistant polymer microspheres. The obtained composite microspheres have an average particle size of 2-4um, a uniform particle size, and have the advantages of simple operation, mild reaction conditions, and short reaction time. The use of silica of different particle sizes can effectively disperse stress and carry out composite modification on the polymer, which can play the role of strengthening inorganic materials while also achieving the purpose of toughening, and can significantly improve the heat resistance of the material. Small-particle silica, large-particle silica and polymer matrix are crosslinked with each other, which limits the movement of polymer chains, has strong deformation recovery ability and the ability to resist erosion and damage, can more easily enter the formation micropores under the action of displacement pressure difference, and realize dynamic plugging. Due to the excellent mechanical properties and temperature and salt resistance of the microspheres, they have good migration capabilities for oil reservoirs with different permeability. They can continuously migrate to deep formations and form a dynamic plugging process of "plugging, migration, re-plugging, and re-migration". BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a scanning electron microscope image of the temperature-resistant and salt-resistant polymer microspheres of Example 9;

[0023] Figure 2 This is a transmission electron micrograph of the temperature-resistant and salt-resistant polymer microspheres of Example 9. DETAILED DESCRIPTION

[0024] In order to more clearly understand the purpose, technical solutions and advantages of the present invention, the present invention is further described in detail below in conjunction with embodiments.

[0025] Example 1

[0026] A method for preparing temperature-resistant and salt-resistant polymer microspheres comprises the following steps:

[0027] (1) Weighing 0.1 parts of small-size silica particles and 1 part of large-size silica particles respectively, dispersing them in a solvent, then adding 1 part of a double-bond silane coupling agent, stirring for reaction, and post-treating to obtain mixed modified silica particles; wherein the small-size silica particles have a volume D50 of 10 nm as measured by laser scattering; and the large-size silica particles have a volume D50 of 100 nm as measured by laser scattering;

[0028] (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 1 part of a surfactant, 8 parts of acrylamide, 8 parts of acrylic acid, 1 part of N,N-methylenebisacrylamide, and 0.1 part of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 55°C for 6 hours to obtain a mixed solution;

[0029] (3) centrifuging the mixed solution, washing, and drying to obtain temperature-resistant and salt-resistant polymer microspheres;

[0030] Wherein, the solvent in step (1) is a mixed solution of ethanol and water. The double-bond silane coupling agent is vinyl triethoxysilane. The stirring rate is 400 r / min, and the reaction temperature is 40° C. The post-treatment is a centrifugation, washing and drying process.

[0031] In step (2), the solvent is a mixed solution of ethanol and ethyl acetate. The surfactant is polyvinyl pyrrolidone. The initiator is azobisisobutyronitrile. The inert gas is nitrogen.

[0032] Example 2

[0033] A method for preparing temperature-resistant and salt-resistant polymer microspheres comprises the following steps:

[0034] (1) Weighing 0.2 parts of small-size silica particles and 2 parts of large-size silica particles respectively, dispersing them in a solvent, then adding 3 parts of a double-bond silane coupling agent, stirring for reaction, and post-treating to obtain mixed modified silica particles; wherein the small-size silica particles have a volume D50 of 20 nm as measured by laser scattering; and the large-size silica particles have a volume D50 of 200 nm as measured by laser scattering;

[0035] (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 4 parts of a surfactant, 16 parts of acrylamide, 16 parts of acrylic acid, 2 parts of N,N-methylenebisacrylamide, and 0.5 parts of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 75°C for 3 hours to obtain a mixed solution;

[0036] (3) The mixed solution is centrifuged, washed, and dried to obtain temperature-resistant and salt-resistant polymer microspheres.

[0037] Wherein, the solvent in step (1) is a mixed solution of ethanol and water. The double-bond silane coupling agent is 3-(isobutyleneoxy)propyltrimethoxysilane. The stirring rate is 700 r / min, and the reaction temperature is 60°C. The post-treatment is a centrifugation, washing and drying process.

[0038] In step (2), the solvent is a mixed solution of ethanol and ethyl acetate. The surfactant is polyvinyl pyrrolidone. The initiator is azobisisobutyronitrile. The inert gas is nitrogen.

