Substrate-free ice microneedle and preparation method thereof

Through the preparation method of base-free ice microneedles, the use of metal core and insulation material wrapping technology solves the problems of difficult demoulding and rapid melting of ice microneedles, achieving more efficient freezing and a more stable structure.

CN118750751APending Publication Date: 2024-10-11GUANGDONG UNIV OF TECH
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410847181.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing ice microneedles are difficult to demold and tend to melt quickly after being taken out of the storage environment.

Method used

A substrate-free ice microneedle preparation method is used, by processing the metal core and wrapping it with thermal insulation material, combining the PDMS microneedle mold and polymer solution freezing to prepare ice microneedles. The metal core serves as a cold source to slow down the melting rate of the ice microneedle.

Benefits of technology

It shortens the freezing time of the ice microneedles, improves the ease of demoulding, and prevents the ice microneedles from melting quickly after removal, ensuring its mechanical strength and integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118750751A_ABST
    Figure CN118750751A_ABST
Patent Text Reader

Abstract

The invention discloses a substrate-free ice microneedle and a preparation method thereof, and belongs to the technical field of ice microneedles, and the preparation method comprises the following preparation steps: (1) processing a metal core according to the size of a PDMS microneedle mold, and wrapping the metal core with a thermal insulation material; and (2) pretreating the metal core wrapped by the thermal insulation material, then dissolving polymer powder to prepare a solution, pouring the solution into the PDMS microneedle mold groove, carrying out vacuumizing treatment to remove bubbles, after the PDMS microneedle mold groove is filled with the solution, putting the pretreated metal core wrapped by the thermal insulation material into the bottom surface of the PDMS microneedle mold groove, and finally, freezing the metal core and the PDMS microneedle mold groove in a refrigerator to obtain the PDMS microneedle mold. The ice microneedle is obtained. Therefore, by adopting the substrate-free ice microneedle and the preparation method thereof, the problems that in the prior art, the ice microneedle is difficult to demould and is easy to melt quickly after being taken out from a storage environment are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of ice microneedles, and in particular, relates to a substrate-free ice microneedle and a preparation method thereof. Background Art

[0002] Microneedle patch is a micron-scale medical device. As a new type of transdermal drug delivery method, microneedles have the advantages of minimally invasive and painless drug delivery. They can enhance the skin's permeability to drugs, especially macromolecular drugs, and can also achieve controlled release of drugs. Microneedles can significantly improve the efficiency of transdermal drug delivery by directly penetrating the skin and creating reversible microchannels to reduce pain. Moreover, microneedles allow patients to administer drugs by themselves, which brings great convenience. Ice microneedles can deliver living cells and active substances into the body to overcome the shortcomings of polymer microneedles that cannot transport active substances, hollow microneedles that are prone to clogging, and needle tips that are prone to brittle fracture. In addition, ice microneedles do not affect the activity and proliferation ability of organisms.

[0003] The preparation of ice microneedles in current research requires ultra-low temperature transportation and storage conditions. For example, ice microneedles prepared by the reverse molding method need to be frozen at -80°C for 4 hours to ensure that the ice microneedles have sufficient mechanical strength to puncture the skin for drug molecule delivery. However, there are still problems such as difficulty in demolding and rapid melting of ice microneedles after being taken out of the storage environment. Therefore, there is an urgent need for an ice microneedle that is easier to demold and does not melt quickly. Summary of the invention

[0004] The purpose of the present application is to provide a substrate-free ice microneedle and a preparation method thereof, so as to solve the problem in the prior art that the ice microneedle is difficult to demould and tends to melt quickly after being taken out of the storage environment.

[0005] The present application provides a method for preparing substrate-free ice microneedles, comprising the following preparation steps:

[0006] (1) processing a metal core according to the size of the PDMS microneedle mold, and wrapping the metal core with a heat-insulating material to obtain a metal core wrapped with a heat-insulating material;

[0007] (2) The metal core wrapped with the thermal insulation material is pretreated, and then the polymer powder is dissolved to make a solution, which is poured into the groove of the PDMS microneedle mold and vacuumed to remove bubbles. After the solution fills the groove of the PDMS microneedle mold, the metal core wrapped with the pretreated thermal insulation material is placed on the bottom surface of the groove of the PDMS microneedle mold. Finally, both are placed in a refrigerator to freeze, thereby obtaining ice microneedles.

