Method for recovering metal from retired photovoltaic laminated part
By using a sulfuric acid-copper sulfate mixed solution and acid leaching treatment in an oxygen-free atmosphere combined with chemical precipitation, the problem of low metal recovery rates in decommissioned photovoltaic modules is solved, efficient multi-metal selective separation and recovery is achieved, and production costs are reduced. cost and environmental pollution, in line with the concept of circular economy.
Patent Information
- Application Number
- CN202410772757.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-15
AI Technical Summary
Existing methods for recycling decommissioned photovoltaic modules have problems such as incomplete recovery of metal components, low metal recovery rates, low value of metal recovery products, and complex processes. It is difficult to effectively dissociate and separate multi-component systems, resulting in low efficiency of metal resource recovery. And may cause secondary pollution to the environment.
By placing the welding ribbon into a sulfuric acid-copper sulfate mixed solution in an oxygen-free atmosphere for a displacement reaction, combined with acid leaching treatment and chemical precipitation, the selectivity of aluminum, silver, copper, tin, and lead in silicon wafers and welding ribbons is achieved. Separation and recovery, using the difference in redox potential for selective separation and directional enrichment of metals.
It achieves efficient recovery of valuable metals in decommissioned photovoltaic laminates, reduces production costs and energy consumption, increases metal recovery rates, conforms to the concept of circular economy, and reduces environmental pollution.
Smart Images

Figure CN118773449A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photovoltaic component recycling, and in particular to a method for recycling metals from retired photovoltaic laminates. Background Art
[0002] Energy crisis and climate crisis, as the dual challenges faced by the 21st century, are prompting the world to accelerate the transformation of its energy structure and urgently need to come up with solutions to alleviate climate problems. In this context, the development and utilization of renewable energy is particularly important. Among them, solar energy resources have become an important pillar in the field of energy production due to their abundance and low cost. However, with the vigorous development of the global photovoltaic industry, it is predicted that the global photovoltaic power generation capacity will increase to 8519GW by 2050. Due to their limited lifespan, the problem of handling retired photovoltaic modules has gradually surfaced and has become an environmental and economic challenge that needs to be solved urgently worldwide.
[0003] The lifespan of photovoltaic modules is generally 25-30 years. It is predicted that by 2050, the number of waste photovoltaic modules worldwide will reach 9.57 million tons, of which waste crystalline silicon photovoltaic modules account for 85-90% of the total waste. Waste photovoltaic modules contain abundant valuable resources, such as metals (aluminum, copper, silver, etc.), glass, silicon wafers, etc. If they are directly discarded or landfilled by traditional methods, it will not only lead to a huge waste of resources, but also may cause potential harm to the ecological environment and human health.
[0004] Retired photovoltaic laminates are mainly crystalline silicon photovoltaic modules, which are mainly composed of photovoltaic glass, EVA film, silicon wafers, polyvinyl fluoride TPT backboards, aluminum frames and junction boxes. After proper treatment, these materials have high recycling value. In particular, glass, silicon wafers and multi-metal enriched bodies such as silver, aluminum, copper, lead and tin in waste photovoltaic modules can be directly used in circular production after recycling and reprocessing, reducing dependence on new resources.