[0039] Example 3

[0040] A method for preparing temperature-resistant and salt-resistant polymer microspheres comprises the following steps:

[0041] (1) Weighing 0.1 parts of small-size silica particles and 2 parts of large-size silica particles respectively, dispersing them in a solvent, then adding 1.4 parts of a double-bond silane coupling agent, stirring for reaction, and post-treating to obtain mixed modified silica particles; wherein the small-size silica particles have a volume D50 of 10 nm as measured by laser scattering; and the large-size silica particles have a volume D50 of 200 nm as measured by laser scattering;

[0042] (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 2 parts of a surfactant, 10 parts of acrylamide, 9 parts of acrylic acid, 1.2 parts of N,N-methylenebisacrylamide, and 0.25 parts of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 65°C for 4 hours to obtain a mixed solution;

[0043] (3) The mixed solution is centrifuged, washed, and dried to obtain temperature-resistant and salt-resistant polymer microspheres.

[0044] Wherein, the solvent in step (1) is a mixed solution of ethanol and water. The double-bond silane coupling agent is vinyltrimethoxysilane. The stirring rate is 600 r / min, and the reaction temperature is 55° C. The post-treatment is a centrifugation, washing and drying process.

[0045] In step (2), the solvent is a mixed solution of ethanol and ethyl acetate. The surfactant is polyvinyl pyrrolidone. The initiator is azobisisobutyronitrile. The inert gas is nitrogen.

[0046] Example 4

[0047] A method for preparing temperature-resistant and salt-resistant polymer microspheres comprises the following steps:

[0048] (1) Weighing 0.2 parts of small-size silica particles and 1 part of large-size silica particles respectively, dispersing them in a solvent, then adding 2.8 parts of a double-bond silane coupling agent, stirring for reaction, and post-treating to obtain mixed modified silica particles; wherein the small-size silica particles have a volume D50 of 20 nm as measured by laser scattering; and the large-size silica particles have a volume D50 of 100 nm as measured by laser scattering;

[0049] (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 3 parts of a surfactant, 15 parts of acrylamide, 11 parts of acrylic acid, 1.8 parts of N,N-methylenebisacrylamide, and 0.38 parts of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 72°C for 4 hours to obtain a mixed solution;

[0050] (3) The mixed solution is centrifuged, washed, and dried to obtain temperature-resistant and salt-resistant polymer microspheres.

[0051] Wherein, the solvent in step (1) is a mixed solution of ethanol and water. The double-bond silane coupling agent is vinyl tris(β-methoxyethoxy)silane. The stirring rate is 500 r / min, and the reaction temperature is 50° C. The post-treatment is a centrifugation, washing and drying process.

[0052] In step (2), the solvent is a mixed solution of ethanol and ethyl acetate. The surfactant is polyvinyl pyrrolidone. The initiator is azobisisobutyronitrile. The inert gas is nitrogen.

[0053] Example 5

[0054] A method for preparing temperature-resistant and salt-resistant polymer microspheres comprises the following steps:

[0055] (1) Weighing 0.12 parts of small-size silica particles and 1.1 parts of large-size silica particles respectively, dispersing them in a solvent, then adding 1.4 parts of a double-bond silane coupling agent, stirring for reaction, and post-treating to obtain mixed modified silica particles; wherein the small-size silica particles have a volume D50 of 12 nm as measured by laser scattering; and the large-size silica particles have a volume D50 of 130 nm as measured by laser scattering;

[0056] (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 2 parts of a surfactant, 10 parts of acrylamide, 14 parts of acrylic acid, 1.6 parts of N,N-methylenebisacrylamide, and 0.27 parts of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 66°C for 5.5 hours to obtain a mixed solution;

[0057] (3) The mixed solution is centrifuged, washed, and dried to obtain temperature-resistant and salt-resistant polymer microspheres.

