Thermoplastic polyether ester elastomer with broadband microwave strong absorption electromagnetic shielding and preparation method thereof
By introducing a multi-layer structure of liquid metal, MXenes and its derivative materials and rare earth magnetic materials into the polyetherester elastomer, the problem of high-frequency and low-frequency electromagnetic field shielding effects is solved, and strong microwave absorption and electromagnetic shielding in a wide band are achieved, enhancing The loss and conduction effect of electromagnetic waves are eliminated.
Patent Information
- Application Number
- CN202410842002.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult to achieve effective electromagnetic shielding under high-frequency and low-frequency electromagnetic fields simultaneously with existing technology, and traditional metal shielding materials have problems with poor impedance matching and self-stacking tendencies.
The multi-layer spatial structure of one-dimensional conductive material liquid metal, high dielectric constant MXenes and its derivative materials and rare earth magnetic materials is used to enhance the electromagnetic shielding effect by forming heterogeneous interfaces and multiple reflection mechanisms.
It achieves strong absorption of broad-band microwaves and electromagnetic shielding, effectively reduces the surface reflection of electromagnetic waves, increases the loss of incident waves, optimizes the propagation path of electromagnetic waves, and improves the electromagnetic wave energy loss and conduction loss of materials.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer synthesis, in particular to a thermoplastic polyether ester elastomer with wide-band microwave strong absorption and electromagnetic shielding and a preparation method thereof. Background Art
[0002] 3C electronic devices or communication devices such as mobile phones, Bluetooth wireless chargers, laptops, GPS, ADSL and mobile phones are increasingly used in daily life, and also play an important role in industries such as industry and aerospace. During operation, they inevitably generate high-frequency electromagnetic interference (EMI) and noise to the outside world, which affect each other's normal operation and communication quality. With the high frequency and high power of electronic products in the 5G era, a large number of electronic components will generate electromagnetic radiation when working, which will not only cause a certain degree of electromagnetic interference to surrounding equipment, but also increase the risk of people suffering from headaches, depression, immunodeficiency and other diseases. If the human body is exposed to strong electromagnetic fields for a long time, it may even cause cancer. According to investigations by authoritative organizations, electromagnetic radiation pollution has become one of the world's recognized environmental pollution. Therefore, there is an urgent need for efficient electromagnetic shielding materials to attenuate electromagnetic waves to protect the normal operation of electronic equipment and human health.
[0003] Because the shielding body absorbs energy (eddy current loss), reflects energy (interface reflection of electromagnetic waves on the shielding body) and offsets energy (electromagnetic induction generates a reverse electromagnetic field on the shielding layer, which can offset some of the interfering electromagnetic waves) from external interfering electromagnetic waves such as wires, cables, components, circuits or systems, so the shielding body has the function of reducing interference. When the frequency of the interfering electromagnetic field is high, the eddy current generated in the metal material with low resistivity is used to form an offsetting effect on external electromagnetic waves, thereby achieving the shielding effect. When the frequency of the interfering electromagnetic wave is low, high magnetic permeability materials should be used to limit the magnetic lines of force inside the shielding body to prevent them from spreading to the shielded space. In some cases, if good shielding effects are required for both high-frequency and low-frequency electromagnetic fields, different metal materials are often used to form a multi-layer shielding body.
[0004] Conductive paint and EMI conductive paint spraying technology have the characteristics of high conductivity, high electromagnetic shielding efficiency, simple spraying operation (just like surface spraying operation, only a thin layer of conductive paint needs to be sprayed inside the plastic shell), etc. It is suitable for shielding of various plastic products (PC, PC+ABS, ABS, etc.), and is widely used in EMI shielding of electronic equipment such as communication products (mobile phones), computers (notebooks), portable electronic products, consumer electronics, network hardware (servers, etc.), medical equipment, household electronic products, and aerospace and national defense. Spraying conductive paint solves the limitations of space, operation, and cost pressures in making metal shielding covers. Because the spraying operation of conductive paint is extremely simple and plastic metallization is achieved, it has received more and more attention and promotion, and has gradually replaced the previous processes of pasting tin foil, copper paper, and making metal shielding covers.
[0005] Two-dimensional transition metal carbides / nitrides (MXenes) have emerged as potential candidates for microwave absorption (MA) due to their high mechanical stability, high carrier mobility, and good electrochemical stability. However, they still have defects such as poor impedance matching and high self-stacking tendency. Summary of the invention
[0006] The present invention relates to a combination of one-dimensional conductive material liquid metal, high dielectric constant MXenes and its derivative materials, and rare earth magnetic materials and their oxides, which can enhance the electromagnetic shielding effect. A shielding layer with a multi-layer space structure is used to form multiple heterogeneous interfaces, so that the electromagnetic interference field forms eddy currents in the shielding body and generates reflections on the interface between the shielding body and the protected space, thereby greatly weakening the field strength of the interference field in the protected space, curbing the influence of high-frequency electromagnetics, and achieving a shielding effect; at the same time, a rare earth magnetic material with high magnetic permeability is used to increase the eddy current effect, realize impedance matching and electromagnetic wave absorption loss and multiple reflection mechanisms.
[0007] To achieve the above object, the present invention provides the following technical solutions: The present invention discloses a thermoplastic polyether ester elastomer with wide-band microwave strong absorption and electromagnetic shielding, which is prepared from the following components in parts by weight: 35-90 parts of benzoic acid ester, 10 to 65 parts of polyether alcohol, Catalyst 0.01~0.1 parts, Low melting point polyurethane hot melt adhesive 0-30 parts, 0.2-1 part of liquid metal, MXenes and their derivative materials 0.2-2 parts, 0.2 to 2 parts of rare earth magnetic material, Surface grafting agent 0.01~0.6 parts, 0.2 parts of antioxidant.
[0008] As a further embodiment of the present invention: benzoic acid esters and their derivatives are preferably one of dimethyl phthalate, dimethyl isophthalate, ethylene isophthalate, ethylene glycol phthalate, propylene isophthalate, propylene glycol phthalate, butylene isophthalate, butylene phthalate, diphenyl phthalate, a copolymer of dimethyl 1,4-phthalate, 1,4-cyclohexanedimethanol and 1,2-ethylene glycol, 1,4-dimethylenecyclohexane terephthalate and 2,6-butylene naphthalate.
