High-performance two-step low-pressure anti-gravity casting method and device
By combining the ebullated bed cooling furnace in the low-pressure anti-gravity casting method and adjusting the pressure and flow rate of the ebullating cooling medium, the problem of low cooling rate of complex parts castings is solved, and high-performance castings are produced with efficient cooling and low defects. .
Patent Information
- Application Number
- CN202411043402.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-01
AI Technical Summary
In fields such as aerospace and automotive transportation, when low-pressure anti-gravity casting methods are used to cast complex parts, the cooling rate of the castings is low, resulting in problems such as coarse grains, high defect rates, and low yields.
Using a high-performance two-step low-pressure anti-gravity casting method, combined with an ebullated bed cooling furnace to enhance cooling, the pressure and flow rate of the ebullating cooling medium are adjusted during the mold filling and solidification processes to achieve smooth mold filling and uniform cooling of the casting.
It improves the fineness of grains, low defect rate and dense structure of castings, reduces shrinkage cavities, shrinkage porosity and hot cracking defects, and obtains high-performance high-end complex castings.
Smart Images

Figure CN118720102A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a high-performance two-step low-pressure anti-gravity casting method and a device. Background Art
[0002] Low-pressure counter-gravity casting is a casting method that allows liquid metal to fill the mold cavity and solidify under a certain pressure. First, place the molten metal in the insulation furnace and seal it. Then, dry compressed gas is introduced into the sealed insulation furnace. The molten metal in the insulation furnace rises along the riser under gas pressure and enters the mold cavity through the gate. The gas pressure above the insulation furnace is maintained until the molten metal completely fills the mold cavity. The gas pressure in the insulation furnace is maintained until it solidifies to form a casting. Then the pressure in the insulation furnace is released, and the unsolidified molten metal in the riser of the insulation furnace flows back to the insulation furnace. Finally, the pressure of the clamping device on the top of the mold is released and the casting is taken out. Compared with gravity casting, low-pressure counter-gravity casting can not only reduce filling turbulence, achieve smooth filling, reduce air entrainment and oxidation slag defects, but also solidify under pressure, so that the interdendritic space is filled with filling components, which can reduce casting defects such as shrinkage cavities, shrinkage and hot cracking, and obtain a dense solidification structure.
[0003] Therefore, in key areas such as aerospace, automobile transportation, etc., low-pressure anti-gravity casting methods are used to cast parts. However, the structure of the parts used in these key areas is often more complex, and the cooling rate of the castings is low during the casting process, resulting in bottleneck problems such as coarse grains, high defect rate, and low yield rate of the castings. Summary of the invention
[0004] The main purpose of the present invention is to provide a device and a method of using the device to solve the problems raised in the above background.
[0005] The purpose of the present invention can be achieved by adopting the following technical solutions:
[0006] A high performance two-step low pressure counter gravity casting method comprising two steps:
[0007] 1. Stable filling of the metal melt 3, including steps S1 to S3:
[0008] Step S1: Proportioning the metal elements according to the requirements, melting the metal elements with good proportions to make a metal melt 3, and transferring the metal melt 3 to the crucible 2 for standby use;
[0009] Step S2: invert the casting mold 7 and connect it to the horizontal section riser pipe 6 to wait for filling;
[0010] Step S3: introducing compressed gas into the holding furnace 1 through the gas inlet 4, so that the molten metal 3 in the crucible 2 enters the casting mold 7 through the vertical section riser 5 and the horizontal section riser 6 in sequence until the casting mold 7 is full;
[0011] 2. Solidification under low pressure maintenance and enhanced cooling in a fluidized bed cooling furnace 8, including steps S4 to S8:
[0012] Step S4: After the mold 7 is filled, the mold 7 is turned over 180 degrees to make it upright, and the air pressure is continued to be increased until the air pressure is maintained at the desired value;
[0013] Step S5: Start the lifting platform 9, the fluidized bed cooling furnace 8 rises, and the casting mold 7 is gradually immersed in the fluidized bed cooling furnace 8 from bottom to top;
[0014] Step S6: in the process of the casting mold 7 being gradually immersed in the fluidized bed cooling furnace 8, the pressure and flow rate of the boiling cooling medium are adjusted according to the cross-sectional area and wall thickness of the casting mold 7 at different heights immersed in the fluidized bed cooling furnace 8, so that the cooling speed of the casting mold 7 at different heights by the fluidized bed cooling furnace 8 is consistent;
[0015] Step S7: After the casting mold 7 is completely immersed in the fluidized bed cooling furnace 8, the gas pressure applied to the molten metal 3 is maintained at a desired value until the molten metal 3 is completely solidified;
[0016] Step S8: venting and reducing the pressure to allow the molten metal 3 in the vertical section riser 5 and the horizontal section riser 6 to flow back into the crucible 2, taking the casting mold 7 out of the fluidized bed cooling furnace 8 and separating it from the horizontal section riser 6, and then taking the casting out of the casting mold 7 for post-processing.