[0058] Wherein, the solvent in step (1) is a mixed solution of ethanol and water. The double-bond silane coupling agent is 3-(isobutyleneoxy)propyltrimethoxysilane. The stirring rate is 650 r / min, and the reaction temperature is 50° C. The post-treatment is a centrifugation, washing and drying process.

[0059] In step (2), the solvent is a mixed solution of ethanol and ethyl acetate. The surfactant is polyvinyl pyrrolidone. The initiator is azobisisobutyronitrile. The inert gas is nitrogen.

[0060] Example 6

[0061] A method for preparing temperature-resistant and salt-resistant polymer microspheres comprises the following steps:

[0062] (1) Weighing 0.19 parts of small-size silica particles and 1.8 parts of large-size silica particles respectively, dispersing them in a solvent, then adding 2.7 parts of a double-bond silane coupling agent, stirring for reaction, and post-treating to obtain mixed modified silica particles; wherein the small-size silica particles have a volume D50 of 17 nm as measured by laser scattering; and the large-size silica particles have a volume D50 of 190 nm as measured by laser scattering;

[0063] (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 2.5 parts of a surfactant, 14 parts of acrylamide, 9 parts of acrylic acid, 1.4 parts of N,N-methylenebisacrylamide, and 0.34 parts of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 68°C for 5 hours to obtain a mixed solution;

[0064] (3) The mixed solution is centrifuged, washed, and dried to obtain temperature-resistant and salt-resistant polymer microspheres.

[0065] Wherein, the solvent in step (1) is a mixed solution of ethanol and water. The double-bond silane coupling agent is vinyl triethoxysilane. The stirring rate is 500 r / min, and the reaction temperature is 52° C. The post-treatment is a centrifugation, washing and drying process.

[0066] In step (2), the solvent is a mixed solution of ethanol and ethyl acetate. The surfactant is polyvinyl pyrrolidone. The initiator is azobisisobutyronitrile. The inert gas is nitrogen.

[0067] Example 7

[0068] A method for preparing temperature-resistant and salt-resistant polymer microspheres comprises the following steps:

[0069] (1) Weighing 0.15 parts of small-size silica particles and 1.5 parts of large-size silica particles respectively, dispersing them in a solvent, then adding 2 parts of a double-bond silane coupling agent, stirring for reaction, and post-treating to obtain mixed modified silica particles; wherein the small-size silica particles have a volume D50 of 15 nm as measured by laser scattering; and the large-size silica particles have a volume D50 of 70 nm as measured by laser scattering;

[0070] (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 3 parts of a surfactant, 12 parts of acrylamide, 12 parts of acrylic acid, 1.5 parts of N,N-methylenebisacrylamide, and 0.25 parts of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 65°C for 5 hours to obtain a mixed solution;

[0071] (3) The mixed solution is centrifuged, washed, and dried to obtain temperature-resistant and salt-resistant polymer microspheres.

[0072] Wherein, the solvent in step (1) is a mixed solution of ethanol and water. The double-bond silane coupling agent is 3-(isobutyleneoxy)propyltrimethoxysilane. The stirring rate is 600 r / min, and the reaction temperature is 50° C. The post-treatment is a centrifugation, washing and drying process.

[0073] In step (2), the solvent is a mixed solution of ethanol and ethyl acetate. The surfactant is polyvinyl pyrrolidone. The initiator is azobisisobutyronitrile. The inert gas is nitrogen.

[0074] Example 8

[0075] A method for preparing temperature-resistant and salt-resistant polymer microspheres comprises the following steps:

[0076] (1) Weighing 0.15 parts of small-size silica particles and 1.5 parts of large-size silica particles respectively and dispersing them in a solvent, then adding 2 parts of a double-bond silane coupling agent, stirring for reaction, and post-treating to obtain mixed modified silica particles; wherein the small-size silica particles have a volume D50 of 15 nm as measured by laser scattering; and the large-size silica particles have a volume D50 of 300 nm as measured by laser scattering;

[0077] (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 3 parts of a surfactant, 12 parts of acrylamide, 12 parts of acrylic acid, 1.5 parts of N,N-methylenebisacrylamide, and 0.25 parts of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 65°C for 5 hours to obtain a mixed solution;

[0078] (3) The mixed solution is centrifuged, washed, and dried to obtain temperature-resistant and salt-resistant polymer microspheres.

