Zirconium oxide dispersion liquid as well as preparation method and application thereof

By dispersing nano-zirconia in optical resin, the problem of low refractive index of photo-cured resin is solved, and a zirconium oxide dispersion with excellent rheology and high light transmittance is prepared, which is used to improve the hardness and stability of the optical path adjustment coating. .

CN118725624AActive Publication Date: 2024-10-01SHANDONG SINOCERA FUNCTIONAL MATERIAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410923482.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-01
Estimated Expiration
2044-07-10

AI Technical Summary

Technical Problem

The refractive index of existing photo-curable resins is low and it is difficult to meet the requirements of high light transmittance and rheology, which affects its application in the optical field.

Method used

By dispersing nano-zirconia into optical resin, defining the particle size distribution of zirconia particles (D30≤20nm, D80≤30nm, D95≤100nm), and using surface modifiers and dispersants, we can prepare nano-zirconia particles with excellent rheology and high Translucent zirconia dispersion.

Benefits of technology

The rheological properties and light transmittance of the zirconium oxide dispersion are improved, and the optical path adjustment coating formed has higher hardness and stability, and is suitable for optical communication technology, display panels and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004937373870000151
    Figure BDA0004937373870000151
  • Figure BDA0004937373870000152
    Figure BDA0004937373870000152
  • Figure BDA0004937373870000153
    Figure BDA0004937373870000153
Patent Text Reader

Abstract

The invention discloses zirconium oxide dispersion liquid as well as a preparation method and application thereof, and belongs to the technical field of zirconium oxide materials. The zirconium oxide dispersion liquid comprises a zirconium oxide component, a dispersing agent and a resin component, d30 < = 20 nm, D80 < = 30 nm, and D95 < = 100 nm of a zirconia raw material used in the zirconia component. By controlling D30 < = 20nm and D80 < = 30nm of nano zirconium oxide, the nano particle size in the system can be relatively uniform, the whole particle size distribution is relatively narrow, and the rheological property of the prepared dispersion liquid is relatively excellent. And the nano particles are uniformly and tightly arranged during curing and film forming, so that the hardness after film forming is improved. And zirconium oxide D95 is controlled to be less than or equal to 100nm, so that large particles in the whole dispersion liquid system can be controlled, and the light transmission of the dispersion liquid can be improved. The zirconium oxide dispersion liquid has better rheological property and light transmission, and the obtained film has better film-forming uniformity and film-forming hardness and can be used for adjusting a light path.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of zirconium oxide materials, and in particular to a zirconium oxide dispersion liquid and a preparation method and application thereof. Background Art

[0002] In recent years, high refractive index transparent materials have been used in many fields, such as optical communication technology, photonic computers, display panels, lenses, optical films, optical waveguides, solar cells and light-emitting diodes.

[0003] Optically transparent polymer materials are widely used due to their low cost, good processing performance, and high visible light transmittance. However, the refractive index of most photocurable resins is relatively low, such as acrylate resins, which usually have a refractive index of 1.40 to 1.60. Although the refractive index can be further increased by changing the type and number of resin groups, such as increasing the benzene ring structure, conjugated structure, and π electron structure in the molecule, when a large amount of such structures is contained, the polymer will have light scattering properties and birefringence absorption coefficients, making it unsuitable as an optical material. Therefore, it is usually necessary to add a certain amount of inorganic nanoparticles to the photocurable resin to increase the refractive index of the photocurable resin.

[0004] Nano-zirconia has the advantages of high refractive index, high strength, thermal stability and chemical inertness. Dispersing inorganic nano-zirconia into organic optical resins can not only greatly improve the optical properties of organic resins, but also improve the mechanical properties after film formation. In order to ensure that this zirconium oxide-resin dispersion can play its due functional effect in various optical fields, the dispersion must not only have high light transmittance, but also have good rheological properties to ensure the continuity and stability of the subsequent glue use process (such as inkjet printing, spin coating, roller coating, etc.), and ensure the uniformity and functionality of the coating after curing.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The object of the present invention is to provide a zirconium oxide dispersion and a preparation method and application thereof, so as to solve or improve the above technical problems.

[0007] The present invention can be implemented like this:

[0008] In a first aspect, the present invention provides a zirconium oxide dispersion, which comprises a zirconium oxide component, a dispersant and a resin component;

[0009] Among them, the D of the zirconium oxide raw material used in the zirconium oxide component 30 ≤20nm, D 80 ≤30nm and D 95 ≤100nm.

[0010] In an optional embodiment, the D of the zirconium oxide raw material used in the zirconium oxide component is 30 3nm~20nm, D 80 6nm~30nm and D 95 It is 30nm~100nm.

[0011] In an optional embodiment, the D of the zirconium oxide raw material used in the zirconium oxide component is 30 3.87nm~19.87nm, D 80 6.46nm~29.55nm and D 95 It is 30.05nm~95.05nm.