[0017] Preferably, the fluidized bed cooling furnace 8 implements enhanced cooling by boiling a mixed medium of high thermal conductivity solid particles and gas.
[0018] Preferably, in step S2 and step S4, a turning mechanism or a robot can be used to fix and turn the casting mold 7.
[0019] Preferably, in step S3, the pressurization rate of the compressed gas is 5-50 mBar / s, and in steps S4 and S7, the gas pressure is maintained at a required value in the range of 1.1-10 bar.
[0020] Preferably, in step S5, a split type fluidized bed cooling furnace 8 can be used to merge the two sides of the casting mold 7 to wrap the casting mold 7, and then a cooling medium is introduced to cool it.
[0021] Preferably, in step S6 and step S7, the cross-sectional area S and the wall thickness T of the casting satisfy the mathematical relationship with the cooling rate Q, the boiling cooling medium pressure P and the boiling cooling medium flow rate V: S×T=1000×P×V / Q, wherein the unit of the cross-sectional area S of the casting is mm 2 , the unit of wall thickness T is mm, the unit of cooling speed Q is K / s, the unit of boiling cooling medium pressure P is bar, and the unit of boiling cooling medium flow rate V is L / Min.
[0022] Preferably, in step S7, after the casting mold 7 is completely immersed in the fluidized bed cooling furnace 8, it can be separated from the horizontal section riser 6 to allow the metal melt 3 to solidify naturally under atmospheric pressure.
[0023] A high-performance two-step low-pressure anti-gravity casting device comprises a holding furnace 1, wherein a crucible 2 is arranged in the holding furnace 1, wherein a metal melt 3 is arranged in the crucible 2, wherein an air inlet 4 is arranged on the side wall of the holding furnace 1 above the crucible 2, wherein a vertical section riser 5 is connected to the crucible 2, wherein a horizontal section riser 6 is connected to the vertical section riser 5, wherein a casting mold 7 is connected to the horizontal section riser 6, wherein a fluidized bed cooling furnace 8 is arranged below the casting mold 7, wherein a lifting platform 9 is arranged below the fluidized bed cooling furnace 8.
[0024] Preferably, the bottom surface of the horizontal section riser pipe 6 is an inclined structure with a high outer side and a low inner side.
[0025] Preferably, one end of the horizontal section riser pipe 6 connected to the casting mold 7 is an inwardly contracting conical structure, the casting mold 7 is provided with an outwardly expanding conical gate 10, the casting mold 7 is provided with a horizontal runner 11 connecting the conical gate 10 and the cavity, and the inner side of the conical gate 10 is provided with a ceramic ring 12 that fits with its inner wall.
[0026] Compared with the prior art, the beneficial technical effects of the present invention are:
[0027] 1. The present invention combines low-pressure counter-gravity casting with enhanced cooling in a fluidized bed cooling furnace. The first step is to achieve high-performance low-pressure counter-gravity stable filling of the metal melt, and the second step is to achieve high-performance solidification of the metal melt under low-pressure pressure holding and enhanced cooling conditions of a fluidized bed cooling furnace. This can not only achieve the advantages of stable filling of low-pressure counter-gravity casting, less defects of air entrainment and oxidation slag inclusion, sufficient solidification and shrinkage compensation under pressure solidification, less shrinkage holes, shrinkage and thermal cracking defects, and dense organization, but also achieve the beneficial effects of fine grains, low defect rate, small secondary dendrite arm spacing, and dense organization under enhanced cooling conditions of a fluidized bed cooling furnace, and finally obtain high-performance high-end complex castings.