[0079] Wherein, the solvent in step (1) is a mixed solution of ethanol and water. The double-bond silane coupling agent is 3-(isobutyleneoxy)propyltrimethoxysilane. The stirring rate is 600 r / min, and the reaction temperature is 50° C. The post-treatment is a centrifugation, washing and drying process.

[0080] In step (2), the solvent is a mixed solution of ethanol and ethyl acetate. The surfactant is polyvinyl pyrrolidone. The initiator is azobisisobutyronitrile. The inert gas is nitrogen.

[0081] Example 9

[0082] A method for preparing temperature-resistant and salt-resistant polymer microspheres comprises the following steps:

[0083] (1) Weighing 0.15 parts of small-size silica particles and 1.5 parts of large-size silica particles respectively, dispersing them in a solvent, then adding 2 parts of a double-bond silane coupling agent, stirring for reaction, and post-treating to obtain mixed modified silica particles; wherein the small-size silica particles have a volume D50 of 15 nm as measured by laser scattering; and the large-size silica particles have a volume D50 of 150 nm as measured by laser scattering;

[0084] (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 3 parts of a surfactant, 12 parts of acrylamide, 12 parts of acrylic acid, 1.5 parts of N,N-methylenebisacrylamide, and 0.25 parts of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 65°C for 5 hours to obtain a mixed solution;

[0085] (3) The mixed solution is centrifuged, washed, and dried to obtain temperature-resistant and salt-resistant polymer microspheres.

[0086] Wherein, the solvent in step (1) is a mixed solution of ethanol and water. The double-bond silane coupling agent is 3-(isobutyleneoxy)propyltrimethoxysilane. The stirring rate is 600 r / min, and the reaction temperature is 50° C. The post-treatment is a centrifugation, washing and drying process.

[0087] In step (2), the solvent is a mixed solution of ethanol and ethyl acetate. The surfactant is polyvinyl pyrrolidone. The initiator is azobisisobutyronitrile. The inert gas is nitrogen.

[0088] Comparative Example 1

[0089] A method for preparing temperature-resistant and salt-resistant polymer microspheres comprises the following steps:

[0090] (1) Weighing 1.65 parts of small-size silica particles and dispersing them in a solvent, then adding 2 parts of a double-bond silane coupling agent, stirring to react, and post-treating to obtain mixed modified silica particles; wherein the small-size silica particles have a volume D50 of 15 nm as measured by laser scattering;

[0091] (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 3 parts of a surfactant, 12 parts of acrylamide, 12 parts of acrylic acid, 1.5 parts of N,N-methylenebisacrylamide, and 0.25 parts of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 65°C for 5 hours to obtain a mixed solution;

[0092] (3) The mixed solution is centrifuged, washed, and dried to obtain temperature-resistant and salt-resistant polymer microspheres.

[0093] Wherein, the solvent in step (1) is a mixed solution of ethanol and water. The double-bond silane coupling agent is 3-(isobutyleneoxy)propyltrimethoxysilane. The stirring rate is 600 r / min, and the reaction temperature is 50° C. The post-treatment is a centrifugation, washing and drying process.

[0094] In step (2), the solvent is a mixed solution of ethanol and ethyl acetate. The surfactant is polyvinyl pyrrolidone. The initiator is azobisisobutyronitrile. The inert gas is nitrogen.

[0095] Comparative Example 2

[0096] A method for preparing temperature-resistant and salt-resistant polymer microspheres comprises the following steps:

[0097] (1) Weighing 1.65 parts of large-size silica particles and dispersing them in a solvent, then adding 2 parts of a double-bond silane coupling agent, stirring to react, and post-treating to obtain mixed modified silica particles; wherein the large-size silica particles have a volume D50 of 150 nm as measured by laser scattering;

[0098] (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 3 parts of a surfactant, 12 parts of acrylamide, 12 parts of acrylic acid, 1.5 parts of N,N-methylenebisacrylamide, and 0.25 parts of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 65°C for 5 hours to obtain a mixed solution;

[0099] (3) The mixed solution is centrifuged, washed, and dried to obtain temperature-resistant and salt-resistant polymer microspheres.