[0009] As a further embodiment of the present invention: the polyether alcohol is one of polyoxypropylene polyol, diethylene glycol diethyl ether, polyoxytetramethylene polyol and tetrahydrofuran-oxypropylene copolymer glycol.
[0010] As a further solution of the present invention: the catalyst should have efficient chemical catalytic activity, preferably tetrabutyl titanate is used as the main catalyst, and one of zirconium tetraoxide, zirconium hydroxide, and ruthenium / zirconium chelate is used as the co-catalyst; and / or, the weight ratio of the main catalyst to the co-catalyst is preferably 1:0.5.
[0011] As a further solution of the present invention: the low melting point polyurethane hot melt adhesive should have low (slow) heat dissipation or thermal hysteresis characteristics and excellent bonding strength, and is a high melt index low melting point hot melt polyurethane with a melt index of at least 10 g / 10min (190°C, 2.16kg), and at least one of WHT-6290, WHT-6227C, WHT-6275H, WHT-6236, WHT-6228C, WHT-6235B, WHT-6229C, WHT-6420C, WHT-6229, and WHT-6232 is optionally selected.
[0012] As a further embodiment of the present invention: the liquid metal is one of liquid nano-silver solution, liquid nano-gold solution, gallium-based liquid metal and its alloys, bismuth-based liquid metal or its alloys; and / or, the nano-gold in the liquid nano-gold solution is preferably at least one of PEG-coated nano-gold particles and BSA-coated nano-gold particles.
[0013] As a further embodiment of the present invention: the gallium-based liquid metal is one of low-melting-point liquid metal gallium, a low-melting-point eutectic gallium-indium alloy (EGaIn, 45-75 wt% Ga and 25-55 wt% In), and a low-melting-point eutectic gallium-indium-tin alloy (55-68 wt% Ga, 22-39 wt% In, 6-10 wt% Sn).
[0014] As a further solution of the present invention: MXenes and their derivative materials should have good heat retardation function, high specific surface area, and easy dispersion characteristics, which are widely used in MXenes. n+1 X nTwo-dimensional transition metal nitrides, carbides or carbonitrides (MXenes) with a Tx-type structure (wherein M represents a transition metal site, X represents nitrogen or carbon, n can vary from 1 to 4, and Tx represents a terminal group (-F, -O, -OH or -Cl) on its surface) and synthetic derivatives MAX and MBene materials derived therefrom (two-dimensional transition metal nitrides, carbides or carbonitrides) can be homogeneous structures, isolated structures, porous structures or layered structures, etc., and at least one of MXenes two-dimensional transition metal carbonitrides, MXenes-Max two-dimensional transition metal carbonitrides, MBene-MAB two-dimensional transition metal borides, and MBene two-dimensional transition metal borides is selected, wherein the MXenes two-dimensional transition metal carbonitride is preferably Ti 3 C 2 Tx MXene、Ti 4 N 3 Tx MXene、Mo 2 Ga 2 CMXene、Ti 2 CTx MXene、Ti 3 AlC 2 、V 2 AlC、Mo 3 AlC 2 , Nb 2 AlC、Nb 4 AlC 3 、 2 AlC、Cr 2 AlC、Mo 2 Ga 2 C. Ti 2 SnC、Ti 3 SiC 2 、Ti 3 AlCN、Ti 2 AlN, TiNbAlC, VCrAlC, TiVAlC, Mo 2 Ti 2 AlC 3 、Mo 2 TiAlC 2 、Ti 3 C 2 I 2 、 4 AlC 3 、V 4 AlC 3 、Ti 4 AlN 3 、TiVNbMoAlC 3、TiVCrNbAlC 3 、(Mo 2 / 3 Sc 1 / 3 ) 2 AlC, (Mo 2 / 3 Y 1 / 3 ) 2 AlC, (W 2 / 3 Y 1 / 3 ) 2 AlC、Ti 3 C 2 、Ti 2 C、Nb 2 C.V 2 C. Ti 2 N, Mo 2 C. Ti 3 CN、Nb 4 C 3 、 4 C 3 、VCrC、V 2 CTx, TiNbC, Mo 2 Ti 2 C 3 One or more of the following: MXene-Max two-dimensional transition metal carbonitride is preferably MXene-based high conductive slurry, single-layer MXene solution, single-layer MXenes powder, multi-layer MXenes solution, multi-layer MXene powder, Nb 2 C MXene, TiVC MXene, V 2 N MXene、V 4 C 3 MXene, TiNbC MXene, Mo 2 TiC 2 MXene、Mo 2 C MXene, Cr 2 C MXene, Ta 2 C MXene, W 1.33 C MXene, Mo 1.33 C MXene、Ti 4 N 3 MXene, aminocarboxylated MXene, polyhedral oligomeric silsesquioxane modified MXene, V 2 In situ growth of MnO 2 MXene, porous MXene, in-situ doped MXene, high entropy MXene, MXene-loaded metal, single atom-doped MXene, element-doped MXene, foam metal-loaded MXene, MXene quantum dots, MXene ink, MXene-TiVNbMoC3 、MXene-TiVCrMoC 3 、Ti 3 AlC 2 MAX、Ti 4 AlN 3 MAX、Ti 3 GeC 2 MAX、Ti 2 SnC MAX、TiVAlCMAX、Ti 2 AlN MAX、Ti 3 AlCNMAX、Ti 3 SiC 2 MAX、Ti 2 AlC MAX、Nb 4 AlC 3 MAX、Nb 2 AlC MAX、VCrAICMAX、V 4 AlC 3 MAX、V 2 AlC MAX、Mo 2 Ti 2 AlC 3 MAX、Mo 2 TiAlC 2 MAX、Ti 2 AlC、MoAlB MAX、Mo 2 Ga 2 C MAX、Mo 3 AlC 2 MAX、ScAl 3 C 3 MAX、Cr 2 AlC MAX、V 2 PC MAX、V 2 ZnC MAX、V 2 GaC MAX、V 2 GeC MAX、Ti 3 SnC 2 MAX、Ti 3 Al 0.5 Cu 0.5 C 2 、Ti 2 VAlC 2 MAX、TiNbAlC MAX、Ta 2 AlC MAX、Ta 4 AlC 3 MAX、Cr 2 TiAlC 2 MAX、(Mo 2 / 3 Sc1 / 3 ) 2 AlC MAX, (W 2 / 3 Sc 1 / 3 ) 2 AlC MAX, (Mo 2 / 3 Y 1 / 3 ) 2 AlC i-MAX, (W 2 / 3 Y 1 / 3 ) 2 AlC i-MAX、Mo 2 Ti 2 One or more of AlC MAX; MBene-MAB two-dimensional transition metal boride and MBene two-dimensional transition metal boride are preferably MnB, Fe 2 B 2 Cr 2 B 2 、CrB、ZrB、Mo 1.33 B. Mo 4 / 3 B 2-x 、V 3 B 2 、MoB、LiNiB、Mo 4 / 3 B 2-x T x 、Li-Mo 2 B 2 、Ti 2 IB 2 、Mo 2 AB 2 , Na-V 2 B 2 , single-layer MBene, or multi-layer MBene, or two or more thereof.