[0005] At present, some methods have been used to recycle retired photovoltaic modules, such as mechanical separation, hydrometallurgy, heat treatment, etc., to separate and remove organic matter in retired photovoltaic laminates, recover valuable metals such as glass, copper, and silver, and realize the recycling of retired photovoltaic laminates. For example, the comprehensive recycling method of waste photovoltaic modules disclosed in CN115647007A first removes the backplane assembly, and performs diamond wire cutting on the obtained assembly containing glass, EVA, and silicon wafers to separate the glass and silicon wafers, and then heat treats the obtained glass and silicon wafers, etches the silicon wafers with acid and alkali solutions, and recovers the valuable metals in the silicon wafers. This method focuses on the complete recovery of glass and silicon wafers, and the process flow is relatively complicated, and there is a problem of low recovery rate of valuable metals. For example, CN114833176A discloses a method for comprehensive recycling of all components of waste crystalline silicon photovoltaic modules. This method disassembles waste crystalline silicon photovoltaic modules by pre-sorting, separates complete panels from incomplete panels, and independently recycles them. This method can achieve low-cost, non-damaged, and high-efficiency secondary resource utilization of components that have not lost their functions, but this method does not involve multi-metal selective separation and enrichment. Another example is CN116371879A discloses a method for recycling all components of scrapped photovoltaic modules. This method disassembles aluminum frames and junction boxes by hydraulic riveting, and then uses thermal cutting to separate tempered glass, back panels, and battery cells. After the battery cells are crushed and sorted, they are separated and purified by acid dissolution-separation. Silicon powder and aluminum are smelted to obtain silicon-aluminum alloy, realizing green and efficient recycling of scrapped photovoltaic modules. However, this method does not consider the recycling of metals such as copper, lead, and tin, and has low economic benefits.
[0006] In addition, the existing recycling process for retired photovoltaic modules mainly focuses on the recycling of glass, silicon wafers, and metal silver and aluminum, and does not take into account the recovery of metals in welding ribbons, resulting in a low recovery rate of valuable metals, high energy consumption, and a complicated process.
[0007] As can be seen from the above, traditional methods for recycling retired photovoltaic modules often have problems such as incomplete metal component recovery, low metal recovery rate, low metal recovery product value, low resource level, and complex process flow. When these methods are used to process retired photovoltaic laminates, it is often difficult to effectively dissociate and separate the multi-component system, resulting in low metal resource recovery efficiency and possible secondary pollution to the environment. Therefore, it is urgent to develop an economical, efficient, and environmentally friendly method for resource utilization of retired photovoltaic modules. Summary of the invention
[0008] In view of this, an object of the present invention is to provide a method for recovering metals from retired photovoltaic laminates, so as to achieve the recovery of valuable metals in solder ribbons and silicon wafers in retired photovoltaic laminates.
[0009] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0010] A method for recovering metals from retired photovoltaic laminates, comprising the steps of:
[0011] Pre-treating the retired photovoltaic laminate to obtain a mixture of initial silicon wafers and initial solder strips;
[0012] Physically sorting the mixture of the initial silicon wafer and the initial solder strip to obtain silicon wafers, solder strips and a silicon wafer-solder strip mixture;
[0013] The silicon wafer is subjected to acid leaching treatment to obtain an aluminum-containing leaching solution and silver-containing silicon powder;
[0014] In an oxygen-free atmosphere, the solder strip is placed in a sulfuric acid-copper sulfate mixed solution to undergo a replacement reaction to obtain lead sulfate, tin-containing leaching solution and copper strips;
[0015] The silicon wafer-welding strip mixture is subjected to acid leaching to obtain an aluminum-containing leaching solution and a silver-containing silicon powder-welding strip (Cu / Pb / Sn);
[0016] The aluminum-containing leachate is subjected to a neutralization reaction to obtain aluminum hydroxide;
[0017] The silver-containing silicon powder-welding strip (Cu / Pb / Sn) is treated with a hydrochloric acid solution to obtain a copper strip, a leaching solution containing tin and lead, and a silver-containing silicon powder;
[0018] The silver-containing silicon powder is treated with acid to obtain a silver-containing leaching solution and silicon powder, and a chloride salt is added to the silver-containing leaching solution to obtain silver chloride;
[0019] The leaching solution containing tin and lead is subjected to sulfate precipitation to obtain lead sulfate and tin-containing leaching solution;
[0020] The tin-containing leaching solution is oxidized to obtain tin dioxide.