[0100] Wherein, the solvent in step (1) is a mixed solution of ethanol and water. The double-bond silane coupling agent is 3-(isobutyleneoxy)propyltrimethoxysilane. The stirring rate is 600 r / min, and the reaction temperature is 50° C. The post-treatment is a centrifugation, washing and drying process.

[0101] In step (2), the solvent is a mixed solution of ethanol and ethyl acetate. The surfactant is polyvinyl pyrrolidone. The initiator is azobisisobutyronitrile. The inert gas is nitrogen.

[0102] Comparative Example 3

[0103] A method for preparing temperature-resistant and salt-resistant polymer microspheres comprises the following steps:

[0104] (1) Weighing 0.15 parts of small-size silica particles and 1.5 parts of large-size silica particles respectively and dispersing them in a solvent, then adding 2 parts of a double-bond silane coupling agent, stirring for reaction, and post-treating to obtain mixed modified silica particles; wherein the small-size silica particles have a volume D50 of 5 nm as measured by laser scattering; and the large-size silica particles have a volume D50 of 150 nm as measured by laser scattering;

[0105] (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 3 parts of a surfactant, 12 parts of acrylamide, 12 parts of acrylic acid, 1.5 parts of N,N-methylenebisacrylamide, and 0.25 parts of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 65°C for 5 hours to obtain a mixed solution;

[0106] (3) The mixed solution is centrifuged, washed, and dried to obtain temperature-resistant and salt-resistant polymer microspheres.

[0107] Wherein, the solvent in step (1) is a mixed solution of ethanol and water. The double-bond silane coupling agent is 3-(isobutyleneoxy)propyltrimethoxysilane. The stirring rate is 600 r / min, and the reaction temperature is 50° C. The post-treatment is a centrifugation, washing and drying process.

[0108] In step (2), the solvent is a mixed solution of ethanol and ethyl acetate. The surfactant is polyvinyl pyrrolidone. The initiator is azobisisobutyronitrile. The inert gas is nitrogen.

[0109] Comparative Example 4

[0110] A method for preparing temperature-resistant and salt-resistant polymer microspheres comprises the following steps:

[0111] (1) Weighing 0.15 parts of small-size silica particles and 1.5 parts of large-size silica particles respectively and dispersing them in a solvent, then adding 2 parts of a double-bond silane coupling agent, stirring for reaction, and post-treating to obtain mixed modified silica particles; wherein the small-size silica particles have a volume D50 of 40 nm as measured by laser scattering; and the large-size silica particles have a volume D50 of 150 nm as measured by laser scattering;

[0112] (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 3 parts of a surfactant, 12 parts of acrylamide, 12 parts of acrylic acid, 1.5 parts of N,N-methylenebisacrylamide, and 0.25 parts of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 65°C for 5 hours to obtain a mixed solution;

[0113] (3) The mixed solution is centrifuged, washed, and dried to obtain temperature-resistant and salt-resistant polymer microspheres.

[0114] Wherein, the solvent in step (1) is a mixed solution of ethanol and water. The double-bond silane coupling agent is 3-(isobutyleneoxy)propyltrimethoxysilane. The stirring rate is 600 r / min, and the reaction temperature is 50° C. The post-treatment is a centrifugation, washing and drying process.

[0115] In step (2), the solvent is a mixed solution of ethanol and ethyl acetate. The surfactant is polyvinyl pyrrolidone. The initiator is azobisisobutyronitrile. The inert gas is nitrogen.