[0012] In an optional embodiment, the content of the zirconium oxide raw material in the zirconium oxide dispersion is 40 wt % to 75 wt %.

[0013] In an optional embodiment, the content of the zirconium oxide raw material in the zirconium oxide dispersion is 45 wt % to 70 wt %.

[0014] In an optional embodiment, the content of the zirconium oxide raw material in the zirconium oxide dispersion is 50 wt % to 65 wt %.

[0015] In an optional embodiment, the zirconium oxide component is obtained by modifying a zirconium oxide raw material with a surface modifier.

[0016] In an optional embodiment, the amount of the surface modifier used is 1 wt% to 30 wt% of the zirconium oxide raw material.

[0017] In an optional embodiment, the amount of the surface modifier used is 5 wt% to 20 wt% of the zirconium oxide raw material.

[0018] In an optional embodiment, the surface modifier includes at least one of an organic acid compound, a phosphonic acid compound, a coupling agent and a chelating agent.

[0019] In an optional embodiment, the coupling agent is a silane coupling agent.

[0020] In an optional embodiment, the amount of the dispersant used is 1 wt% to 20 wt% of the zirconium oxide raw material.

[0021] In an optional embodiment, the amount of the dispersant used is 5 wt % to 10 wt % of the zirconium oxide raw material.

[0022] In an alternative embodiment, the resin component is an optical resin.

[0023] In an optional embodiment, the resin component is a UV-curable acrylic resin.

[0024] In an optional embodiment, the zirconium oxide dispersion has at least one of the following characteristics:

[0025] Feature 1: Zirconia dispersion at a shear rate of 50s -1 The viscosity value under the condition of is lower than 6000mPa·s;

[0026] Feature 2: Zirconia dispersion at a shear rate of 1000s -1 The viscosity value under the condition of is lower than 4000mPa·s;

[0027] Feature 3: The rheology of the zirconium oxide dispersion is 1.1 to 2.5;

[0028] Feature 4: The transmittance of the zirconium oxide dispersion corresponding to a wavelength of 600nm is not less than 50%;

[0029] Feature 5: The refractive index of the zirconium oxide dispersion is greater than 1.65.

[0030] In a second aspect, the present invention provides a method for preparing a zirconium oxide dispersion as described in any one of the aforementioned embodiments, comprising the following steps: mixing a mixed solution containing an organic solvent, a zirconium oxide component and a dispersant with a resin component, and then removing the organic solvent.

[0031] In an optional embodiment, the content of the zirconium oxide raw material in the mixed solution is 10 wt % to 80 wt %.

[0032] In an optional embodiment, the content of the zirconium oxide raw material in the mixed solution is 20 wt % to 50 wt %.

[0033] In an optional embodiment, the content of the zirconium oxide raw material in the mixed solution is 20 wt % to 30 wt %.

[0034] In an alternative embodiment, the organic solvent includes at least one of alcohols, ketones, ethers, esters, aliphatic hydrocarbons, cycloaliphatic hydrocarbons and aromatics.

[0035] In an optional embodiment, the organic solvent includes at least one of propylene glycol methyl ether, propylene glycol methyl ether acetate, ethyl lactate, toluene, butanone and butyl acetate.

[0036] In a third aspect, the present invention provides an optical path regulating coating, wherein the raw material for preparing the optical path regulating coating comprises the zirconium oxide dispersion of any one of the aforementioned embodiments.

[0037] In an optional embodiment, the raw materials for preparing the optical path regulating coating further include an initiator.

[0038] In an optional embodiment, when the resin component is an ultraviolet light-curable acrylic resin, the initiator is a photoinitiator.

[0039] In an optional embodiment, the amount of the initiator used is 1 wt% to 5 wt% of the zirconium oxide dispersion.

[0040] In an optional embodiment, the method includes the following steps: coating the raw materials for preparing the optical path regulating coating on the surface of the substrate, and curing the coating.

[0041] In an optional embodiment, the light transmittance of the substrate is not less than 89%.

[0042] In an optional embodiment, the light transmittance of the substrate is not less than 90%.

[0043] In alternative embodiments, the substrate comprises polyethylene terephthalate, cellulose triacetate, polycarbonate, or polymethyl methacrylate.

[0044] In an optional embodiment, the light path adjusting coating is used to adjust the light path.

[0045] In an optional embodiment, the light path regulating coating is used in optical communication technology, photonic computers, display panels, lenses, optical films, optical waveguides, solar cells or light emitting diodes.