[0028] 2. The present invention uses counter-gravity casting to gradually solidify the casting from the part away from the gate toward the gate under the action of pressure. After the first step of filling is completed and the mold is inverted, the casting is solidified sequentially from bottom to top. At the same time, the fluidized bed cooling furnace is lifted by a lifting platform, so that the casting is immersed in the fluidized bed cooling furnace from bottom to top, and the air pressure and flow rate of the boiling cooling medium in the fluidized bed cooling furnace are adjusted in real time according to the wall thickness and cross-sectional area of the immersed casting, so as to achieve enhanced cooling of the casting from bottom to top, so that various parts of the casting can achieve a consistent high cooling rate in a sequence from bottom to top, effectively enhance the effect of sequential solidification, reduce the time required for sequential solidification, and further improve the performance of the casting.
[0029] 3. The present invention uses a fluidized bed cooling furnace for cooling instead of traditional single medium water cooling or air cooling. It uses a mixed medium of high thermal conductivity solid particles and gas to implement enhanced cooling in a boiling manner, which can maintain the suspension of high thermal conductivity solid medium particles, enhance the convection heat exchange between the cooling medium and the mold, and prevent the mold from cracking and collapsing due to excessive temperature difference between the melt and the cooling medium on both sides of the mold. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a schematic diagram of the overall steps of an embodiment of the present invention;
[0031] Figure 2 It is a schematic diagram of steps S1-S2 of an embodiment of the present invention;
[0032] Figure 3 This is a schematic diagram of step S3 of an embodiment of the present invention;
[0033] Figure 4 It is a schematic diagram of S4 of an embodiment of the present invention;
[0034] Figure 5 It is a schematic diagram of steps S5-S7 of an embodiment of the present invention;
[0035] Figure 6 This is a schematic diagram of step S8 of an embodiment of the present invention;
[0036] Figure 7 A schematic diagram of a split-type fluidized bed cooling furnace according to an embodiment of the present invention;
[0037] Figure 8 It is a schematic diagram of natural solidification under atmospheric pressure according to an embodiment of the present invention.
[0038] In the figure: 1. Holding furnace; 2. Crucible; 3. Metal melt; 4. Air inlet; 5. Vertical riser; 6. Horizontal riser; 7. Mold; 8. Fluidized bed cooling furnace; 9. Lifting platform; 10. Conical gate; 11. Horizontal runner; 12. Ceramic ring. DETAILED DESCRIPTION
[0039] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0040] See also Figures 1 to 8 , an embodiment provided by the present invention:
[0041] A high performance two-step low pressure counter gravity casting method comprising two steps:
[0042] 1. Stable filling of the metal melt 3, including steps S1 to S3:
[0043] Step S1: Proportioning the metal elements according to the requirements, melting the metal elements with good proportions to make a metal melt 3, and transferring the metal melt 3 to the crucible 2 for standby use;
[0044] Step S2: invert the casting mold 7 and connect it to the horizontal section riser pipe 6 to wait for filling;
[0045] Step S3: introducing compressed gas into the holding furnace 1 through the gas inlet 4, so that the molten metal 3 in the crucible 2 enters the casting mold 7 through the vertical section riser 5 and the horizontal section riser 6 in sequence until the casting mold 7 is full;
[0046] 2. Solidification under low pressure maintenance and enhanced cooling in a fluidized bed cooling furnace 8, including steps S4 to S8:
[0047] Step S4: After the mold 7 is filled, the mold 7 is turned over 180 degrees to make it upright, and the air pressure is continued to be increased until the air pressure is maintained at the desired value;
[0048] Step S5: Start the lifting platform 9, the fluidized bed cooling furnace 8 rises, and the casting mold 7 is gradually immersed in the fluidized bed cooling furnace 8 from bottom to top;
[0049] Step S6: in the process of the casting mold 7 being gradually immersed in the fluidized bed cooling furnace 8, the pressure and flow rate of the boiling cooling medium are adjusted according to the cross-sectional area and wall thickness of the parts at different heights of the casting mold 7 immersed in the fluidized bed cooling furnace 8, so that the cooling speed of the fluidized bed cooling furnace 8 on the parts at different heights of the casting mold 7 is consistent;
[0050] Step S7: After the casting mold 7 is completely immersed in the fluidized bed cooling furnace 8, the gas pressure applied to the molten metal 3 is maintained at a desired value until the molten metal 3 is completely solidified;
[0051] Step S8: venting and reducing the pressure to allow the molten metal 3 in the vertical section riser 5 and the horizontal section riser 6 to flow back into the crucible 2, taking the casting mold 7 out of the fluidized bed cooling furnace 8 and separating it from the horizontal section riser 6, and then taking the casting out of the casting mold 7 for post-processing.