[0116] Comparative Example 5

[0117] A method for preparing temperature-resistant and salt-resistant polymer microspheres comprises the following steps:

[0118] (1) Weighing 0.4 parts of small-size silica particles and 1.25 parts of large-size silica particles respectively, dispersing them in a solvent, then adding 2 parts of a double-bond silane coupling agent, stirring for reaction, and post-treating to obtain mixed modified silica particles; wherein the small-size silica particles have a volume D50 of 15 nm as measured by laser scattering; and the large-size silica particles have a volume D50 of 150 nm as measured by laser scattering;

[0119] (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 3 parts of a surfactant, 12 parts of acrylamide, 12 parts of acrylic acid, 1.5 parts of N,N-methylenebisacrylamide, and 0.25 parts of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 65°C for 5 hours to obtain a mixed solution;

[0120] (3) The mixed solution is centrifuged, washed, and dried to obtain temperature-resistant and salt-resistant polymer microspheres.

[0121] Wherein, the solvent in step (1) is a mixed solution of ethanol and water. The double-bond silane coupling agent is 3-(isobutyleneoxy)propyltrimethoxysilane. The stirring rate is 600 r / min, and the reaction temperature is 50° C. The post-treatment is a centrifugation, washing and drying process.

[0122] In step (2), the solvent is a mixed solution of ethanol and ethyl acetate. The surfactant is polyvinyl pyrrolidone. The initiator is azobisisobutyronitrile. The inert gas is nitrogen.

[0123] Comparative Example 6

[0124] A method for preparing temperature-resistant and salt-resistant polymer microspheres comprises the following steps:

[0125] (1) Weighing 0.15 parts of small-size silica particles and 1.5 parts of large-size silica particles respectively, dispersing them in a solvent, then adding 5 parts of a double-bond silane coupling agent, stirring for reaction, and post-treating to obtain mixed modified silica particles; wherein the small-size silica particles have a volume D50 of 15 nm as measured by laser scattering; and the large-size silica particles have a volume D50 of 150 nm as measured by laser scattering;

[0126] (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 3 parts of a surfactant, 12 parts of acrylamide, 12 parts of acrylic acid, 1.5 parts of N,N-methylenebisacrylamide, and 0.25 parts of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 65°C for 5 hours to obtain a mixed solution;

[0127] (3) The mixed solution is centrifuged, washed, and dried to obtain temperature-resistant and salt-resistant polymer microspheres.

[0128] Wherein, the solvent in step (1) is a mixed solution of ethanol and water. The double-bond silane coupling agent is 3-(isobutyleneoxy)propyltrimethoxysilane. The stirring rate is 600 r / min, and the reaction temperature is 50° C. The post-treatment is a centrifugation, washing and drying process.

[0129] In step (2), the solvent is a mixed solution of ethanol and ethyl acetate. The surfactant is polyvinyl pyrrolidone. The initiator is azobisisobutyronitrile. The inert gas is nitrogen.

[0130] Comparative Example 7

[0131] A method for preparing temperature-resistant and salt-resistant polymer microspheres comprises the following steps:

[0132] (1) Weighing 0.15 parts of small-size silica particles and 1.5 parts of large-size silica particles respectively, dispersing them in a solvent, then adding 2 parts of a double-bond silane coupling agent, stirring for reaction, and post-treating to obtain mixed modified silica particles; wherein the small-size silica particles have a volume D50 of 15 nm as measured by laser scattering; and the large-size silica particles have a volume D50 of 150 nm as measured by laser scattering;

[0133] (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 3 parts of a surfactant, 12 parts of acrylamide, 12 parts of acrylic acid, 1.5 parts of N,N-methylenebisacrylamide, and 0.25 parts of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 85°C for 5 hours to obtain a mixed solution;

[0134] (3) The mixed solution is centrifuged, washed, and dried to obtain temperature-resistant and salt-resistant polymer microspheres.

[0135] Wherein, the solvent in step (1) is a mixed solution of ethanol and water. The double-bond silane coupling agent is 3-(isobutyleneoxy)propyltrimethoxysilane. The stirring rate is 600 r / min, and the reaction temperature is 50° C. The post-treatment is a centrifugation, washing and drying process.

[0136] In step (2), the solvent is a mixed solution of ethanol and ethyl acetate. The surfactant is polyvinyl pyrrolidone. The initiator is azobisisobutyronitrile. The inert gas is nitrogen.