[0008] Preferably, the thermal insulation material is one or more of foam plastic, polyurethane foam, polystyrene foam, thermal insulation paper, foam glass, and aerogel.

[0009] Preferably, the pretreatment in step (2) is to place the metal core wrapped with the thermal insulation material into a refrigerator.

[0010] Preferably, the soluble polymer includes one or more of sodium hyaluronate, carboxymethyl cellulose, hydroxypropyl methyl cellulose, sodium alginate, chitosan, polycaprolactone, polyvinyl alcohol, polyvinyl pyrrolidone, silk fibroin, chondroitin sulfate, polyethylene glycol diacrylate, methacrylate gelatin, trehalose, polylactic acid-glycolic acid copolymer, galactose, dextrin, and maltose.

[0011] Preferably, the freezing temperature of the refrigerator is -20°C to -80°C, and the freezing time of the refrigerator is 10-240 minutes.

[0012] Preferably, the metal core includes one or more materials of stainless steel, titanium alloy, aluminum alloy, nickel-titanium alloy, and copper alloy.

[0013] The present invention also provides an ice microneedle prepared according to the above-mentioned method for preparing substrate-free ice microneedles.

[0014] Therefore, the present application adopts the above-mentioned substrate-free ice microneedle and preparation method thereof, which has the following beneficial effects:

[0015] Metal has good thermal conductivity. When a metal below zero degrees comes into contact with water, the heat in the water will be transferred through the metal and the temperature will drop rapidly. The metal surface is usually hydrophilic because it carries chemical substances such as oxides on its surface. These substances attract water molecules, making the metal surface hydrophilic. In a low-temperature environment, the aqueous solution freezes on the metal surface and adheres firmly. When the ice microneedles are taken out of the storage environment, the metal can be used as a cold source to cool the ice microneedles and slow down the melting rate of the ice microneedles. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a flow chart of the preparation of ice microneedles of this application;

[0017] Figure 2 is a structural diagram of the metal core and the PDMS microneedle mold of Example 1;

[0018] Figure 3 The structure diagram of the ice microneedle obtained in Example 1, wherein a is the structure diagram and b is the ice microneedle diagram under a microscope;

[0019] Figure 4 It is a comparison chart of melting speed of Example 2 and Comparative Example 1;

[0020] Figure 5 It is a demoulding difficulty comparison diagram of Example 2 and Comparative Example 2; wherein, Figure a is a demoulding difficulty diagram of Example 2, and Figure b is a demoulding difficulty diagram of Comparative Example 2;

[0021] Figure 6 It is a comparison diagram of the microstructures of Example 2 and Comparative Example 2, wherein a corresponds to Example 2, and b corresponds to Comparative Example 2; in Figure a, the structure of the ice microneedle is intact after demolding; in Figure b, the ice microneedle is demolded using tweezers, and a portion of the microneedle base is melted by the tweezers.

[0022] 1. Thermal insulation material; 2. Metal core; 3. Solution; 4. PDMS microneedle mold. DETAILED DESCRIPTION

[0023] The present application provides a method for preparing substrate-free ice microneedles, comprising the following preparation steps:

[0024] (1) According to the size of the PDMS microneedle mold 4, the metal core 2 is processed, and the metal core 2 is wrapped with a heat-insulating material 1; during the subsequent freezing process, the heat-insulating material 1 can effectively reduce the heat exchange between the metal core 2 and the outside, thereby ensuring that the metal core 2 remains at a low temperature during the entire freezing process;