[0046] The beneficial effects of the present invention include:

[0047] The present invention limits the D of nano zirconium oxide in the zirconium oxide dispersion system. 30 ≤20nm and D 80 ≤30nm, the particle size of the nanoparticles in the zirconium oxide dispersion system can be made relatively uniform, and the particle size distribution of all nanoparticles can be made narrower, thereby obtaining a zirconium oxide dispersion with excellent rheological properties. In addition, the above D 30 and D 80 The nano-zirconia in the above range can make the nano-particles arranged more evenly and tightly when the zirconium oxide dispersion system formed by it is cured into a film, which is beneficial to improve the hardness of the coating after film formation. 30 and D 80 On the basis of the above, the D of nano zirconium oxide is limited. 95 , which can effectively control the content of large particles in the entire zirconium oxide dispersion system, prevent large particles from affecting the light transmittance of the dispersion, and thus help improve the light transmittance of the dispersion. The resulting zirconium oxide dispersion has good rheology and light transmittance, and a high refractive index. The optical path adjustment coating further prepared from the zirconium oxide dispersion has a higher hardness, which is conducive to maintaining the stability and functionality of the product. DETAILED DESCRIPTION

[0048] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0049] The zirconium oxide dispersion provided by the present invention and its preparation method and application are described in detail below.

[0050] The present invention provides a zirconium oxide dispersion liquid, which comprises a zirconium oxide component, a dispersant and a resin component.

[0051] Among them, the D of the zirconium oxide raw material used in the zirconium oxide component 30 ≤20nm, D 80 ≤30nm and D 95 ≤100nm. The above zirconium oxide raw material is nanometer grade.

[0052] For example, the D of the zirconium oxide raw material used in the zirconium oxide component is 30 It can be 20nm, 18nm, 16nm, 14nm, 12nm, 10nm, 8nm, 6nm, 4nm, 2nm or 1nm, etc., or other values ​​within the range of ≤20nm and >0. 80 It can be 30nm, 25nm, 20nm, 18nm, 16nm, 14nm, 12nm, 10nm, 8nm, 6nm, 4nm, 2nm or 1nm, etc., and can also be other values ​​within the range of ≤30nm and >0. 95 It may be 100 nm, 90 nm, 80 nm, 70 nm, 60 nm, 50 nm, 40 nm, 30 nm, 20 nm or 10 nm, etc., or may be other values ​​within the range of ≤100 nm and >0.

[0053] It should be emphasized that in the 30 , D 80 and D 95 When setting, D 30 ≤20nm, D 80 ≤30nm and D 95 ≤100nm.

[0054] In some embodiments, the D of the zirconium oxide raw material used in the zirconium oxide component is 30 3nm~20nm, D 80 6nm~30nm and D 95 In some preferred embodiments, the D of the zirconium oxide raw material used in the zirconium oxide component is 30 nm to 100 nm. 303.87nm~19.87nm, D 80 6.46nm~29.55nm and D 95 It is 30.05nm~95.05nm.

[0055] In the above, the present invention limits the D of nano zirconium oxide in the zirconium oxide dispersion system. 30 ≤20nm and D 80 ≤30nm, the particle size of the nanoparticles in the zirconium oxide dispersion system can be made relatively uniform, and the particle size distribution of all nanoparticles can be made narrower, thereby obtaining a zirconium oxide dispersion with excellent rheological properties. In addition, the above D 30 and D 80 The nano-zirconia in the above range can make the nano-particles arranged more evenly and tightly when the zirconium oxide dispersion system formed by it is cured into a film, which is beneficial to improve the hardness of the coating after film formation. 30 and D 80 On the basis of the above, the D of nano zirconium oxide is limited. 95 , which can effectively control the content of large particles in the entire zirconium oxide dispersion system, prevent large particles from affecting the light transmittance of the dispersion, and thus help improve the light transmittance of the dispersion.

[0056] In the present invention, the crystal form of the zirconium oxide raw material is not limited. When used, the zirconium oxide raw material with a monoclinic, tetragonal or mixed phase crystal form can be used.

[0057] In some embodiments, the content of the zirconium oxide raw material in the zirconium oxide dispersion can be 40wt% to 75wt%, such as 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt% or 75wt%, or other values ​​within the range of 40wt% to 75wt%. In some preferred embodiments, the content of the zirconium oxide raw material in the zirconium oxide dispersion is 45wt% to 70wt%. In some more preferred embodiments, the content of the zirconium oxide raw material in the zirconium oxide dispersion is 50wt% to 65wt%.

[0058] If the content of the zirconium oxide raw material in the zirconium oxide dispersion is lower than 45wt%, the prepared dispersion has a low refractive index, which is not conducive to optical path adjustment; if the content of the zirconium oxide raw material in the zirconium oxide dispersion is higher than 75wt%, the dispersion cannot be prepared.

[0059] In accordance with the above, while satisfying the D 30 , D 80 and D 95 The zirconium oxide dispersion prepared by using zirconium oxide raw materials in the above dosage ratio can have better rheology and higher light transmittance.