[0015] As a further embodiment of the present invention, the rare earth magnetic material is at least one of gold-coated iron oxide particles, samarium iron nitrogen (SmFeN) magnetic powder, neodymium iron nitrogen (NdFeN) magnetic powder, neodymium iron boron magnetic powder, samarium cobalt magnetic powder, aluminum nickel cobalt magnetic powder, ferrite magnetic powder, and rare earth magnetic oxides. The rare earth magnetic oxides are oxides of 15 lanthanide elements with atomic numbers from 57 to 71 in the periodic table, and oxides of 17 elements including scandium (Sc) and yttrium (Y) with chemical properties similar to lanthanide elements, preferably lutetium oxide (Lu 2 O 3 ), Ytterbium oxide (Yb 2 O 3 ), europium oxide (Eu 2 O 3 ), thulium oxide (Tm 2 O 3 ), yttrium oxide (Y 2 O 3), Erbium Oxide (Er 2 O 3 ), Dysprosium oxide (Dy 2 O 3 ), scandium oxide (Sc 2 O 3 ), gadolinium oxide (Gd 2 O 3 ), holmium oxide (Ho 2 O 3 )、Lanthanum oxide(La 2 O 3 ), neodymium oxide (Nd 2 O 3 ), praseodymium oxide (Pr 6 O 11 ), samarium oxide (Sm 2 O 3 ), cerium oxide (CeO 2 ) and terbium oxide (Tb 4 O 7 ). In these magnetic rare earth materials, each layer retains its intrinsic properties and can interact with adjacent layers through weak interlayer interactions. This electronic structure gives it good properties for efficient conduction of carriers and charges.
[0016] As a further embodiment of the present invention: the surface grafting agent is preferably one of dopamine and its derivatives, and polyphenol compounds, wherein the polyphenol compound is one of tannic acid, gallic acid, ellagic acid, proanthocyanidin, resveratrol, protocatechuic acid, epigallocatechin, theophylline gallate, gossypol, caffeic acid, and curcumin; And / or, dopamine and its derivatives may be one of hydroxy polyethylene glycol dopamine, phenol-dopamine, aldehyde polyethylene glycol dopamine, polydopamine, with a molecular weight not exceeding 5000, preferably 3000.
[0017] As a further solution of the present invention: the antioxidant has excellent properties of preventing thermal oxidation degradation and aging, and is preferably at least one of hindered phenols, hindered amines, aromatics, and phosphites.
[0018] Another aspect of the present invention also discloses a method for preparing the thermoplastic polyether ester elastomer, comprising the following steps: S1. Pretreatment of liquid metals, MXenes and their derivatives, and rare earth magnetic materials: The dried liquid metal, MXenes and its derivative materials, and rare earth magnetic materials are immersed in a solution of a surface grafting agent and deionized water in a mass ratio of 1:5, respectively, and a surface grafting reaction is carried out for 4 to 8 hours at a reaction temperature of 50 to 80°C; after being taken out, washed, filtered, and dried, grafted liquid metal, grafted MXenes and its derivative materials, and grafted rare earth magnetic materials are obtained; S2. Add grafted MXenes and their derivative materials to part of the polyether alcohol at a constant temperature of 60 to 100° C., and stir ultrasonically for 0.5 to 2 hours; then add grafted liquid metal and grafted rare earth magnetic material, and continue to stir ultrasonically to obtain a uniform polyether alcohol mother liquor; Among them, grafted liquid metal, MXenes and its derivative materials and rare earth magnetic materials account for 0.5-4% in the polyether alcohol mixture; S3, placing benzoic acid ester, another part of polyether alcohol, catalyst and low melting point polyurethane hot melt adhesive in a polymerization kettle filled with nitrogen for prepolymerization reaction, the reaction temperature is 160-200° C., and the reaction time is 40-120 min; S4. When the amount of the alcohol substance obtained by the prepolymerization reaction reaches 120% of the amount of the benzoate substance, the polyether alcohol mother liquor and the antioxidant are added to the reactor to carry out a secondary reaction at a reaction temperature of 160 to 200° C. for a reaction time of 0.5 to 2 h; S5. When the viscosity of the mixture in the polymerization kettle reaches 4000~6000 At the same time, the nitrogen in the kettle is purged to a vacuum negative pressure of 0.02-0.4 MPa, and the temperature is raised to 190-230°C for a low-viscosity final polycondensation reaction in vacuum for 1-2 hours. The material is discharged and granulated to obtain a thermoplastic polyether ester elastomer with wide-band microwave strong absorption and electromagnetic shielding.
[0019] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention rationally introduces one-dimensional liquid metal and three-dimensional MXene and its derivatives and rare earth magnetic materials, and designs them into a multi-level spatial structure and an uneven interface structure. This not only gives full play to the advantages of each component material and avoids unbalanced impedance and a single loss mechanism, but also effectively reduces the surface reflection of electromagnetic waves and increases the loss of incident waves. It is also beneficial to optimize the propagation path of electromagnetic waves and achieve additional electromagnetic wave energy loss.