[0025] (2) placing the metal core 2 wrapped by the thermal insulation material 1 into a refrigerator, then dissolving the polymer powder to prepare a solution 3, pouring it into the groove of the PDMS microneedle mold 4, and performing a vacuum treatment to remove bubbles. After the solution 3 fills the groove of the PDMS microneedle mold 4, the metal core 2 wrapped by the pretreated thermal insulation material 1 is placed on the bottom surface of the groove of the PDMS microneedle mold 4, and finally both are placed in a refrigerator to freeze to obtain ice microneedles; the thermal insulation material 1 is one or more of foam plastic, polyurethane foam, polystyrene foam, insulation paper, foam glass, and aerogel; the wrapping of the thermal insulation material 1 can effectively reduce the metal in The temperature rises during the insertion process, and the polymer powder is one or more of sodium hyaluronate, carboxymethyl cellulose, hydroxypropyl methyl cellulose, sodium alginate, chitosan, polycaprolactone, polyvinyl alcohol, polyvinyl pyrrolidone, silk fibroin, chondroitin sulfate, polyethylene glycol diacrylate, methacrylate gelatin, trehalose, polylactic acid-glycolic acid copolymer, galactose, dextrin, and maltose; the freezing temperature of the refrigerator is -20°C to -80°C, and the freezing time of the refrigerator is 10-240 minutes; the metal core includes one or more of stainless steel, titanium alloy, aluminum alloy, nickel-titanium alloy, and copper alloy.

[0026] The present invention also provides an ice microneedle prepared according to the above-mentioned method for preparing substrate-free ice microneedles.

[0027] Example 1

[0028] A PDMS mold with a microneedle body height of 1000 μm, a bottom diameter of 700 μm, and an area of ​​9×9 mm was selected, and a 304 stainless steel plate was cut into a metal core 2 of 9×9×20 mm using a laser processing machine, and the metal core 2 was wrapped with polyurethane foam;

[0029] Preparation of ice microneedles: First, place the metal core 2 wrapped in polyurethane foam in a refrigerator and freeze it for 1 hour in advance, then dissolve the hyaluronic acid powder into a 10% hyaluronic acid solution 3, pour it into the PDMS mold groove, and vacuum it to remove bubbles. After the solution 3 fills the mold groove, add the metal core 2 wrapped in polyurethane foam so that the metal contacts the bottom of the mold groove, and finally put it in a refrigerator and freeze it at -20°C for 15 minutes to obtain hyaluronic acid ice microneedles.

[0030] Example 2

[0031] Preparation of metal core 2-PDMS combined mold: Select a PDMS mold with a microneedle body height of 1000 μm, a bottom diameter of 800 μm, and an area of ​​9x9 mm, use a laser processing machine to cut a 304 stainless steel plate into a metal core 2 of 9x9x20 mm, and wrap the metal core 2 with polystyrene foam;

[0032] Preparation of ice microneedles: First, the metal core 2 wrapped in polystyrene foam is placed in a refrigerator and frozen for 1 hour in advance. Then, the sodium alginate powder is dissolved into a 5% sodium alginate solution 3, poured into the PDMS mold groove, and vacuumed to remove bubbles. After the solution 3 fills the mold groove, the metal core 2 wrapped in polystyrene foam is added so that the metal contacts the bottom surface of the mold groove. Finally, it is placed in a refrigerator and frozen at -20°C for 30 minutes to obtain sodium alginate ice microneedles.

[0033] Example 3

[0034] A PDMS mold with a microneedle body height of 1000 μm, a bottom diameter of 700 μm, and an area of ​​9×9 mm was selected, and an aluminum alloy was cut into a metal core 2 of 9×9×20 mm using a laser processing machine, and the metal core 2 was wrapped with polyurethane foam;

[0035] Preparation of ice microneedles: First, the metal core 2 wrapped in polyurethane foam is placed in a refrigerator and frozen for 1 hour in advance. Then, the hyaluronic acid powder is dissolved into a 10% hyaluronic acid solution 3, poured into the PDMS mold groove, and vacuumed to remove bubbles. After the solution 3 fills the mold groove, the metal core 2 wrapped in polyurethane foam is added so that the metal contacts the bottom of the mold groove. Finally, it is placed in a refrigerator and frozen at -80°C for 240 minutes to obtain hyaluronic acid ice microneedles.

[0036] Comparative Example 1

[0037] Preparation of metal core 2-PDMS combination mold: Select a PDMS mold with a microneedle body height of 1000μm, a bottom diameter of 800μm, and an area of ​​9x9mm, and use a laser processing machine to cut the 304 stainless steel plate into a metal core 2 of 9x9x20mm. The outside of the metal core in this comparative example is not wrapped with foam plastic.