[0060] In some embodiments, the zirconium oxide component is obtained by modifying a zirconium oxide raw material with a surface modifier.

[0061] The surface properties of the zirconium oxide raw material can be improved by surface modification of the zirconium oxide raw material, so that groups that are compatible with the resin can be grafted onto the surface of the zirconium oxide raw material.

[0062] The surface modification method is not limited, for example, it can be grinding, heating or mixing and stirring.

[0063] The type of surface modifier is not limited, as long as it can play the role of affinity resin. In some embodiments, the surface modifier may include at least one of organic acid compounds with various types of groups, phosphonic acid compounds, coupling agents and chelating agents.

[0064] In some preferred embodiments, the surface modifier is a silane coupling agent, for example, a silane containing an acrylate group, a (meth)acrylic group, an epoxy group, an alkyl group, an alkoxy group, a vinyl group, a phenyl group, a methacryloxy group, an amino group, a chlorosilyl group, a chloropropyl group or a mercapto group.

[0065] The amount of the surface modifier can be 1wt% to 30wt% of the zirconium oxide raw material, such as 1wt%, 5wt%, 10wt%, 15wt%, 20wt%, 25wt% or 30wt%, etc., or other values ​​within the range of 1wt% to 30wt%. In some preferred embodiments, the amount of the surface modifier is 5wt% to 20wt% of the zirconium oxide raw material.

[0066] In the present invention, the dispersant can play a role in assisting dispersion and wetting. The above-mentioned dispersant can be a commercially available dispersant of various models and types, and each dispersant can be used alone, or a plurality of dispersants can be used in combination. Exemplarily, the dispersant can include at least one of a polyether acid compound, a polyether amine compound, a polyether acid / amine mixture, an ester compound of a phosphoric acid group, and a polyether compound including a phosphoric acid group. The dispersion method can be ultrasound, stirring, grinding, etc., and is not specifically limited.

[0067] In some embodiments, the amount of the dispersant is 1 wt% to 20 wt% of the zirconium oxide raw material, such as 1 wt%, 2 wt%, 5 wt%, 8 wt%, 10 wt%, 12 wt%, 15 wt%, 18 wt% or 20 wt%, etc., and may also be other values ​​within the range of 1 wt% to 20 wt%. In some preferred embodiments, the amount of the dispersant is 5 wt% to 10 wt% of the zirconium oxide raw material.

[0068] In the present invention, the resin component is an optical resin. In some preferred embodiments, the resin component is a UV-curable acrylic resin, which may exemplarily but not limitatively include at least one of benzyl acrylate, benzyl methacrylate, phenyl acrylate, diphenyl acrylate, biphenyl acrylate, phenoxybenzyl acrylate, 3-phenoxybenzyl acrylate, phenyl methacrylate, biphenyl methacrylate, 4-nitrophenyl methacrylate, 4-nitrobenzyl methacrylate, 2-chlorophenyl acrylate, 4-chlorophenyl acrylate, 2-chlorophenyl methacrylate, biphenylmethanol acrylate, 4-chlorophenyl methacrylate, o-phenylphenol ethyl acrylate, bisphenol diacrylate, hydroxyethyl acrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate.

[0069] In some embodiments, the amount of the resin can be obtained by subtracting the total content of the zirconium oxide raw material, the surface modifier and the dispersant in the zirconium oxide dispersion from 100%.

[0070] In some embodiments, the zirconium oxide dispersion is heated at a shear rate of 50 s -1 The viscosity value under the conditions is lower than 6000 mPa·s, for example, it can be 196 mPa·s to 5756 mPa·s.

[0071] In some embodiments, the zirconium oxide dispersion is subjected to a shear rate of 1000 s -1 The viscosity value under the conditions is lower than 4000 mPa·s, for example, it can be 154 mPa·s to 3350 mPa·s.

[0072] In some embodiments, the rheological property of the zirconium oxide dispersion is 1.1 to 2.5, for example, 1.167 to 2.456.

[0073] In some embodiments, the transmittance of the zirconium oxide dispersion corresponding to a wavelength of 600 nm is not less than 50%, for example, it may be 51.4% to 65.2%.

[0074] In some embodiments, the refractive index of the zirconium oxide dispersion is >1.65, further >1.67, and further >1.70.

[0075] Accordingly, the present invention also provides a method for preparing the above zirconium oxide dispersion, which comprises the following steps: mixing a mixed solution containing an organic solvent, a zirconium oxide component and a dispersant with a resin component, and then removing the organic solvent.

[0076] In some embodiments, the zirconium oxide raw material is first modified with a surface modifier to obtain a zirconium oxide component; the zirconium oxide component is mixed with a dispersant and an organic solvent to obtain a mixed solution; the mixed solution is mixed with a resin component, and the organic solvent is removed to obtain a zirconium oxide dispersion.