[0020] (2) The present invention introduces the synergy of one-dimensional liquid metal material, three-dimensional MXene material and its derivatives, and rare earth magnetic material to greatly improve the microwave conduction loss induced by multiple reflections inside the material.
[0021] (3) Compared with the blending process of filling a large amount of conductive fillers, the present invention uses a prepolymerization and premixing process to graft one-dimensional liquid metal and three-dimensional MXene and its derivatives and rare earth magnetic materials into the molecular chain segment of polyether ester thermoplastic elastomer. At the same time, due to the large number of OH groups on the surface of MXene, it can form anchor points with TPU containing a large number of urethane structures through hydrogen bonding, avoiding the chronic problem of easy stacking of MXene and its derivatives during blending, and forming a well-dispersed three-dimensional conductive network, which effectively extends the path of micro-current transmission and improves impedance matching, thereby enhancing the conduction loss of electromagnetic waves.
[0022] (4) The electromagnetic shielding thermoplastic polyether ester elastomer of the present invention can be used as an adhesive material in fields with electromagnetic shielding requirements such as laptop computers, PCs, wireless routers, cabin radio transmitters and drones. DETAILED DESCRIPTION
[0023] For ease of understanding of the present invention, the present invention will be described more fully below in conjunction with specific embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.
[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0025] The specific information of the raw materials used in the following examples and comparative examples is as follows: Parabens and their derivatives: The CAS number of dimethyl isophthalate is 1459-93-4, purchased from Merck Reagents; The CAS number of butylene phthalate is 84-74-2, which was purchased from Shanghai Jiader Chemical Technology Co., Ltd. The CAS number of diphenyl phthalate is 84-62-8, and the manufacturer is Hubei Nona Technology Co., Ltd. The CAS number of 2,6-butylene naphthalene diol ester is 94686-82-5, and the manufacturer is Zhengzhou Alpha Chemical Co., Ltd.
[0026] Polyether alcohol: The CAS number of polyoxyethylene polyol is 25322-68-3, and the manufacturer is Dow Chemical of the United States; The CAS number of diethylene glycol diethyl ether is 112-36-7, and the manufacturer is Shanghai Chuangsai Technology Co., Ltd. The CAS number of polytetramethylene ether glycol is 25190-06-1, and the manufacturer is Shanghai Aladdin Biochemical Technology Co., Ltd.
[0027] catalyst: The CAS numbers of tetrabutyl titanate, zirconium tetroxide and zirconium hydroxide are 5593-70-4, 64417-98-7 and 5593-70-4 respectively, and the manufacturers are all Merck Reagent Company; The commercial brand of organic titanium zirconium chelate is Tyzor®NPZ, and the manufacturer is DuPont of the United States.
[0028] Low melting point polyurethane hot melt adhesive: The commercial grade of high melt index and low melting point hot melt TPU is WHT-6228C, and the manufacturer is Wanhua Chemical Group Co., Ltd.
[0029] Liquid Metal: The commercial grades of carboxyl spherical gold nanoparticles and BSA-coated gold nanoparticles are Q-0148898 and Q-0268078, respectively, and both are manufactured by Xi'an Qiyue Biotechnology Co., Ltd. Water-soluble liquid nanosilver, customized, specification 100nm, manufactured by Beijing Zhongke Keyou Technology Co., Ltd.; The commercial brand of the low-melting-point eutectic gallium-indium alloy is TUNGSTITE, the specification is Elyslum, and the manufacturer is Tongxiang Metal Materials (Shanghai) Co., Ltd.
[0030] MXenes and their derivative materials: The commercial grades of TiNbAlC, (Mo2 / 3Y1 / 3)2AlC, W1.33C MXene, Nb4AlC3 MAX, (W2 / 3Y1 / 3)2AlC i-MAX and Fe2B2 are BKA1130132, BKA1240243, BK2021022403, BKA1050053, BK2021022204 and BKM0101121, respectively, and the manufacturers are all Beijing Beike Nanotechnology Co., Ltd.
[0031] Rare earth magnetic materials: The manufacturers of samarium iron nitride (SmFeN) and neodymium iron nitride (NdFeN) magnetic powders are Ningxia Junci New Materials Technology Co., Ltd. The CAS numbers of ytterbium oxide (Yb2O3) and lanthanum oxide (La2O3) are 1314-37-0 and 1312-81-8 respectively, and the manufacturer is Merck Reagent Company.
[0032] Surface grafting agent: The commercial brand of dopamine is A849306, and the manufacturer is Shanghai MacLean Biochemical Technology Co., Ltd.; The CAS number of gallic acid is 141-84-4, and the manufacturer is Guangdong Hongjiang Chemical Reagent Co., Ltd.; The CAS number of ellagic acid is 476-66-4, and the manufacturer is Chengdu Medson Technology Co., Ltd. The CAS number of resveratrol is 501-36-0, and the manufacturer is Hefei Norda Biotechnology Co., Ltd. The CAS number of gossypol is 303-45-7, and the manufacturer is Shandong Xiya Chemical Co., Ltd. The CAS number of caffeic acid is 331-39-5, and the manufacturer is Shandong Xuchen Chemical Technology Co., Ltd.
[0033] The commercial brand of antioxidant 1010 is Irganox 1010, and the manufacturer is BASF of Germany.
[0034] All materials are commercially available common products.
[0035] It is to be understood that the above raw materials and reagents are only examples of some specific embodiments of the present invention, so that the technical solution of the present invention is clearer, and it does not mean that the present invention can only use the above reagents, and the specific scope in the claims shall prevail. In addition, the "parts" described in the examples and comparative examples, unless otherwise specified, refer to parts by weight.
[0036] Any range described in the present invention includes the end value and any numerical value between the end values and any sub-range formed by the end value or any numerical value between the end values.
