Pre-coating coarse aggregate self-compacting concrete
By using pre-coated coarse aggregate self-compacting technology in concrete, the bonding force and interface bonding force between the aggregate and cement paste are enhanced, which solves the problem of insufficient performance of the interface transition zone in the existing technology and significantly improves the performance of the interface transition zone. Mechanical properties and durability of concrete.
Patent Information
- Application Number
- CN202411029212.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-15
AI Technical Summary
The existing technology cannot effectively improve the performance of the interface transition zone between aggregates and hydrates in concrete, resulting in low concrete strength and difficulty in improving the mechanical properties and durability of concrete.
Pre-coated coarse aggregate self-compacting concrete technology is used to enhance the bonding force between the aggregate and cement paste by coating an incompletely cured adhesive film layer on the surface of the coarse aggregate, and utilize the adhesive during the mixing process. The plasticity of the layer enables adaptive deformation and enhances the interface bonding force.
It improves the flexural and tensile properties and deformation properties of concrete, enhances the interface strength between aggregates and hydrates, significantly improves the mechanical properties and durability of concrete, and has good economy.
Abstract
Description
Technical Field
[0001] The invention relates to the field of concrete, in particular to a pre-coated coarse aggregate self-compacting concrete. Background Art
[0002] The interfacial transition zone is a thin layer with a thickness of 20 to 100 μm between the cement matrix and the aggregate, which is mainly composed of calcium hydroxide crystals that grow outward perpendicular to the aggregate surface and hydrated calcium silicate close to the cement matrix. Whether it is coarse aggregate or fine aggregate, an interfacial transition zone will be generated on the aggregate surface. The interfacial transition zone is the weak part between the cement paste and the aggregate, and has the characteristics of high porosity, enrichment of calcium hydroxide crystals and directional arrangement. Its formation mechanism mainly includes the side wall effect, micro-area bleeding effect, ion migration and nucleation effect, unilateral growth effect, flocculation effect and dehydration shrinkage effect. The synergistic effect of various effects makes the interfacial transition zone the weakest link in concrete. From the perspective of damage-fracture mechanics, the defects formed inside the interfacial transition zone are the origin of concrete structural damage and performance failure, and provide a path for the development of cracks. In order to improve the mechanical properties and durability of concrete structures, many scholars have improved the performance of the interfacial transition zone by adding mineral admixtures and nanomaterials, inducing biomineralization and carbon dioxide curing. In the prior art, some additives (water reducing agent, fiber, etc.) are added to concrete to improve the performance of cement hydrate matrix, thereby improving the shrinkage and strength characteristics of concrete materials. The above methods have limited improvement on the concrete interface transition zone, and none of them can substantially improve the performance of the interface transition zone. In fact, the weak interface between cement and aggregate has always been the main factor leading to the low strength of concrete materials. Therefore, only by solving the interface problem between aggregate and hydrate in concrete can the strength problem of the formed interface transition zone be truly improved, thereby achieving the purpose of improving the mechanical properties and durability of concrete structures. In the prior art, nano-silicon dioxide slurry and silica ash slurry are added to the surface of aggregates. These materials are auxiliary cementitious materials, and the aggregates are immediately mixed with concrete cement paste after adding the coating. During the mixing process, the coating on the surface of the aggregates has not yet hardened and is easily dissolved by the water in the concrete or rubbed off by the substances in the concrete, resulting in a large part of the aggregates not being attached to the coating, and thus ultimately not playing an ideal role.
[0003] Therefore, only by effectively improving the interface between aggregate and hydration in concrete can the strength of the interface transition zone be essentially improved, thereby achieving the goal of improving the mechanical properties and durability of concrete. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a pre-coated coarse aggregate self-compacting concrete, which can improve the mechanical properties and durability of concrete by strengthening the interface between aggregate and hydrate in concrete.