[0137] Performance Test:

[0138] The heat-resistant and salt-resistant polymer microspheres prepared in Examples 1-9 and Comparative Examples 1-7 were dispersed in deionized water, and their initial particle sizes were determined by laser particle size analyzer. The heat-resistant and salt-resistant polymer microspheres prepared in Examples 1-9 and Comparative Examples 1-7 were then dispersed in simulated formation water with a mineralization of 30,000 mg / L, and expanded at 80°C for different times, and their expansion multiples were determined. The results are shown in Table 1.

[0139] The core tube was connected to the process and water-flooded at a rate of 0.5 ml / min. After the pressure stabilized, the pressure value was recorded as A. Then, 1.5 wt% of microsphere flooding fluid 2PV was injected at a rate of 0.5 ml / min, and the core injected with microspheres was aged at the experimental temperature for 8 days. Then, subsequent water flooding was carried out at a rate of 0.5 ml / min until the pressure stabilized. The pressure value was recorded as B, and the plugging rate was calculated. The plugging rate η% = (BA) / B×100%, and the results are shown in Table 2.

[0140]

[0141]

[0142] From the experimental data of the above embodiments and comparative examples, it can be seen that the present invention uses silicon dioxide with different particle sizes to carry out composite modification on polymers, which can not only play the role of strengthening inorganic materials, but also achieve the purpose of toughening and can significantly improve the heat resistance of materials.

[0143] Figure 1 This is a scanning electron microscope image of the heat-resistant and salt-resistant polymer microspheres of Example 9. It can be seen from the image that the surface of the particles is relatively rough, indicating that the polymer has been successfully coated on the surface of the silica particles. Figure 2 The transmission electron microscope image of the heat-resistant and salt-resistant polymer microspheres of Example 9 shows that there is a small amount of small-sized silica around the large-sized silica particles in the middle of the polymer microspheres, and the outermost layer is a polymer coating layer. This indicates that during the polymerization process, the small-sized silica particles partially agglomerated around the large-sized silica particles to form a multi-core structure. In particular, it can be seen from Examples 7-9 that when the D50 of the large-sized silica particles is 100-200nm by volume as measured by laser scattering, the polymer microspheres have better high temperature resistance, salt resistance and plugging performance.

[0144] Compared with Example 9, Comparative Examples 1 and 2 do not add small-particle silica or large-particle silica, and their salt resistance, heat resistance, expansion performance and plugging performance are deteriorated. It is speculated that this may be because the present invention adds a large amount of large-particle silica, supplemented by a small amount of small-particle silica, and the small amount of small-particle silica has a tendency to aggregate on the surface of large-particle silica during the polymerization process, thereby synthesizing inorganic-polymer microspheres with a dual-core or even multi-core structure. The multi-core structure can effectively disperse the shear force on the microspheres, and the covalent bond between the silica cores of different particle sizes and the adjacent polymer chains can promote the rearrangement of the microsphere network structure under the action of external forces, thereby consuming a large amount of energy, and the different particle sizes of silica work together to enhance the microspheres' ability to resist shear and high heat and high salt. A small amount of small-sized silica-polymer microspheres that have not formed a multi-core structure can improve the dispersion of large-sized silica-polymer microspheres in the organism, play the dispersing role of inorganic fillers, increase the stress required for the microspheres to deform under stress, and enhance the viscoelasticity of the system. The small-sized silica, large-sized silica and polymer matrix are cross-linked with each other, which limits the movement of polymer chains, has strong deformation recovery ability and the ability to resist erosion and damage, and can more easily enter the micropores of the formation under the action of displacement pressure difference and achieve dynamic plugging.

[0145] It can be seen from Comparative Examples 3-5 that when the particle size of small-particle silica is too small or the dosage is too large, it is easy to agglomerate; when the particle size is too large, it cannot play the role of dispersion and internal nucleation, affecting the high temperature resistance and salt resistance of the polymer microspheres. It can be seen from Comparative Example 6 that when the dosage of double-bond silane coupling agent is too much, it will cause excessive cross-linking of silica, resulting in adhesion or agglomeration, affecting the plugging performance. It can be seen from Comparative Example 7 that the polymerization temperature is too high, the reaction rate is too fast, and the reaction system is unstable, which will also lead to agglomeration, affecting the molding of microspheres, and is not conducive to improving the salt resistance, heat resistance and other properties.