[0052] Furthermore, the fluidized bed cooling furnace 8 implements enhanced cooling in a boiling manner through a mixed medium of high thermal conductivity solid particles and gas, instead of traditional single medium water cooling or air cooling, which can significantly refine the grains, improve shrinkage cavities, shrinkage porosity and thermal cracking defects, reduce the spacing between secondary dendrite arms, and improve the density of the solidification structure.
[0053] Furthermore, in step S2 and step S4, a turning mechanism or a manipulator can be used to fix and turn the mold 7, which is an automated operation with high efficiency and good effect.
[0054] Further, in step S3, the pressurization rate of the compressed gas is 5-50 mBar / s, and in steps S4 and S7, the gas pressure is maintained in the required value range of 1.1-10 bar.
[0055] Furthermore, in step S5, a split type fluidized bed cooling furnace 8 may be used to merge the two sides of the casting mold 7 so as to wrap the casting mold 7, and then a cooling medium is introduced to cool the casting mold 7.
[0056] Further, in step S6 and step S7, the cross-sectional area S and the wall thickness T of the casting satisfy the mathematical relationship with the cooling rate Q, the boiling cooling medium pressure P and the boiling cooling medium flow rate V: S×T=1000×P×V / Q, where the unit of the cross-sectional area S of the casting is mm 2 , the unit of wall thickness T is mm, the unit of cooling speed Q is K / s, the unit of boiling cooling medium pressure P is bar, and the unit of boiling cooling medium flow rate V is L / Min.
[0057] Furthermore, in step S7, after the casting mold 7 is completely immersed in the fluidized bed cooling furnace 8, it can be separated from the horizontal section riser 6 to allow the metal melt 3 to solidify naturally under atmospheric pressure.
[0058] A high-performance two-step low-pressure anti-gravity casting device comprises a holding furnace 1, a crucible 2 is arranged in the holding furnace 1, a metal melt 3 is arranged in the crucible 2, an air inlet 4 is arranged on the side wall of the holding furnace 1 above the crucible 2, a vertical section liquid riser 5 is connected to the crucible 2, a horizontal section liquid riser 6 is connected above the vertical section liquid riser 5, a casting mold 7 is connected to the horizontal section liquid riser 6, a fluidized bed cooling furnace 8 is arranged below the casting mold 7, and a lifting platform 9 is arranged below the fluidized bed cooling furnace 8. During casting, air is added to the holding furnace 1 through the air inlet 4. The metal melt 3 in the crucible 2 is pressurized to pass through the vertical riser 5 and the horizontal riser 6 in turn into the casting mold 7, and the air pressure is maintained. Then the casting mold 7 is turned over, and the lifting platform 9 is started to make the boiling bed cooling furnace 8 gradually wrap the casting mold 7 from the bottom. During the wrapping process, the air pressure and flow rate of the boiling cooling medium are adjusted to make the casting in the casting mold 7 reach a consistent high cooling rate in various parts, realize layer-by-layer sequential shrinkage compensation, reduce shrinkage defects, reduce hot cracking and residual stress caused by local uneven solidification and shrinkage, and cast high-performance castings.
[0059] Furthermore, the bottom surface of the horizontal section riser 6 is an inclined structure with a high outer side and a low inner side, so that the molten metal 3 in the vertical section riser 5 and the horizontal section riser 6 can flow back into the crucible 2 when the pressure is reduced.