[0005] The pre-coated coarse aggregate self-compacting concrete of the present invention comprises a pre-coated coarse aggregate, wherein the pre-coated coarse aggregate is prepared by coating a rubber material on the coarse aggregate, wherein the rubber material forms an uncured rubber film layer having a certain deformation capacity and bonding force on the surface of the coarse aggregate;
[0006] Furthermore, the adhesive film layer is in a wet-to-touch state when mixed with other raw materials of concrete;
[0007] Furthermore, the adhesive comprises the adhesive and a curing agent, the adhesive is pre-mixed with coarse aggregate and then the curing agent is added and mixed; or the adhesive and the curing agent are pre-mixed and then mixed with the coarse aggregate;
[0008] Further, the adhesive is a two-component epoxy resin;
[0009] Further, the adhesive is directly cured into a film after being mixed with the coarse aggregate;
[0010] Furthermore, the sizing material is one or a mixture of two or more of epoxy resins, polyacrylic acid, polyurethane, thermosetting phenolic resin, unsaturated polyurethane resin, and polyurea;
[0011] Furthermore, the dosage ratio of the rubber material to the coarse aggregate is 0.01-0.5:1; the dosage of the coarse aggregate in the pre-coating layer is 10-100% by volume;
[0012] Further, the particle size of the coarse aggregate is 5-50 mm;
[0013] Furthermore, the rubber material also includes a thickener and a diluent. The thickener is any one of fumed silica, aluminum hydroxide, magnesium oxide, and magnesium hydroxide; and the diluent is any one of commercially available epoxy reactive diluents, acetone, ethanol, dimethyl carbonate, and sec-butyl acetate.
[0014] The beneficial effects of the present invention are as follows: the pre-coated coarse aggregate self-compacting concrete of the present invention is coated with a glue layer on the coarse aggregate before mixing, and the glue layer is cured to a state where the surface is dry and has a certain adhesion and plasticity and has subsequent bonding ability, and then mixed with other raw materials of the concrete. Since the glue layer on the surface of the coarse aggregate still has a certain plasticity, the bonding strength between the pre-coated material and the aggregate and the cement paste is higher, so the bonding force between the coarse aggregate and the cement paste can be enhanced, and the gripping performance of the coarse aggregate and the concrete is improved; and the glue layer can be adaptively deformed during the mixing process of the pre-coated coarse aggregate and other raw materials of the concrete. After curing, a mechanical bite with any solid particles in the concrete is formed to increase the bonding force with the concrete, and the interface between the aggregate and the hydrate in the concrete is strengthened, so that the advantages of the self-compacting concrete can be fully utilized, the bending and tensile performance of the concrete is improved, and the deformation performance of the concrete is further enhanced by utilizing the excellent deformation ability of the cured glue layer, so as to achieve the purpose of improving the mechanical properties and durability of the concrete, and has good economy. DETAILED DESCRIPTION
[0015] For a better understanding of the present invention, the following examples are provided to further illustrate the present invention, but the present invention is not limited to the following examples.
[0016] In the examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.
[0017] The pre-coated coarse aggregate self-compacting concrete of this embodiment includes a pre-coated coarse aggregate, which is made by coating a rubber compound on the coarse aggregate, and the rubber compound forms an uncured rubber film layer on the surface of the coarse aggregate with a certain deformation capacity and bonding force; concrete aggregate refers to a granular loose material that plays a skeleton or filling role in concrete. It is divided into coarse aggregate and fine aggregate. Coarse aggregate refers to pebbles, crushed stones, etc., and fine aggregate refers to natural sand, artificial sand, etc. Apply glue layer on the coarse aggregate before mixing, and mix with concrete material after the glue layer is cured to a certain adhesion and plasticity on the surface and has the ability to bond in the future. Since the glue layer on the surface of the coarse aggregate still has a certain plasticity, it can enhance the bonding force between the coarse aggregate and cement paste, improve the pull-out resistance of the coarse aggregate and the gripping performance with the concrete; and the glue layer can be adaptively deformed during the mixing process of the pre-coated coarse aggregate with other raw materials of concrete. After curing, it forms a mechanical bite with any solid particles in the concrete, increases the bonding force with the concrete, and strengthens the interface between the aggregate and the hydrate in the concrete. It can fully take advantage of the self-compacting concrete, improve the bending and tensile performance of the concrete, and further enhance the deformation performance of the concrete by utilizing the excellent deformation ability of the cured glue layer, so as to achieve the purpose of improving the mechanical properties and durability of the concrete, and has good economic efficiency. Since there is a strong bonding tendency between the glue layers that are not fully cured, they must be dispersed while waiting to cure to the set hardness, otherwise they will be bonded together and cannot be produced in the future. Therefore, the purpose of the present invention can be achieved by manual processing with low efficiency or by using a dispersing device with high efficiency. As for the dispersing device, conventional devices in the prior art can be used, or special devices specifically for the dispersion of the coarse aggregate of the pre-coating layer of the present invention can be used. As for how to apply the glue to the coarse aggregate, a spraying method can be used, where the glue is sprayed on the coarse aggregate, and cement, sand, and fine aggregate are added after the glue is cured to a set hardness; and finally mixing is performed.