[0077] In some embodiments, the content of the zirconium oxide raw material in the mixed solution can be 10wt% to 80wt%, such as 10wt%, 20wt%, 30wt%, 40wt%, 50wt%, 60wt%, 70wt% or 80wt%, etc., or other values ​​within the range of 10wt% to 80wt%. In some preferred embodiments, the content of the zirconium oxide raw material in the mixed solution is 20wt% to 50wt%, and in some more preferred embodiments, the content of the zirconium oxide raw material in the mixed solution is 20wt% to 30wt%.

[0078] In some embodiments, the amount of the organic solvent used can be obtained by subtracting the total content of the zirconium oxide raw material, the surface modifier, and the dispersant in the mixed solution from 100%.

[0079] The present invention does not specifically limit the organic solvent. In some embodiments, the organic solvent may include at least one of alcohols, ketones, ethers, esters, aliphatic hydrocarbons, cycloaliphatic hydrocarbons and aromatics. In some preferred embodiments, the organic solvent may include at least one of propylene glycol methyl ether, propylene glycol methyl ether acetate, ethyl lactate, toluene, butanone and butyl acetate.

[0080] The present invention does not specifically limit the method for removing the organic solvent. For example but not limitation, a rotary evaporator or other vacuum distillation device may be used for removal.

[0081] In addition, the present invention also provides an optical path regulating coating, and the raw materials for preparing the optical path regulating coating include the above-mentioned zirconium oxide dispersion.

[0082] Furthermore, the raw materials for preparing the optical path regulating coating also include an initiator.

[0083] In an optional embodiment, when the resin component is an ultraviolet light-curable acrylic resin, the initiator is a photoinitiator.

[0084] The present invention does not specifically limit the photoinitiator. In some embodiments, the photoinitiator may include at least one of cationic photoinitiators such as diazonium salts, sulfonium salts and imidazoles. In some other embodiments, the photoinitiator may also include at least one of free radical photoinitiators such as phosphorus, triazine, benzophenone, benzoin, oxime, acetone, aminoketone, ketone, anthraquinone and aromatic phosphine oxide compounds. In some preferred embodiments, the photoinitiator may include at least one of TPO, 1173, 184 and 907.

[0085] In some embodiments, the amount of photoinitiator used can be 1wt% to 5wt% of the zirconium oxide dispersion, such as 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt% or 5wt%, etc., or it can be other values ​​within the range of 1wt% to 5wt%.

[0086] Correspondingly, the present invention also provides a method for preparing the above-mentioned optical path regulating coating, comprising the following steps: coating the raw materials for preparing the optical path regulating coating on the surface of the substrate, and curing.

[0087] The coating method is not particularly limited, and exemplary but not limiting methods include roller coating, spray coating, flow coating, or spin coating.

[0088] The coating substrate is also not particularly limited, and is preferably a substrate having a high transmittance. In some embodiments, the light transmittance of the substrate is not less than 89%, preferably not less than 90%. In some specific embodiments, the substrate may include polyethylene terephthalate, triacetyl cellulose, polycarbonate or polymethyl methacrylate.

[0089] The curing method can be achieved by using a mercury lamp, LED and the like, for example but not limited thereto.

[0090] The optical path adjustment coating has a relatively high hardness.

[0091] In addition, the present invention also provides an application of the above-mentioned optical path adjustment coating, and the optical path adjustment coating can be used to adjust the optical path.

[0092] In some embodiments, the optical path regulating coating can be used in optical communication technology, photonic computers, display panels, lenses, optical films, optical waveguides, solar cells or light emitting diodes, wherein the optical film includes an anti-reflection film.

[0093] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0094] Example 1

[0095] The present invention provides an optical path regulating coating, and the preparation method thereof comprises:

[0096] Step 1: Use 5.1g of silane coupling agent 3-(methacryloyloxy)propyltrimethoxysilane to 51g of zirconium oxide raw material powder (D 30 16.85nm, D 80 is 21.98nm and D 95The modified zirconium oxide was modified by ball milling and dispersion in an organic solvent of propylene glycol methyl ether using 2.55 g of dispersant BYK-111 to obtain a mixed solution. The content of the zirconium oxide raw material powder in the mixed solution was 30 wt%.

[0097] Step 2: 41.35 g of 3-phenylbenzyl acrylate was added to the above mixed solution as a resin component, and propylene glycol methyl ether was removed by a rotary evaporator to obtain a zirconium oxide dispersion with a refractive index RI>1.65.

[0098] Step 3: Add 2 wt % of the photoinitiator TPO to the above zirconium oxide dispersion, and then apply it on PET for photocuring to form a film to obtain a light path regulating coating.