[0037] Example 1 S1, placing 35 parts of dimethyl isophthalate, 45 parts of polyethylene oxide polyol, 0.02 parts of tetrabutyl titanate, and 0.02 parts of zirconium tetraoxide in a polymerization reactor filled with nitrogen, and reacting at a constant temperature of 160° C. for 130 min to obtain a prepolymer; S2, the dried TiNbAlC, carboxyl spherical nano-gold, and samarium iron nitrogen magnetic powder are immersed in a 70°C constant temperature dopamine\deionized water (dopamine\deionized water is mixed in a weight ratio of 1:5) solution for grafting for 6 hours, and then washed with ethanol and filtered and dried to obtain grafted TiNbAlC, grafted carboxyl spherical nano-gold, and grafted samarium iron nitrogen magnetic powder; S3. At a constant temperature of 60° C., firstly add 2 parts of grafted TiNbAlC and 0.2 parts of grafted carboxyl spherical nano-gold to 20 parts of polyethylene oxide polyol solvent, place under constant temperature and constant speed stirring for 2 hours of ultrasonication, then add 0.2 parts of grafted samarium iron nitrogen magnetic powder and stir and ultrasonicate at the same temperature for 2 hours to obtain a uniformly dispersed polyethylene oxide polyol mixture; S4, when the amount of the alcohol substance obtained by the prepolymerization reaction in step S1 reaches more than 120% of the amount of dimethyl isophthalate substance, the polyoxyethylene polyol mixture obtained in step S3 is added into the polymerization kettle in step S1 to carry out a secondary reaction for 0.5 h, and 0.2 parts of antioxidant 1010 are added at the same time; S5, when the viscosity of the mixture in the polymerization kettle in step S4 reaches 5000 At the same time, the nitrogen in the kettle was purged to a vacuum negative pressure of 0.03 MPa, and the temperature was raised to 200°C for a vacuum low-viscosity final polycondensation reaction for 2 hours. The material was discharged, granulated and cooled to obtain an electromagnetic shielding thermoplastic polyether ester elastomer.
[0038] Comparative Example 1 Compared with Example 1, the only difference is that WHT-6228C, carboxyl spherical nano-gold, TiNbAlC and SmFeN magnetic powder are not introduced.
[0039] Example 2 S1, placing 90 parts of butylene phthalate, 5 parts of diethylene glycol diethyl ether, 0.02 parts of tetrabutyl titanate, 0.02 parts of zirconium hydroxide and 20 parts of WHT-6228C in a polymerization reactor filled with nitrogen, and reacting at a constant temperature of 240° C. for 80 minutes to obtain a prepolymer; S2, the dried BSA is wrapped with nano-gold, (Mo 2 / 3 Y 1 / 3 ) 2 AlC and NdFeN magnetic powder were immersed in a 80℃ constant temperature gallic acid\deionized water solution (gallic acid and deionized water were mixed in a weight ratio of 1:5) for 8 hours, and then washed with ethanol and filtered and dried to obtain grafted BSA-coated nano-gold, (Mo 2 / 3 Y 1 / 3 ) 2 AlC and NdFeN magnetic powder; S3, at a constant temperature of 60 ° C, first add 0.2 parts of grafted (Mo 2 / 3 Y 1 / 3 ) 2 The AlC was placed under constant temperature and constant speed stirring for 1 hour, and then 0.5 parts of grafted BSA-coated nano-gold and 0.2 parts of grafted NdFeN magnetic powder were added and then ultrasonically stirred for 2 hours in the same environment to obtain a uniformly dispersed diethylene glycol diethyl ether mixture; S4, when the amount of the alcohol substance obtained by the prepolymerization reaction in step S1 reaches more than 120% of the amount of butylene phthalate substance, the diethylene glycol diethyl ether mixture obtained in step S3 is added into the polymerization kettle in step S1 to carry out a secondary reaction for 0.5 h, and 0.2 parts of antioxidant 1010 are added at the same time; S5, when the viscosity of the mixture in the polymerization kettle in step S4 reaches 5000 At the same time, the nitrogen in the kettle was purged to a vacuum negative pressure of 0.2 MPa, and the temperature was raised to 230°C for a vacuum low-viscosity final polycondensation reaction for 1 hour. The material was discharged, granulated and cooled to obtain an electromagnetic shielding thermoplastic polyether ester elastomer.
[0040] Comparative Example 2 Compared with Example 2, the only difference is that no (Mo 2 / 3 Y 1 / 3 ) 2 AlC and NdFeN magnetic powder.
[0041] Example 3 S1, placing 70 parts of diphenyl phthalate, 15 parts of diethylene glycol diethyl ether, 0.02 parts of tetrabutyl titanate, 0.02 parts of zirconium tetraoxide and 10 parts of WHT-6228C in a polymerization reactor filled with nitrogen, and reacting at a constant temperature of 160° C. for 100 min to obtain a prepolymer; S2, drying the obtained water-soluble liquid nanosilver, W 1.33 C MXene and ytterbium oxide were immersed in a constant temperature ellagic acid\deionized water solution (ellagic acid and deionized water were mixed in a weight ratio of 1:5) at 80°C for 8 hours, and then washed with ethanol and filtered and dried to obtain grafted water-soluble liquid nanosilver and W 1.33 C MXene with ytterbium oxide; S3, at a constant temperature of 60°C, add 0.2 parts of grafted W to 15 parts of diethylene glycol diethyl ether. 1.33 The CMXene was placed under constant temperature and constant speed stirring for 1 hour, and then 1 part of grafted water-soluble liquid nanosilver and 1 part of grafted ytterbium oxide were added and ultrasonically stirred for 2 hours in the same environment to obtain a uniformly dispersed diethylene glycol diethyl ether mixture; S4, when the amount of the alcohol substance obtained by the prepolymerization reaction in step S1 reaches more than 120% of the amount of diphenyl phthalate substance, the diethylene glycol diethyl ether mixture obtained in step S3 is added to the polymerization kettle in step S1 to carry out a secondary reaction for 0.5 h, and 0.2 parts of antioxidant 1010 are added at the same time; S5, when the viscosity of the mixture in the polymerization reactor in step S4 reaches 6000 At the same time, the nitrogen in the kettle was purged to a vacuum negative pressure of 0.1 MPa, and the temperature was raised to 240°C for a vacuum low-viscosity final polycondensation reaction for 1.5 hours. The material was discharged, granulated and cooled to obtain an electromagnetic shielding thermoplastic polyether ester elastomer.
[0042] Comparative Example 3 Compared with Example 3, the only difference is that water-soluble liquid nanosilver and ytterbium oxide are not introduced.