[0018] In this embodiment, the adhesive film layer is in a state of being wet to the touch (wet to the touch or plastic to the surface) when mixed with other raw materials of concrete; the so-called "wet to the touch state" refers to the surface dry state where the coating feels sticky when the finger touches it lightly, but there is no coating sticking to the hand. At this time, the adhesive film layer has a certain adhesive force and deformation ability, which can not only ensure that it adheres to the surface of the coarse aggregate without being washed away during the mixing process with the cement slurry, but also ensure that the surface of the adhesive layer will undergo adaptive deformation during the mixing process, thereby reducing the contact angle and increasing the adhesion. And because the coarse aggregate, such as stone, is irregular and has many edges and corners, after the adhesive film layer is applied, the contact area of the stone can be increased to prevent the stone from breaking during the mixing and extrusion process. If the adhesive film layer is cured, the adhesive coating will lose its viscosity. At this time, the surface of the adhesive layer is relatively smooth, and there is also a large contact angle with the concrete. At this time, the adhesive film layer does not play any pre-coating role on the coarse aggregate, and the effect is not much different from that of simply using coarse aggregate. However, if the degree of curing of the film layer is too low, the adhesion of the film layer to the coarse aggregate is low, and the film layer has not yet hardened and is easily dissolved by the moisture in the concrete or rubbed off by the substances in the concrete, thus failing to achieve the ideal effect.
[0019] In this embodiment, the adhesive includes the adhesive and a curing agent. The adhesive is pre-mixed with coarse aggregate and then the curing agent is added and mixed; or the adhesive and the curing agent are pre-mixed and then mixed with coarse aggregate. The adhesive includes the adhesive and a curing agent for reacting with the adhesive to form an adhesive film layer; the adhesive alone has no curing effect, and only after mixing with the curing agent or adding the curing agent can the adhesive be cured to form an adhesive film layer. This is equivalent to the adhesive being a two-component, or AB glue, which can only work if the two components exist at the same time. Therefore, it is convenient for transportation and storage. Therefore, before use, the adhesive can be mixed with the coarse aggregate, and then the curing agent can be added to cure to the set hardness during the construction process. Alternatively, the adhesive and the curing agent can be mixed at the construction site and then mixed with the coarse aggregate for construction.
[0020] Preferably, the adhesive is a two-component epoxy resin; after spraying the epoxy resin glue, a thin film is formed on the surface of the coarse aggregate, which enhances the bonding performance while improving the connection ability between the aggregate and the cement mortar, effectively improving the bonding ability of the interface, and further improving the flexural strength of the concrete. At the microscopic level, most of the damage to concrete comes from the damage to the interface between the cement mortar and the aggregate. The bonding ability between the aggregate and the cement paste can be enhanced by a specific epoxy resin glue coating, which can effectively improve the flexural strength.
[0021] Of course, the adhesive may also have a component that can cure with coarse aggregate to form a film, that is, the adhesive is a single component, and the adhesive also has a curing agent that reacts with water in the cement slurry to form a film layer.
[0022] In this embodiment, the rubber material is one or a mixture of two or more of epoxy resin, polyacrylic acid, polyurethane, thermosetting phenolic resin, unsaturated polyurethane resin, and polyurea. Preferably, it is E51, E44, etc. in epoxy resin; methyl methacrylate, butyl methacrylate, GMA copolymer in polyacrylic acid; MDI type polyurethane, polyurethane prepolymer, etc. in polyurethane.