[0060] Furthermore, one end of the horizontal section riser 6 connected to the casting mold 7 is a tapered structure that contracts inwardly, and the casting mold 7 is provided with an outwardly expanding tapered gate 10, which is convenient for inserting the horizontal section riser 6 into the tapered gate 10, and for facilitating the rising and reflux of the molten metal 3. The casting mold 7 is provided with a horizontal runner 11 connecting the tapered gate 10 and the cavity, so that the casting mold 7 will not be blocked by the insulation furnace 1 when flipping, and the flipping action can be completed smoothly, so that it can be immersed in the boiling bed cooling furnace 8 from bottom to top. The inner side of the tapered gate 10 is provided with a ceramic ring 12 that fits with its inner wall, so that the connection between the horizontal section riser 6 and the tapered gate 10 is tighter, thereby ensuring the sealing.
[0061] Example 1
[0062] 1. Smooth filling of the molten metal 3. The required casting is a magnesium alloy casting with a variable cross-sectional area in the height direction. The metal elements with a ratio of 6.16wt.% Gd, 3.12wt.% Y, 0.33wt.% Zr and the rest Mg are melted to make the molten metal 3, and the molten metal 3 is transferred to the crucible 2 for standby use; the casting mold 7 is inverted and connected to the horizontal section riser 6 to wait for filling; compressed gas is introduced into the holding furnace 1 through the air inlet 4 at a pressurization rate of 20mBar / s, so that the molten metal 3 in the crucible 2 enters the casting mold 7 through the vertical section riser 5 and the horizontal section riser 6 in turn until the casting mold 7 is full;
[0063] 2. Low-pressure pressure maintenance and enhanced cooling by the fluidized bed cooling furnace 8. After the mold 7 is filled, turn the mold 7 180 degrees to make it upright, continue to increase the air pressure, and finally keep the air pressure at 1.2 bar; start the lifting platform 9, the fluidized bed cooling furnace 8 rises, and the mold 7 is gradually immersed in the fluidized bed cooling furnace 8 from bottom to top; in the process of the mold 7 gradually being immersed in the fluidized bed cooling furnace 8, according to the cross-sectional area and wall thickness of the different height parts of the mold 7 immersed in the fluidized bed cooling furnace 8, adjust the gas pressure of the boiling cooling medium. The pressure and flow rate are adjusted so that the fluidized bed cooling furnace 8 can achieve the same cooling speed for different height parts of the mold 7; after the mold 7 is completely immersed in the fluidized bed cooling furnace 8, the gas pressure applied to the molten metal 3 is maintained at 1.2 bar until the molten metal 3 is completely solidified; the gas is released and the pressure is reduced so that the molten metal 3 in the vertical section riser 5 and the horizontal section riser 6 flow back into the crucible 2, the mold 7 is taken out of the fluidized bed cooling furnace 8 and separated from the horizontal section riser 6, and then the casting is taken out of the mold 7 for post-processing.
[0064] The specific adjustment of the gas pressure and flow rate of the boiling cooling medium in the boiling bed cooling furnace 8 is as follows:
[0065] (1) The casting is immersed in the fluidized bed cooling furnace 8 at a height of 10 mm and a cross-sectional area of 250 mm. 2 , when the wall thickness is 6mm, adjust the boiling cooling medium pressure to 10bar, adjust the boiling cooling medium flow rate to 6L / Min, and make the cooling speed of the boiling bed cooling furnace 8 40k / s;
[0066] (2) The casting is immersed in the fluidized bed cooling furnace 8 at a height of 25 mm and a cross-sectional area of 350 mm. 2 , when the wall thickness is 9 mm, the boiling cooling medium pressure is adjusted to 14.5 bar, the boiling cooling medium flow rate is adjusted to 8.7 L / Min, and the cooling rate of the boiling bed cooling furnace 8 is 40 k / s;
[0067] (3) The casting is immersed in the fluidized bed cooling furnace 8 at a height of 40 mm and a cross-sectional area of 450 mm. 2 , when the wall thickness is 12 mm, adjust the boiling cooling medium pressure to 19.0 bar, adjust the boiling cooling medium flow rate to 11.4 L / Min, and make the cooling speed of the boiling bed cooling furnace 8 40 k / s;
[0068] (4) The casting is immersed in the fluidized bed cooling furnace 8 at a height of 55 mm and a cross-sectional area of 300 mm. 2 , when the wall thickness is 3mm, adjust the boiling cooling medium pressure to 7.7bar, adjust the boiling cooling medium flow rate to 4.6L / Min, and make the cooling speed of the boiling bed cooling furnace 8 40k / s;
[0069] The post-treatment is to apply T6 heat treatment to the casting, including solution treatment at 500°C for 12 hours, hot water quenching at 70°C, and aging treatment at 200°C for 120 hours, thereby obtaining a Mg-6.16Gd-3.12Y-0.33Zr (wt.%) high-performance magnesium alloy casting with a defect rate of 0.03%, a maximum defect of 20um, a grain size of 10um, a yield strength of 236MPa, a tensile strength of 357MPa, and an elongation of 15.3%.