[0043] Example 4 S1, placing 60 parts of 2,6-naphthalene diol butanediol, 20 parts of polytetramethylene ether glycol, 0.05 parts of organic titanium zirconium chelate and 3 parts of WHT-6228C in a polymerization kettle filled with nitrogen, and continuously reacting at a constant temperature of 210° C. for 120 min to obtain a prepolymer; S2, drying the low melting point eutectic gallium indium alloy, Nb 4 AlC 3 MAX and lanthanum oxide were immersed in a 80°C constant temperature resveratrol\deionized water solution (resveratrol and deionized water were mixed in a weight ratio of 1:5) for 8 hours, and then washed with ethanol and filtered and dried to obtain the grafted low melting point eutectic gallium indium alloy and Nb 4 AlC 3 MAX and lanthanum oxide; S3, at a constant temperature of 60°C, first add 2 parts of grafted Nb 4 AlC 3 MAX was placed under constant temperature and constant speed stirring for 2 h, and then 0.2 parts of grafted low melting point eutectic gallium-indium alloy and 0.5 parts of grafted lanthanum oxide were added and ultrasonically stirred for 2 h in the same environment to obtain a uniformly dispersed polytetrahydrofuran ether glycol mixture; S4, when the amount of the alcohol substance obtained by the prepolymerization reaction in step S1 reaches more than 120% of the amount of 2,6-butylene naphthalene diol ester, the polytetrahydrofuran ether diol mixture obtained in step S3 is added into the polymerization kettle in step S1 to carry out a secondary reaction for 0.5 h, and 0.2 parts of antioxidant 1010 are added at the same time; S5, when the viscosity of the mixture in the polymerization kettle in step S4 reaches 5000 At the same time, the nitrogen in the kettle was purged to a vacuum negative pressure of 0.4 MPa, and the temperature was raised to 200°C for a vacuum low-viscosity final polycondensation reaction for 1 hour. The material was discharged, granulated and cooled to obtain an electromagnetic shielding thermoplastic polyether ester elastomer.
[0044] Comparative Example 4 Compared with Example 4, the only difference is that the low melting point eutectic gallium-indium alloy is not introduced.
[0045] Example 5 S1, placing 70 parts of dimethyl isophthalate, 15 parts of polyethylene oxide polyol, 0.05 parts of organic titanium zirconium chelate and 10 parts of WHT-6228C in a polymerization kettle filled with nitrogen, and reacting at a constant temperature of 160° C. for 100 min to obtain a prepolymer; S2, the dried (W 2 / 3 Y 1 / 3 ) 2AlC i-MAX and SmFeN magnetic powder were immersed in a 70℃ constant temperature gossypol\deionized water solution (gossypol\deionized water was mixed in a weight ratio of 1:5) for 8 hours, and then washed with ethanol and filtered to obtain the grafted (W 2 / 3 Y 1 / 3 ) 2 AlC i-MAX and SmFeN magnetic powder; S3, at a constant temperature of 60°C, add 1 part of grafted (W 2 / 3 Y 1 / 3 ) 2 AlC i-MAX was placed under constant temperature and constant speed stirring and ultrasonicated for 2 hours, and then 0.5 parts of grafted carboxyl spherical nano-gold and 0.5 parts of grafted samarium iron nitrogen magnetic powder were added and stirred and ultrasonicated for 2 hours at the same temperature to obtain a uniformly dispersed polyethylene oxide polyol mixture; S4, when the amount of the alcohol substance obtained by the prepolymerization reaction in step S1 reaches more than 120% of the amount of dimethyl isophthalate substance, the polyoxyethylene polyol mixture obtained in step S3 is added into the polymerization kettle in step S1 to carry out a secondary reaction for 0.5 h, and 0.2 parts of antioxidant 1010 are added at the same time; S5, when the viscosity of the mixture in the polymerization kettle in step S4 reaches 5000 At the same time, the nitrogen in the kettle was purged to a vacuum negative pressure of 0.03 MPa, and the temperature was raised to 200°C for a vacuum low-viscosity final polycondensation reaction for 2 hours. The material was discharged, granulated and cooled to obtain an electromagnetic shielding thermoplastic polyether ester elastomer.
[0046] Comparative Example 5 S1, placing 70 parts of dimethyl isophthalate, 30 parts of polyethylene oxide polyol, 0.05 parts of organic titanium zirconium chelate and 10 parts of WHT-6228C in a polymerization kettle filled with nitrogen, and reacting at a constant temperature of 160° C. for 100 min to obtain a prepolymer; S2. When the amount of the alcohol substance obtained in step S1 reaches more than 120% of the amount of dimethyl isophthalate, the polymerization kettle is heated to 200° C. to carry out a secondary reaction for 0.5 h, and 0.2 parts of antioxidant 1010 are added at the same time; S3, when the viscosity of the mixture in the polymerization reactor in step S2 reaches 4000 When the nitrogen in the kettle is purged to a vacuum negative pressure of 0.03 MPa, the temperature is raised to 240°C for a final polycondensation reaction in vacuum for 2 hours, and the discharged material is granulated and cooled to obtain a thermoplastic polyether ester elastomer; S4, the dried (W 2 / 3 Y 1 / 3 ) 2AlC i-MAX and SmFeN magnetic powder were immersed in a 70℃ constant temperature gossypol\deionized water solution (gossypol\deionized water was mixed in a weight ratio of 1:5) for 8 hours, and then washed with ethanol and filtered to obtain the grafted (W 2 / 3 Y 1 / 3 ) 2 AlC i-MAX and SmFeN magnetic powder; S5, the thermoplastic polyether ester elastomer obtained in step S2 and 1 part of the grafted (W 2 / 3 Y 1 / 3 ) 2 AlC i-MAX, 0.5 parts of samarium iron nitrogen magnetic powder and 0.5 parts of carboxyl spherical nano-gold were fed together into a twin-screw extruder with an aspect ratio of 56 for melt blending, extrusion and granulation to obtain an electromagnetic shielding thermoplastic polyether ester elastomer.