[0023] In this embodiment, the ratio of the adhesive to the coarse aggregate is 0.01-0.5:1; the amount of the pre-coated coarse aggregate is 10-100%. Since the coarse aggregate obtained after the pre-coating has good toughness, and the adhesive layer surface will undergo adaptive deformation during the mixing process with concrete, the adhesion is increased, and the side wall effect between the aggregate and cement particles is eliminated. Therefore, compared with the traditional coarse aggregate, the pre-coated coarse aggregate of the present invention can achieve the purpose of improving the mechanical properties and durability of concrete with a smaller usage amount. By pre-coating the coarse aggregate, the bonding between the coarse aggregate and the cement paste is enhanced, and the flexural tensile strength of the concrete is improved.
[0024] In this embodiment, the particle size of the coarse aggregate is 5-50mm. The particle size of the coarse aggregate refers to the particle size of the coarse aggregate in the concrete, and the particle size is a direct factor affecting the quality of the concrete. The size of the coarse aggregate particle size directly affects the uniformity, fluidity, compressive strength and other properties of the concrete. When the particle size of the coarse aggregate is too large, the voids are too small, and the air in the concrete easily enters the concrete structure, resulting in a decrease in the compressive strength of the concrete; when the particle size of the coarse aggregate is too small, there are too many voids, and the water in the concrete is too permeable, causing the concrete to lose fluidity and reduce the compressive strength; due to the different sizes of the coarse aggregate particles, the voids formed by the coarse aggregate in the concrete will also be different, which will affect the uniformity, fluidity and compressive strength of the concrete. The coarse aggregate of the present invention, combined with the action of the rubber coating, can maximize the bending and tensile strength of the concrete. As for the pre-coated coarse aggregate of the present invention, if the particle size of the pre-coated coarse aggregate is too large, it will affect the mixing performance. If the particle size is too small, it is easy to unite during the mixing process and cannot play the role of the coarse aggregate.
[0025] In this embodiment, the rubber compound further includes a thickener and a diluent, wherein the thickener is any one of fumed silica, aluminum hydroxide, magnesium oxide, and magnesium hydroxide; and the diluent is any one of commercially available epoxy reactive diluents, acetone, ethanol, dimethyl carbonate, and sec-butyl acetate. The diluent and the thickener are combined with the rubber compound to improve the fluidity and interfacial capacity of the colloid, thereby achieving better coating performance with coarse aggregate and other raw materials of concrete, thereby improving the overall performance of the material.
[0026] Embodiment 1
[0027] The pre-coat layer coarse aggregate self-compacting concrete of this embodiment is prepared by adding 100% of the pre-coat layer coarse aggregate into concrete (including cement, sand, and fine aggregate, as in the following embodiment), wherein the particle size of the coarse aggregate is 5 to 10 mm. The surface of the coarse aggregate is sprayed with epoxy resin material (80 kg per cubic meter), and after curing until it is not dry to the touch, the coarse aggregate is first placed in a mixing bin, and then cement, sand, fine aggregate, water, etc. are added for mixing, molded, and conventionally maintained to obtain the pre-coat layer coarse aggregate self-compacting concrete.
[0028] Embodiment 2
[0029] The pre-coat layer coarse aggregate self-compacting concrete of this embodiment is prepared by adding 80% of the pre-coat layer coarse aggregate into concrete, wherein the particle size of the coarse aggregate is 20-50 mm. The surface of the coarse aggregate is stirred with an epoxy resin material (40 kg per cubic meter), and after solidification until it is not dry to the touch, the coarse aggregate is first placed in a mixing bin, and then cement, sand, fine aggregate, water, etc. are added for mixing, molded, and conventionally maintained to obtain the pre-coat layer coarse aggregate self-compacting concrete.
[0030] Embodiment 3
[0031] The pre-coat layer coarse aggregate self-compacting concrete of this embodiment is prepared by adding 50% of the pre-coat layer coarse aggregate into concrete, wherein the particle size of the coarse aggregate is 10-20 mm. The surface of the coarse aggregate is sprayed with epoxy resin material (20 kg per cubic meter), and after curing until it is not dry to the touch, the pre-coat layer coarse aggregate is first put into a mixing bin, and then steel fiber is slowly added, and finally cement, sand, fine aggregate, water, etc. are added and mixed to obtain the pre-coat layer coarse aggregate self-compacting concrete.