[0146] It can be seen that the present invention uses acrylamide, acrylic acid, N, N-methylenebisacrylamide as reaction monomers and crosslinking agents, and different particle size silica as reinforcing materials to prepare heat-resistant and salt-resistant polymer microspheres, which has the advantages of simple operation, mild reaction conditions, short reaction time, stable reaction process, etc. The small particle size silica, large particle size silica and polymer matrix are crosslinked with each other, which can significantly improve the heat resistance and salt resistance of the microspheres while playing the role of inorganic material reinforcement.

Claims

1. A method for preparing temperature-resistant and salt-resistant polymer microspheres, characterized in that: The following steps are involved: (1) Weighing 0.1-0.2 parts of small-size silica particles and 1-2 parts of large-size silica particles respectively, dispersing them in a solvent, then adding 1-3 parts of a double-bond silane coupling agent, stirring for reaction, and post-treating to obtain mixed modified silica particles; wherein the small-size silica particles have a volume D50 of 10-20 nm as measured by laser scattering; and the large-size silica particles have a volume D50 of 70-300 nm as measured by laser scattering; (2) Add the mixed modified silica particles to a container containing a solvent and stir evenly; then add 1-4 parts of a surfactant, 8-16 parts of acrylamide, 8-16 parts of acrylic acid, 1-2 parts of N,N-methylenebisacrylamide, and 0.1-0.5 parts of an initiator, respectively, disperse evenly by ultrasonication, pass an inert gas, and react at 55-75°C for 3-6 hours to obtain a mixed solution; (3) The mixed solution is centrifuged, washed, and dried to obtain temperature-resistant and salt-resistant polymer microspheres.

2. The method for preparing the temperature-resistant and salt-resistant polymer microspheres according to claim 1, characterized in that: The solvent in step (1) is a mixed solution of ethanol and water.

3. The method for preparing the temperature-resistant and salt-resistant polymer microspheres according to claim 1, characterized in that: The double bond-containing silane coupling agent in step (1) is at least one of vinyl triethoxysilane, 3-(isobutyleneoxy)propyl trimethoxysilane, vinyl trimethoxysilane, and vinyl tri(β-methoxyethoxy)silane; and the D50 of the large-size silica particles measured by laser scattering is 100-200 nm by volume.

4. The method for preparing the temperature-resistant and salt-resistant polymer microspheres according to claim 1, characterized in that: In step (1), the stirring rate is 400-700 r / min and the reaction temperature is 40-60°C.

5. The method for preparing the temperature-resistant and salt-resistant polymer microspheres according to claim 1, characterized in that: The post-treatment in step (1) is a process of centrifugation, washing and drying.

6. The method for preparing the temperature-resistant and salt-resistant polymer microspheres according to claim 1, characterized in that: The solvent in step (2) is a mixed solution of ethanol and ethyl acetate.

7. The method for preparing the temperature-resistant and salt-resistant polymer microspheres according to claim 1, characterized in that: The surfactant in step (2) is polyvinyl pyrrolidone.

8. The method for preparing the temperature-resistant and salt-resistant polymer microspheres according to claim 1, characterized in that: The initiator in step (2) is azobisisobutyronitrile.

9. The method for preparing the temperature-resistant and salt-resistant polymer microspheres according to claim 1, characterized in that: In step (2), the inert gas is nitrogen.

10. A temperature-resistant and salt-resistant polymer microsphere, characterized in that: The microspheres are prepared by the method for preparing the temperature-resistant and salt-resistant polymer microspheres according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Profile control oil-displacement agent for core-shell type inorganic / organic polymer composite microballoon

    CN102485830A

  • Preparation method of heat-resistant and salt-tolerant oil-displacing polymer containing nano particles

    CN106749898A