[0070] Example 2
[0071] 1. Smooth filling of the molten metal 3. The required casting is a magnesium alloy casting with a variable cross-sectional area in the height direction. The metal elements with a ratio of 6.16wt.% Gd, 3.12wt.% Y, 0.33wt.% Zr and the rest Mg are melted to make the molten metal 3, and the molten metal 3 is transferred to the crucible 2 for standby use; the casting mold 7 is inverted and connected to the horizontal section riser 6 to wait for filling; compressed gas is introduced into the holding furnace 1 through the air inlet 4 at a pressurization rate of 20mBar / s, so that the molten metal 3 in the crucible 2 enters the casting mold 7 through the vertical section riser 5 and the horizontal section riser 6 in turn until the casting mold 7 is full;
[0072] 2. Low-pressure pressure maintenance and enhanced cooling by the fluidized bed cooling furnace 8. After the mold 7 is filled, turn the mold 7 180 degrees to make it upright, continue to increase the air pressure, and finally keep the air pressure at 1.2 bar; start the lifting platform 9, the fluidized bed cooling furnace 8 rises, and the mold 7 is gradually immersed in the fluidized bed cooling furnace 8 from bottom to top; in the process of the mold 7 gradually being immersed in the fluidized bed cooling furnace 8, according to the cross-sectional area and wall thickness of the different height parts of the mold 7 immersed in the fluidized bed cooling furnace 8, adjust the gas pressure of the boiling cooling medium. The pressure and flow rate are adjusted so that the fluidized bed cooling furnace 8 can achieve the same cooling speed for different height parts of the mold 7; after the mold 7 is completely immersed in the fluidized bed cooling furnace 8, the gas pressure applied to the molten metal 3 is maintained at 1.2 bar until the molten metal 3 is completely solidified; the gas is released and the pressure is reduced so that the molten metal 3 in the vertical section riser 5 and the horizontal section riser 6 flow back into the crucible 2, the mold 7 is taken out of the fluidized bed cooling furnace 8 and separated from the horizontal section riser 6, and then the casting is taken out of the mold 7 for post-processing.
[0073] The specific adjustment of the gas pressure and flow rate of the boiling cooling medium in the boiling bed cooling furnace 8 is as follows:
[0074] (1) The casting is immersed in the fluidized bed cooling furnace 8 at a height of 10 mm and a cross-sectional area of 250 mm. 2 , when the wall thickness is 6 mm, adjust the boiling cooling medium pressure to 7.1 bar, adjust the boiling cooling medium flow rate to 4.2 L / Min, and make the cooling speed of the boiling bed cooling furnace 8 20 k / s;
[0075] (2) The casting is immersed in the fluidized bed cooling furnace 8 at a height of 25 mm and a cross-sectional area of 350 mm. 2 , when the wall thickness is 9 mm, adjust the boiling cooling medium pressure to 10.2 bar, adjust the boiling cooling medium flow rate to 6.1 L / Min, and make the cooling speed of the boiling bed cooling furnace 8 20 k / s;
[0076] (3) The casting is immersed in the fluidized bed cooling furnace 8 at a height of 40 mm and a cross-sectional area of 450 mm. 2 , when the wall thickness is 12 mm, adjust the boiling cooling medium pressure to 13.4 bar, adjust the boiling cooling medium flow rate to 8.0 L / Min, and make the cooling speed of the boiling bed cooling furnace 8 to 20 k / s;
[0077] (4) The casting is immersed in the fluidized bed cooling furnace 8 at a height of 55 mm and a cross-sectional area of 300 mm. 2 , when the wall thickness is 3mm, adjust the boiling cooling medium pressure to 5.5bar, adjust the boiling cooling medium flow rate to 3.3L / Min, and make the cooling speed of the boiling bed cooling furnace 8 to 20k / s;
[0078] The post-treatment is to apply T6 heat treatment to the casting, including 500°C solution treatment for 12 hours, 70°C hot water quenching, and 200°C aging treatment for 120 hours, thereby obtaining a high-performance Mg-6.14Gd-3.15Y-0.32Zr (wt.%) magnesium alloy casting with a defect rate of 0.05%, a maximum defect of 36um, a grain size of 18um, a yield strength of 215MPa, a tensile strength of 340MPa, and an elongation of 11.2%.