[0032] Embodiment 4
[0033] The pre-coat layer coarse aggregate self-compacting concrete of this embodiment is prepared by adding 100% of the pre-coat layer coarse aggregate into the concrete, wherein the particle size of the coarse aggregate is 5-20 mm. The surface of the coarse aggregate is sprayed with epoxy resin material (40 kg per cubic meter), and after curing to a hardness of being wet to the touch, the coarse aggregate is first put into a mixing bin, and then steel fiber is slowly added, and finally cement, sand and fine aggregate are added; finally, the mixture is mixed to obtain the pre-coat layer coarse aggregate self-compacting concrete.
[0034] Comparative Example 1
[0035] The same as Example 1, except that the epoxy film layer on the coarse aggregate is mixed with the concrete base material after it is completely cured.
[0036] Comparative Example 2
[0037] The same as Example 1, the only difference is that the coarse aggregate is mixed with the concrete base material immediately after spraying the epoxy adhesive.
[0038] Comparative Example 3
[0039] The other raw materials and coarse aggregate of concrete are mixed according to the conventional method in the prior art.
[0040] The pre-coated coarse aggregate self-compacting concrete of the above embodiment was used to prepare test pieces according to the method in the prior art and perform performance tests. The test results are as follows:
[0041] Coarse aggregate content (volume percentage) Pre-coating weight (kg) Flexural strength Example 1 100 80 8.2Mpa Example 2 80 40 6.8Mpa Example 3 50 20 5.7Mpa Example 4 100 40 7.4Mpa Comparative Example 1 100 80 6.7Mpa Comparative Example 2 100 80 7.2Mpa Comparative Example 3 0 0 4.5Mpa
[0042] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A pre-coated coarse aggregate self-compacting concrete, characterized in that: The invention comprises a pre-coated coarse aggregate, wherein the pre-coated coarse aggregate is prepared by coating a rubber material on the coarse aggregate, wherein the rubber material forms an uncured rubber film layer on the surface of the coarse aggregate and has a certain deformation ability and bonding force.
2. The pre-coated coarse aggregate self-compacting concrete according to claim 1, characterized in that: The adhesive film layer is in a wet-to-touch state when mixed with other raw materials of concrete.
3. The pre-coated coarse aggregate self-compacting concrete according to claim 1, characterized in that: The adhesive material comprises the adhesive and a curing agent. The adhesive is mixed with coarse aggregate in advance and then the curing agent is added and mixed; or the adhesive and the curing agent are mixed in advance and then mixed with the coarse aggregate.
4. The pre-coated coarse aggregate self-compacting concrete according to claim 3, characterized in that: The adhesive is a two-component epoxy resin.
5. The pre-coated coarse aggregate self-compacting concrete according to claim 1, characterized in that: The glue is directly cured into a film after being mixed with the coarse aggregate.
6. The pre-coated coarse aggregate self-compacting concrete according to claim 5, characterized in that: The adhesive is one or a mixture of two or more of epoxy resins, polyacrylic acid, polyurethane, thermosetting phenolic resin, unsaturated polyester resin, vinyl resin and polyurea resin.
7. The pre-coated coarse aggregate self-compacting concrete according to claim 1, characterized in that: The dosage ratio of the rubber material to the coarse aggregate is 0.01-0.5:1; the dosage of the coarse aggregate in the pre-coating layer is 10-100% by volume.
8. The pre-coated coarse aggregate self-compacting concrete according to claim 1, characterized in that: The particle size of the coarse aggregate is 5-50 mm.
9. The pre-coated coarse aggregate self-compacting concrete according to claim 1, characterized in that: The rubber material also includes a thickener and a diluent. The thickener is any one of fumed silica, aluminum hydroxide, magnesium oxide, and magnesium hydroxide; the diluent is any one of commercially available epoxy reactive diluents, acetone, ethanol, dimethyl carbonate, and sec-butyl acetate.
Citation Information
Patent Citations
Concrete with high extension strength and preparation method thereof
CN109626891A
Recycled aggregate concrete and preparation method thereof
CN112374827A
Powder-coated recycled coarse aggregate and preparation method thereof
CN112479616A
High-strength reinforced concrete and preparation method thereof
CN115710105A
Anti-seismic green premixed concrete with post-doped aggregate and preparation process of anti-seismic green premixed concrete
CN115893943A
Cited By
Concrete based on modified shale ceramsite and preparation method thereof
CN120229924A