[0047] Example 6 S1, placing 60 parts of 2,6-naphthalene diol butanediol, 20 parts of polytetramethylene ether glycol, 0.05 parts of organic titanium zirconium chelate and 20 parts of WHT-6228C in a polymerization kettle filled with nitrogen, and reacting at a constant temperature of 210° C. for 120 min to obtain a prepolymer; S2, drying the low melting point eutectic gallium indium alloy, Fe 2 B 2 The lanthanum oxide and the lanthanum oxide were immersed in a 80°C constant temperature caffeic acid\deionized water solution (caffeic acid and deionized water were mixed in a weight ratio of 1:5) for 8 hours, and then the grafted low melting point eutectic gallium-indium alloy and Fe were obtained after washing with ethanol and filtering and drying. 2 B 2 with lanthanum oxide; S3, at a constant temperature of 60 ° C, first add 1 part of grafted Fe to 20 parts of polytetrahydrofuran ether glycol solvent 2 B 2 Place the mixture under constant temperature and constant speed stirring for 2 hours, then add 1 part of grafted low melting point eutectic gallium-indium alloy and 1 part of grafted lanthanum oxide and stir them under the same environment for 2 hours to obtain a uniformly dispersed polytetrahydrofuran ether diol mixture; S4, when the amount of the alcohol substance obtained by the prepolymerization reaction in step S1 reaches more than 120% of the amount of 2,6-butylene naphthalene diol ester, the polytetrahydrofuran ether diol mixture obtained in step S3 is added into the polymerization kettle in step S1 to carry out a secondary reaction for 0.5 h, and 0.2 parts of antioxidant 1010 are added at the same time; S5, when the viscosity of the mixture in the polymerization kettle in step S4 reaches 5000 At the same time, the nitrogen in the kettle was purged to a vacuum negative pressure of 0.4 MPa, and the temperature was raised to 200°C for a vacuum low-viscosity final polycondensation reaction for 1 hour. The material was discharged, granulated and cooled to obtain an electromagnetic shielding thermoplastic polyether ester elastomer.
[0048] The materials prepared in each embodiment and comparative example were tested for samples, and the performance test standards were as follows: Heat deformation temperature (Tm): GB / T 19466.3-2004; Material melt mass flow rate MFR: GB / T 3682.1-2018; Electromagnetic shielding: The electromagnetic shielding effectiveness of the material is measured in accordance with GB / T30142-2013 "Measurement method for shielding effectiveness of planar electromagnetic shielding materials". The shielding effectiveness of the material is expressed by shielding attenuation. The larger the shielding attenuation value, the better the shielding effectiveness. The field strength when there is a shielding body in the space protection zone is E0 or H0, and the field strength when there is no shielding body is E or H; shielding attenuation represents the attenuation value of the interference field strength through the shielding body, which can be obtained by 20l0|E / E0| or 20l0|H / H0|, and the unit is decibel (dB).
[0049] The performance parameters are shown in Table 3.
[0050] Table 3 Performance test results of materials prepared in various embodiments and comparative examples performance Heat Deflection Temperature / °C MFR / (g / 10min) (230℃, 2.16kg) Shielding effectiveness average value (0.5MHz~20GHz) / dB Peel strength / (N / cm) PC / PET or PC / ABS welding effect Example 1 145.3 23.4 62.6 7.9 firm Comparative Example 1 133.6 25.7 13.4 7.6 Barely firm Example 2 136.7 30.8 53.2 13.7 firm Comparative Example 2 134.8 31.3 21.5 12.9 firm Example 3 152.2 22.5 59.8 12.4 firm Comparative Example 3 150.3 23.4 25.3 11.5 firm Experimental Example 4 149.7 25.9 64.7 12.6 firm Comparative Example 4 144.4 26 55.1 11.9 firm Example 5 150.1 22.7 58.7 12.9 firm Comparative Example 5 147.8 23.9 50.3 10.5 Barely firm Example 6 141.3 25.1 66.2 14.6 firm From the data in Table 3, it can be seen that by introducing liquid metal, MXenes and its derivatives and rare earth magnetic materials through polymerization, a thermoplastic polyether ester elastomer with strong microwave absorption and electromagnetic shielding of wide-band is prepared. Specifically, compared with Comparative Example 1 (liquid metal, MXenes and its derivatives and rare earth magnetic materials are not introduced), Example 1 introduces liquid metal, MXenes and its derivatives and rare earth magnetic materials at the same time while basically keeping the peel strength and MFR unchanged, and the electromagnetic shielding effectiveness of the prepared thermoplastic polyether ester elastomer is significantly improved, and the heat deformation temperature is also improved; compared with Comparative Example 2 (only liquid metal is introduced), Example 1 introduces liquid metal, MXenes and its derivatives and rare earth magnetic materials at the same time while basically keeping the peel strength and MFR unchanged, and the electromagnetic shielding effectiveness of the prepared thermoplastic polyether ester elastomer is improved to a greater extent, and the heat deformation temperature is higher. The electromagnetic shielding effectiveness of Comparative Example 1 is better than that of Comparative Example 2, and both are better than Comparative Example 3 (only MXenes and its derivatives are introduced). The above results show that MXenes and their derivatives and rare earth magnetic materials have good electromagnetic shielding effectiveness and heat resistance for thermoplastic polyether ester elastomers, and the two have a synergistic effect; not only that, the electromagnetic shielding effectiveness of rare earth magnetic materials is better than that of MXenes and their derivatives, which may be related to the fact that the strong magnetic field interference and "blocking" electromagnetic transmission of rare earth magnetic materials are stronger than the reflection, absorption, and multiple refraction electromagnetic effects of MXenes and their derivatives. Experimental Examples 2 to 3 all reached the same conclusion, which will not be repeated one by one. Compared with Comparative Example 4 (only MXenes and their derivatives and rare earth magnetic materials are introduced), the thermoplastic polyether ester elastomer prepared in Example 4 has a substantially unchanged heat deformation temperature and electromagnetic shielding effectiveness, while its MFR and peel strength are significantly improved, and it has certain encapsulation and welding properties. Compared with Comparative Example 5 (using traditional melt blending to introduce liquid metal, MXenes and its derivatives and rare earth magnetic materials), Example 4 uses prepolymerization and premixing vacuum polycondensation reaction to obtain a thermoplastic polyether ester elastomer, while keeping the peel strength, heat deformation temperature and MFR basically unchanged, and the electromagnetic shielding effectiveness is significantly improved, which is related to the distribution and dispersion of MXenes and its derivatives and rare earth magnetic materials.