[0079] Comparative Example 1
[0080] The required castings are all Mg-6.18Gd-3.11Y-0.33Zr (wt.%) magnesium alloy castings with variable cross-sectional area in the height direction. The castings are prepared by a conventional low-pressure counter-gravity casting method. During the casting process, the air pressure is maintained at 1.2 bar, air cooling, and the cooling rate of the metal melt 3 is 0.5 k / s. After the casting is formed, T6 heat treatment is applied to it, including 500°C solution treatment for 12 hours, 70°C hot water quenching, and 200°C aging treatment for 120 hours, to obtain Mg-6.18Gd-3.11Y-0.33Zr (wt.%) magnesium alloy castings with a defect rate of 0.62%, a maximum defect of 1650um, a grain size of 120um, a yield strength of 185MPa, a tensile strength of 274MPa, and an elongation of 3.2%.
[0081] Table 1 Casting process parameters used in Example 1, Example 2 and Comparative Example 1
[0082]
[0083] Table 2 Defects, grain size and mechanical properties of castings obtained in Example 1, Example 2 and Comparative Example 1
[0084]
[0085] It can be seen from Table 1 and Table 2 that the castings cast by the casting method of the present invention can significantly improve the cooling rate. By adjusting the gas pressure and flow rate of the boiling cooling medium, each part of the casting can achieve a consistent high cooling rate, so that the defect rate of the casting is lower, the maximum defect is smaller, the grain size is finer, the yield strength is higher, the tensile strength is higher, and the elongation is higher.
[0086] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A high performance two-step low pressure counter gravity casting method, characterized in that: It consists of two steps:
1. Smooth filling of the metal melt (3), including steps S1 to S3: Step S1: metal elements are proportioned according to requirements, the proportioned metal elements are melted to produce a metal melt (3), and the metal melt (3) is transferred to a crucible (2) for standby use; Step S2: invert the casting mold (7) and connect it to the horizontal section riser (6) to wait for filling; Step S3: introducing compressed gas into the holding furnace (1) through the gas inlet (4) so that the molten metal (3) in the crucible (2) enters the casting mold (7) through the vertical section riser (5) and the horizontal section riser (6) in sequence until the casting mold (7) is full; 2. Low pressure holding and fluidized bed cooling furnace (8) to enhance solidification under cooling, including steps S4 to S8: Step S4: After the casting mold (7) is filled, the casting mold (7) is turned over 180 degrees to make it upright, and the air pressure is continued to be increased until the air pressure is maintained at the desired value; Step S5: starting the lifting platform (9), the fluidized bed cooling furnace (8) rises, and the casting mold (7) is gradually immersed in the fluidized bed cooling furnace (8) from bottom to top; Step S6: in the process of the casting mold (7) being gradually immersed in the fluidized bed cooling furnace (8), the pressure and flow rate of the fluidized bed cooling medium are adjusted according to the cross-sectional area and wall thickness of the parts at different heights of the casting mold (7) immersed in the fluidized bed cooling furnace (8), so that the cooling speed of the fluidized bed cooling furnace (8) on the parts at different heights of the casting mold (7) is consistent; Step S7: After the casting mold (7) is completely immersed in the fluidized bed cooling furnace (8), the gas pressure applied to the molten metal (3) is maintained at a desired value until the molten metal (3) is completely solidified; Step S8: venting and reducing the pressure to allow the molten metal (3) in the vertical section riser (5) and the horizontal section riser (6) to flow back into the crucible (2); taking the casting mold (7) out of the fluidized bed cooling furnace (8) and separating it from the horizontal section riser (6); and then taking the casting out of the casting mold (7) for post-processing.