[0099] Example 2

[0100] The present invention provides an optical path regulating coating, and the preparation method thereof comprises:

[0101] Step 1: Use 5.8g of silane coupling agent 3-(methacryloyloxy)propyltrimethoxysilane to 58g of zirconium oxide raw material powder (D 30 9.53nm, D 80 is 15.28nm and D 95 The modified zirconium oxide was modified by ball milling and dispersion in an organic solvent of propylene glycol methyl ether using 2.9 g of dispersant BYK-111 to obtain a mixed solution. The content of the zirconium oxide raw material powder in the mixed solution was 30 wt%.

[0102] Step 2: 33.3 g of 3-phenylbenzyl acrylate was added to the above mixed solution as a resin component, and propylene glycol methyl ether was removed by a rotary evaporator to obtain a zirconium oxide dispersion with a refractive index RI>1.67.

[0103] Step 3: Add 2 wt % of the photoinitiator TPO to the above zirconium oxide dispersion, and then apply it on PET for photocuring to form a film to obtain a light path regulating coating.

[0104] Example 3

[0105] The present invention provides an optical path regulating coating, and the preparation method thereof comprises:

[0106] Step 1: Use 6.2g of silane coupling agent 3-(methacryloyloxy)propyltrimethoxysilane to 62g of zirconium oxide raw material powder (D 30 19.54nm, D 80 is 28.98nm and D 95The modified zirconium oxide was modified by ball milling and dispersion in an organic solvent of propylene glycol methyl ether using 3.1 g of dispersant BYK-111 to obtain a mixed solution. The content of the zirconium oxide raw material powder in the mixed solution was 30 wt%.

[0107] Step 2: 28.7 g of 3-phenylbenzyl acrylate was added to the above mixed solution as a resin component, and propylene glycol methyl ether was removed by a rotary evaporator to obtain a zirconium oxide dispersion with a refractive index RI>1.70.

[0108] Step 3: Add 2 wt % of the photoinitiator TPO to the above zirconium oxide dispersion, and then apply it on PET for photocuring to form a film to obtain a light path regulating coating.

[0109] Example 4

[0110] The difference between this embodiment and embodiment 1 is that: D of the zirconium oxide raw material powder 30 13.48nm, D 80 is 17.20nm and D 95 The particle size is 35.51 nm; the dispersant is BYK-180.

[0111] The refractive index RI of the zirconium oxide dispersion of this embodiment is >1.65.

[0112] Example 5

[0113] The difference between this embodiment and embodiment 2 is that: D of the zirconium oxide raw material powder 30 7.63nm, D 80 is 10.28nm and D 95 The particle size is 33.46 nm; the dispersant is BYK-180.

[0114] The refractive index RI of the zirconium oxide dispersion of this embodiment is >1.67.

[0115] Example 6

[0116] The difference between this embodiment and embodiment 3 is that: D of the zirconium oxide raw material powder 30 3.87nm, D 80 is 6.46nm and D 95 The particle size is 30.05 nm; the dispersant is BYK-180.

[0117] The refractive index RI of the zirconium oxide dispersion of this embodiment is >1.70.

[0118] Example 7

[0119] The difference between this embodiment and embodiment 1 is that: D of the zirconium oxide raw material powder 30 17.45nm, D80 is 27.58nm and D 95 The particle size is 38.36 nm; the silane coupling agent is (2-methylallyloxy)trimethylsilane; and the dispersant is BYK-9010.

[0120] The refractive index RI of the zirconium oxide dispersion of this embodiment is >1.65.

[0121] Example 8

[0122] The difference between this embodiment and embodiment 2 is that: D of the zirconium oxide raw material powder 30 18.37nm, D 80 is 29.55nm and D 95 The nanostructured carbon fiber is 95.05 nm; the silane coupling agent is (2-methylallyloxy)trimethylsilane; and the dispersant is BYK-9010.

[0123] The refractive index RI of the zirconium oxide dispersion of this embodiment is >1.67.

[0124] Example 9

[0125] The difference between this embodiment and embodiment 3 is that: D of the zirconium oxide raw material powder 30 19.87nm, D 80 is 28.46nm and D 95 The nanostructured carbon fiber is 80.39 nm; the silane coupling agent is (2-methylallyloxy)trimethylsilane; and the dispersant is BYK-9010.

[0126] The refractive index RI of the zirconium oxide dispersion of this embodiment is >1.70.

[0127] Comparative Example 1

[0128] The difference between this comparative example and Example 1 is that the D of the zirconium oxide raw material powder is 30 22.77nm, D 80 is 33.96nm and D 95 It is 108.25nm.

[0129] Comparative Example 2

[0130] The difference between this comparative example and Example 2 is that: D of the zirconium oxide raw material powder 30 22.77nm, D 80 is 33.96nm and D 95 It is 112.52nm.

[0131] Comparative Example 3

[0132] The difference between this comparative example and Example 3 is that the D of the zirconium oxide raw material powder is 30 22.77nm, D80 is 33.96nm and D 95 It is 123.56nm.