[0051] Industrial Applicability The thermoplastic polyether ester elastomer composition of the present invention has the characteristics of less introduction of dielectric materials, strong absorption of wide-band microwaves, high electromagnetic reflection absorption and multiple refraction efficiency, and good melt-bonding properties. It is used in 3C electronic products or communication equipment such as laptop computers, GPS, ADSL and mobile phones, as well as wireless routers, cabin wireless transmitters and unmanned aerial vehicles and other rubber-coated or non-rubber-coated fields.
[0052] Although this specification is described according to implementation modes, not every implementation mode includes only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
[0053] Therefore, the above description is only a preferred embodiment of the present application and is not intended to limit the scope of implementation of the present application; that is, all equivalent changes made according to the scope of the claims of the present application are within the protection scope of the claims of the present application.
Claims
1. A thermoplastic polyetherester elastomer with strong broadband microwave absorption and electromagnetic shielding, characterized in that: It is prepared from the following components in parts by weight: 35-90 parts of benzoic acid ester, 10 to 65 parts of polyether alcohol, Catalyst 0.01~0.1 parts, Low melting point polyurethane hot melt adhesive 0-30 parts, 0.2-1 part of liquid metal, MXenes and their derivative materials 0.2-2 parts, 0.2 to 2 parts of rare earth magnetic material, Surface grafting agent 0.01~0.6 parts, 0.2 parts of antioxidant.
2. The thermoplastic polyetherester elastomer according to claim 1, characterized in that The liquid metal is one of liquid nano-silver solution, liquid nano-gold solution, gallium-based liquid metal and its alloy, and bismuth-based liquid metal and its alloy.
3. The thermoplastic polyetherester elastomer according to claim 2, characterized in that The nano-gold in the liquid nano-gold solution is at least one of PEG-wrapped nano-gold particles and BSA-wrapped nano-gold particles.
4. The thermoplastic polyetherester elastomer according to claim 2, characterized in that The gallium-based and alloy liquid metal is one of liquid metal gallium, eutectic gallium-indium alloy, and eutectic gallium-indium-tin alloy, and its melting point is not higher than 100°C.
5. The thermoplastic polyetherester elastomer according to claim 1, characterized in that MXenes and their derivative materials have a Mn+1XnTx structure, where M represents a transition metal site, X represents nitrogen or carbon, n is a natural number from 1 to 4, and Tx represents the two-dimensional transition metal nitride, carbide or carbonitride of the terminal group on the surface of the material, as well as synthetic derivatives based thereon, MAX and its derived MBene materials; the terminal group is -F, -O, -OH or -Cl.
6. The thermoplastic polyetherester elastomer according to claim 1, characterized in that The rare earth magnetic material is at least one of gold-coated iron oxide particles, samarium iron nitrogen magnetic powder, neodymium iron nitrogen magnetic powder, neodymium iron boron magnetic powder, samarium cobalt magnetic powder, aluminum nickel cobalt magnetic powder, ferrite magnetic powder, and rare earth magnetic oxides; and / or the rare earth magnetic oxide is one of lanthanide oxides, scandium oxides, and yttrium oxides.
7. The thermoplastic polyetherester elastomer according to claim 1, characterized in that The surface grafting agent is one of dopamine and its derivatives, and polyphenol compounds, and / or dopamine and its derivatives are one of hydroxy polyethylene glycol dopamine, phenol-dopamine, aldehyde polyethylene glycol dopamine, and polydopamine, and the molecular weight does not exceed 5000.
8. The thermoplastic polyetherester elastomer according to claim 1, characterized in that The catalyst is at least one of tetrabutyl titanate, zirconium tetroxide and zirconium hydroxide.
9. The thermoplastic polyetherester elastomer according to claim 1, characterized in that: Low melting point polyurethane hot melt adhesive is a high melting point low melting point hot melt TPU.
10. The method for preparing a thermoplastic polyetherester elastomer according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Pretreatment of liquid metals, MXenes and their derivatives, and rare earth magnetic materials: The dried liquid metal, MXenes and its derivative materials, and rare earth magnetic materials are immersed in a solution of a surface grafting agent and deionized water in a mass ratio of 1:5, respectively, and a surface grafting reaction is carried out for 4 to 8 hours at a reaction temperature of 50 to 80°C; after being taken out, washed, filtered, and dried, grafted liquid metal, grafted MXenes and its derivative materials, and grafted rare earth magnetic materials are obtained; S2. Add grafted MXenes and their derivative materials to part of the polyether alcohol at a constant temperature of 60 to 100° C., and stir ultrasonically for 0.5 to 2 hours; then add grafted liquid metal and grafted rare earth magnetic material, and continue to stir ultrasonically to obtain a uniform polyether alcohol mother liquor; S3, placing benzoic acid ester, another part of polyether alcohol, catalyst and low melting point polyurethane hot melt adhesive in a polymerization kettle filled with nitrogen for prepolymerization reaction, the reaction temperature is 160-200° C., and the reaction time is 40-120 min; S4. When the amount of the alcohol substance obtained by the prepolymerization reaction reaches 120% of the amount of the benzoate substance, the polyether alcohol mother liquor and the antioxidant are added to the reactor to carry out a secondary reaction at a reaction temperature of 160 to 200° C. for a reaction time of 0.5 to 2 h; S5. When the viscosity of the mixture in the polymerization kettle reaches 4000~6000 At the same time, the nitrogen in the kettle is purged to a vacuum negative pressure of 0.02-0.4 MPa, and the temperature is raised to 190-230°C for a low-viscosity final polycondensation reaction in vacuum for 1-2 hours. The material is discharged and granulated to obtain a thermoplastic polyether ester elastomer with wide-band microwave strong absorption and electromagnetic shielding.
Citation Information
Cited By
Wave-absorbing material and application thereof
CN120414097A
Wave-absorbing material and application thereof
CN120414097B
Thermoplastic elastomer-based foaming composite material with excellent conductivity and electromagnetic shielding performance and preparation method thereof
CN120464051A
Thermoplastic elastomer-based foamed composite material having excellent electrically conductive and electromagnetic shielding properties and method for preparing the same
CN120464051B