2. A high performance two-step low pressure counter gravity casting method according to claim 1, characterized in that: The fluidized bed cooling furnace (8) implements enhanced cooling in a boiling manner using a mixed medium of high thermal conductivity solid particles and gas.
3. A high performance two-step low pressure counter gravity casting method according to claim 1, characterized in that: In step S2 and step S4, the casting mold (7) can be fixed and flipped using a flipping mechanism or a robot.
4. A high performance two-step low pressure counter gravity casting method according to claim 1, characterized in that: In step S3, the pressurization rate of the compressed gas is 5-50 mBar / s, and in steps S4 and S7, the gas pressure is maintained at a required value in the range of 1.1-10 bar.
5. A high performance two-step low pressure counter gravity casting method according to claim 1, characterized in that: In step S5, a split type fluidized bed cooling furnace (8) can be used to merge the two sides of the casting mold (7) to wrap the casting mold (7), and then a cooling medium is introduced to cool it.
6. A high performance two-step low pressure counter gravity casting method according to claim 1, characterized in that: In step S6 and step S7, the cross-sectional area and wall thickness T of the casting satisfy the mathematical relationship with the cooling rate Q, the boiling cooling medium pressure P and the boiling cooling medium flow rate V: S×T=1000×P×V / Q, where the unit of the cross-sectional area S of the casting is mm 2 , the unit of wall thickness T is mm, the unit of cooling speed Q is K / s, the unit of boiling cooling medium pressure P is bar, and the unit of boiling cooling medium flow rate V is L / Min.
7. A high performance two-step low pressure counter gravity casting method according to claim 1, characterized in that: In step S7, after the casting mold (7) is completely immersed in the fluidized bed cooling furnace (8), it can be separated from the horizontal section riser (6) to allow the metal melt (3) to solidify naturally under atmospheric pressure.
8. A high performance two-step low pressure counter gravity casting device as claimed in any one of claims 1 to 7, characterized in that: The invention comprises a heat-insulating furnace (1), wherein a crucible (2) is arranged in the heat-insulating furnace (1), a metal melt (3) is arranged in the crucible (2), an air inlet (4) is arranged on the side wall of the heat-insulating furnace (1) above the crucible (2), a vertical section liquid riser (5) is connected to the crucible (2), a horizontal section liquid riser (6) is connected above the vertical section liquid riser (5), a casting mold (7) is connected to the horizontal section liquid riser (6), a fluidized bed cooling furnace (8) is arranged below the casting mold (7), and a lifting platform (9) is arranged below the fluidized bed cooling furnace (8).
9. A high performance two-step low pressure counter gravity casting device according to claim 8, characterized in that: The bottom surface of the horizontal section liquid riser (6) is an inclined structure with a high outer side and a low inner side.
10. A high performance two-step low pressure counter gravity casting device according to claim 8, characterized in that: One end of the horizontal section riser (6) connected to the casting mold (7) is a conical structure that contracts inwardly, the casting mold (7) is provided with a conical gate (10) that expands outwardly, the casting mold (7) is provided with a horizontal runner (11) that connects the conical gate (10) and the mold cavity, and the inner side of the conical gate (10) is provided with a ceramic ring (12) that fits with the inner wall thereof.
Citation Information
Patent Citations
Immersed water mist cooling metal mould device and using method thereof
CN109128093A
Casting forming system with turnover directional cooling function and using method thereof
CN110202120A
Magnesium alloy anti-gravity casting equipment and pouring flame-retardant method thereof
CN115608957A
Gravity casting method and device integrating flexible gradient sequence and cooling speed enhanced solidification
CN117862468A
Metal casting and solidification
US3381742A
Cited By
Intelligent casting device based on digital boiling cooling channel and control method thereof
CN119319237A
Intelligent casting device based on digital boiling cooling channel and control method thereof
CN119319237B
Intelligent casting device based on robot-assisted enhanced cooling and control method thereof
CN119319238A
Intelligent casting device based on robot-assisted enhanced cooling and control method thereof
CN119319238B
Casting and heat treatment temperature control device based on gas-solid dynamic suspension and control method thereof
CN119549689A