[0038] Preparation of ice microneedles: First, place the metal core 2 in a refrigerator and freeze it for 1 hour. Then, dissolve the sodium alginate powder into a 5% sodium alginate solution 3, pour it into the groove of the PDMS mold, and perform vacuum treatment to remove bubbles. After the solution 3 fills the groove of the mold, add the metal core 2 so that the metal contacts the bottom surface of the mold groove. Finally, place it in a refrigerator and freeze it at -20°C for 30 minutes to obtain sodium alginate ice microneedles. The melting rate is as follows: Figure 4 As shown in Figure a, the ice microneedle can be successfully demolded by lifting it up with your hand; in Figure b, the ice microneedle needs to be lifted out with tweezers, and the tweezers need to be frozen in advance, otherwise the ice microneedle will melt when it touches it, which makes the operation difficult and easily destroys the integrity of the ice microneedle.

[0039] Comparative Example 2

[0040] Sodium alginate powder was dissolved into a 5% sodium alginate solution 3, which was poured into the groove of the PDMS mold and vacuumed to remove bubbles. After the solution 3 filled the groove of the mold, it was placed in a refrigerator and frozen at -20°C for 30 minutes to obtain sodium alginate ice microneedles. Figure 5 As shown in Figure a, the ice microneedle has a complete structure after demolding; Figure b shows that the ice microneedle is demolded using tweezers, and a part of the microneedle base is melted by the tweezers.

[0041] Therefore, the present application provides a substrate-free ice microneedle and a preparation method thereof, which reduces the freezing time required for preparing the ice microneedle and solves the problems of demolding difficulty and rapid melting of the ice microneedle after being taken out of the storage environment.

[0042] In the description of this specification, the description with reference to the terms "an experimental example", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the experimental example or example are included in at least one experimental example or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same experimental example or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more experimental examples or examples in a suitable manner.

[0043] Finally, it should be noted that the above experimental examples are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred experimental examples, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing substrate-free ice microneedles, characterized in that: The method comprises the following preparation steps: (1) processing a metal core according to the size of the PDMS microneedle mold, and wrapping the metal core with a heat insulating material to obtain a metal core wrapped with a heat insulating material; (2) The metal core wrapped with the thermal insulation material is pretreated, and then the soluble polymer is dissolved to make a solution, which is poured into the groove of the PDMS microneedle mold. The solution is vacuumed to remove bubbles. After the solution fills the groove of the PDMS microneedle mold, the metal core wrapped with the pretreated thermal insulation material is placed on the bottom surface of the groove of the PDMS microneedle mold. Finally, both are placed in a refrigerator to freeze, thereby obtaining ice microneedles.

2. The method for preparing substrate-free ice microneedles according to claim 1, characterized in that: The thermal insulation material is one or more of polyurethane foam, polystyrene foam, thermal insulation paper, foam glass or aerogel.

3. The method for preparing substrate-free ice microneedles according to claim 1, characterized in that: The pretreatment in step (2) is to place the metal core wrapped with the heat insulating material into a refrigerator.

4. The method for preparing substrate-free ice microneedles according to claim 1, characterized in that: The soluble polymer includes one or more of sodium hyaluronate, carboxymethyl cellulose, hydroxypropyl methyl cellulose, sodium alginate, chitosan, polycaprolactone, polyvinyl alcohol, polyvinyl pyrrolidone, silk fibroin, chondroitin sulfate, polyethylene glycol diacrylate, methacrylate gelatin, trehalose, polylactic acid-glycolic acid copolymer, galactose, dextrin, and maltose.

5. The method for preparing substrate-free ice microneedles according to claim 1, characterized in that: The freezing temperature of the refrigerator is -20℃~-80℃, and the freezing time of the refrigerator is 10-240 minutes.

6. The method for preparing substrate-free ice microneedles according to claim 1, characterized in that: The metal core includes one or more materials selected from stainless steel, titanium alloy, aluminum alloy, nickel-titanium alloy, and copper alloy.

7. The ice microneedle prepared according to the method for preparing substrate-free ice microneedle according to any one of claims 1 to 6.

Citation Information

Cited By

  • Ice microneedle manufacturing device based on semiconductor chilling plate

    CN119327019A

  • Ice micro-needle manufacturing device based on semiconductor refrigeration sheet

    CN119327019B

  • Microneedle preparation device and application method thereof

    CN120837831A

  • Microneedle preparation device and method of use thereof

    CN120837831B