[0133] Comparative Example 4

[0134] The difference between this comparative example and Example 4 is that the D of the zirconium oxide raw material powder is 30 28.32nm, D 80 is 37.13m and D 95 It is 128.46nm.

[0135] Comparative Example 5

[0136] The difference between this comparative example and Example 5 is that the D of the zirconium oxide raw material powder is 30 28.32nm, D 80 is 37.13nm and D 95 It is 135.46nm.

[0137] Comparative Example 6

[0138] The difference between this comparative example and Example 6 is that: D of the zirconium oxide raw material powder is 30 28.32nm, D 80 is 37.13nm and D 95 It is 141.46nm.

[0139] Comparative Example 7

[0140] The difference between this comparative example and Example 7 is that the D of the zirconium oxide raw material powder is 30 32.92nm, D 80 is 40.56nm and D 95 It is 146.23nm.

[0141] Comparative Example 8

[0142] The difference between this comparative example and Example 8 is that the D of the zirconium oxide raw material powder is 30 32.92nm, D 80 is 40.56nm and D 95 It is 147.23nm.

[0143] Comparative Example 9

[0144] The difference between this comparative example and Example 9 is that the D of the zirconium oxide raw material powder is 30 32.92nm, D 80 is 40.56nm and D 95 It is 156.23nm.

[0145] Comparative Example 10

[0146] The difference between this comparative example and Example 1 is that the D of the zirconium oxide raw material powder is 30 18.11nm, D 80 is 32.54nm and D 95 It is 108.29nm.

[0147] Comparative Example 11

[0148] The difference between this comparative example and Example 1 is that the D of the zirconium oxide raw material powder is 30 23.62nm, D 80 is 28.74nm and D 95 It is 105.36nm.

[0149] Comparative Example 12

[0150] The difference between this comparative example and Example 1 is that the D of the zirconium oxide raw material powder is 30 27.52nm, D 80 is 36.88nm and D 95 It is 96.49nm.

[0151] Comparative Example 13

[0152] The difference between this comparative example and Example 1 is that the D of the zirconium oxide raw material powder is 30 17.44nm, D 80 is 27.62nm and D 95 It is 107.41nm.

[0153] Comparative Example 14

[0154] The difference between this comparative example and Example 1 is that the D of the zirconium oxide raw material powder is 30 18.36nm, D 80 is 32.59nm and D 95 It is 93.72nm.

[0155] Comparative Example 15

[0156] The difference between this comparative example and Example 1 is that the D of the zirconium oxide raw material powder is 30 22.92nm, D 80 is 28.98nm and D 95 It is 96.66nm.

[0157] Comparative Example 16

[0158] The difference between this comparative example and Example 1 is that the pore volume of the zirconium oxide raw material powder is 0.0372 cm 3 / g, pore size is 0.8645nm, average particle size is 10nm, D 30 18.22nm, D80 is 36.54nm and D 95 It is 110.32nm.

[0159] Test example

[0160] ①. The zirconium oxide dispersions prepared in Examples 1 to 9 and Comparative Examples 1 to 16 were subjected to the following tests:

[0161] A. At a shear rate of 50 s -1 The viscosity value is measured under the conditions of mPa·s;

[0162] B. At a shear rate of 1000s -1 The viscosity value is measured under the conditions of mPa·s;

[0163] C. Determine rheological properties. The value of rheological properties = shear rate of 50s -1 The viscosity value measured under the conditions of / shear rate is 1000s -1 The viscosity value is measured under the conditions of

[0164] D. Measure the transmittance at a wavelength of 600nm in %.

[0165] ②. The optical path adjustment coatings prepared in Examples 1 to 9 and Comparative Examples 1 to 16 were subjected to the following tests: Hardness test was performed according to GBT6739-1996 Coating Hardness Pencil Test Method.

[0166] The above test results are shown in Tables 1 to 3.

[0167] Table 1 Test results

[0168]

[0169] Table 2 Test results

[0170]

[0171] Table 3 Test results

[0172]

[0173] It can be seen from Tables 1 to 3 that the zirconium oxide dispersions prepared in Examples 1 to 9 have better rheology and light transmittance and a higher refractive index than those prepared in Comparative Examples 1 to 16. Moreover, the optical path adjustment coatings prepared in Examples 1 to 9 have a higher hardness than those prepared in Comparative Examples 1 to 16, which is beneficial to maintaining the stability and functionality of the product.

[0174] In summary, the present invention limits the D of nano zirconium oxide in the zirconium oxide dispersion system. 30 ≤20nm and D80 ≤30nm, the particle size of the nanoparticles in the zirconium oxide dispersion system can be made relatively uniform, and the particle size distribution of all nanoparticles can be made narrower, thereby obtaining a zirconium oxide dispersion with excellent rheological properties. In addition, the above D 30 and D 80 The nano-zirconia in the above range can make the nano-particles arranged more evenly and tightly when the zirconium oxide dispersion system formed by it is cured into a film, which is beneficial to improve the hardness of the coating after film formation. 30 and D 80 On the basis of the above, the D of nano zirconium oxide is limited. 95 , which can effectively control the content of large particles in the entire zirconium oxide dispersion system, prevent large particles from affecting the light transmittance of the dispersion, and thus help improve the light transmittance of the dispersion. The resulting zirconium oxide dispersion has good rheology and light transmittance, and a high refractive index. The optical path adjustment coating further prepared from the zirconium oxide dispersion has a higher hardness, which is conducive to maintaining the stability and functionality of the product.

[0175] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A zirconium oxide dispersion, characterized in that: The zirconium oxide dispersion comprises a zirconium oxide component, a dispersant and a resin component; Wherein, the D of the zirconium oxide raw material used in the zirconium oxide component is 30 ≤20nm, D 80 ≤30nm and D 95 ≤100nm.

2. The zirconium oxide dispersion according to claim 1, characterized in that D of the zirconium oxide raw material used in the zirconium oxide component 30 3nm~20nm, D 80 6nm~30nm and D 95 It is 30nm~100nm.

3. The zirconium oxide dispersion according to claim 1 or 2, characterized in that: The content of the zirconium oxide raw material in the zirconium oxide dispersion is 40 wt % to 75 wt %.

4. The zirconium oxide dispersion according to claim 1 or 2, characterized in that: The zirconium oxide component is obtained by modifying the zirconium oxide raw material with a surface modifier; Preferably, the surface modifier is used in an amount of 1 wt% to 30 wt% of the zirconium oxide raw material; Preferably, the surface modifier includes at least one of an organic acid compound, a phosphonic acid compound, a coupling agent and a chelating agent.

5. The zirconium oxide dispersion according to claim 1 or 2, characterized in that: The amount of the dispersant is 1wt% to 20wt% of the zirconium oxide raw material; Alternatively, the resin component is an optical resin.

6. The zirconium oxide dispersion according to claim 1 or 2, characterized in that: The zirconium oxide dispersion has at least one of the following characteristics: Feature 1: The zirconium oxide dispersion is at a shear rate of 50s -1 The viscosity value under the condition of is lower than 6000mPa·s; Feature 2: The zirconium oxide dispersion is at a shear rate of 1000s -1 The viscosity value under the condition of is lower than 4000mPa·s; Feature 3: The rheology of the zirconium oxide dispersion is 1.1 to 2.5; Feature 4: The transmittance of the zirconium oxide dispersion corresponding to a wavelength of 600 nm is not less than 50%; Feature 5: The refractive index of the zirconium oxide dispersion is greater than 1.

65.

7. A method for preparing a zirconium oxide dispersion according to any one of claims 1 to 6, characterized in that: The following steps are involved: mixing a mixed solution containing an organic solvent, a zirconium oxide component and a dispersant with a resin component, and then removing the organic solvent; Preferably, the content of the zirconium oxide raw material in the mixed solution is 10wt% to 80wt%; Preferably, the organic solvent includes at least one of alcohols, ketones, ethers, esters, aliphatic hydrocarbons, cycloaliphatic hydrocarbons and aromatics.

8. A light path adjustment coating, characterized in that: The raw material for preparing the optical path adjustment coating includes the zirconium oxide dispersion according to any one of claims 1 to 6; Preferably, the raw materials for preparing the optical path regulating coating further include an initiator; Preferably, the amount of the initiator is 1 wt% to 5 wt% of the zirconium oxide dispersion; Preferably, the hardness of the optical path regulating coating is 2B grade.

9. A method for preparing the optical path regulating coating according to claim 8, characterized in that: The method comprises the following steps: coating the raw materials for preparing the optical path regulating coating on the surface of the substrate and curing the coating; Preferably, the light transmittance of the substrate is not less than 89%; Preferably, the substrate comprises polyethylene terephthalate, cellulose triacetate, polycarbonate or polymethyl methacrylate.

10. An application of the optical path regulating coating as claimed in claim 8, characterized in that: The optical path adjustment coating is used to adjust the optical path; Preferably, the optical path regulating coating is used in optical communication technology, photonic computers, display panels, lenses, optical films, optical waveguides, solar cells or light emitting diodes.

Citation Information

Patent Citations

  • Metal oxide particle dispersion, composition containing metal oxide particles, coating film, and display device

    CN106661362A

  • Photo-curable nano-zirconia dispersion liquid, preparation method thereof and optical film

    CN114736548A

  • Zirconia particle dispersion liquid, its manufacturing method and photocurable composition

    JP2005161111A