[0021] According to the above technical means, by cleverly utilizing the different redox potentials of the metals in the silicon wafers and solder strips of retired photovoltaic laminates, the higher the redox potential, the stronger the oxidizing property, and vice versa, the stronger the reducing property, thereby achieving the selective separation and recovery of the metals. For silicon wafers (Si-Ag-Al), by simply and cleverly using acid leaching treatment, the selective separation of metallic aluminum is effectively achieved, and the product silicon wafers and silver chloride are obtained by nitric acid leaching-sodium chloride precipitation method. For the solder strip (Cu-Pb-Sn) system, by simply and cleverly using the copper sulfate-sulfuric acid system, the selective separation of copper, lead and tin is effectively achieved, and the product copper and lead sulfate can be directly used, and the tin-containing solution can be directly oxidized to obtain the product tin oxide. For the silicon wafer-welding strip (Si-Ag-Al-Cu-Pb-Sn) system, the selective separation of metallic aluminum is effectively achieved by simply and cleverly using sulfuric acid leaching; the selective separation of copper and silver as well as lead and tin is achieved by using hydrochloric acid leaching; the further separation and purification of lead and tin solutions are effectively achieved by chemical precipitation; the silver-containing silicon powder can be directly sent to the silicon wafer system, and the product silicon wafer and silver chloride are obtained by the same nitric acid leaching-sodium chloride precipitation method. The above method not only effectively realizes the efficient recovery of various valuable metals, but also realizes the use of multiple process production lines, reduces production costs, has the advantages of low energy consumption, high product value and environmental friendliness, and is in line with the concept of circular economy.
[0022] The silicon powder obtained by the method of the present invention can be directly used in the regeneration process of silicon wafers, effectively realizing the in-situ utilization of silicon wafers.
[0023] The aluminum hydroxide and silver chloride products obtained by the method of the present invention can be directly sold externally, and can also be used in subsequent production processes of aluminum and silver metals.
[0024] The lead sulfate product obtained by the method of the present invention can be directly sold or roasted to form lead oxide.
[0025] The principle of the method for recovering metals from retired photovoltaic laminates of the present invention is that retired photovoltaic laminates mainly contain valuable metals such as silicon, silver, copper, and aluminum, and the metal distribution is relatively concentrated. Therefore, the present invention targets metal systems that may exist in the current recycling process, such as silicon wafers (Si-Ag-Al), welding strips (Cu-Pb-Sn), and silicon wafers-welding strips (Si-Ag-Al-Cu-Pb-Sn). Based on the different redox potentials of various metals in different systems, the present invention cleverly and simply uses acid leaching, neutralization reaction, replacement reaction, chemical precipitation and other technical means to effectively achieve the selective separation and directional enrichment of various metals in various systems, and further achieves the high-value comprehensive recovery and utilization of metals in retired photovoltaic laminates.
[0026] Preferably, the acid leaching treatment of the silicon wafer comprises: leaching the silicon wafer with a sulfuric acid solution.
[0027] Preferably, the acid leaching treatment of the silicon wafer-welding strip mixture comprises: leaching the silicon wafer-welding strip mixture with a sulfuric acid solution.
[0028] Preferably, the concentration of sulfuric acid in the sulfuric acid solution is 0.1-2 mol / L.
[0029] Preferably, the silicon wafer and sulfuric acid solution are in a kg:L ratio of 1kg:2 to 6L.
[0030] Preferably, the temperature of the leaching treatment is 20°C to 80°C.
[0031] Preferably, the leaching treatment time is 30 min to 90 min.
[0032] Preferably, the silicon wafer-welding ribbon mixture and the sulfuric acid solution are in a kg:L ratio of 1kg:1 to 5L.
[0033] Preferably, in the sulfuric acid-copper sulfate mixed solution, the concentration of copper sulfate is 0.1-1 mol / L, and the concentration of sulfuric acid is 0.1-2 mol / L.
[0034] Preferably, the welding strip and the sulfuric acid-copper sulfate mixed solution are calculated in kg:L at 1kg:1-10L.
[0035] Preferably, the temperature of the replacement reaction is 30°C to 80°C.
[0036] Preferably, the replacement reaction time is 10 min to 60 min.
[0037] Preferably, the aluminum-containing leachate is subjected to a neutralization reaction to obtain aluminum hydroxide by: neutralizing the aluminum-containing leachate with a sodium hydroxide solution to obtain aluminum hydroxide and a sodium sulfate solution.
[0038] Preferably, the concentration of sodium hydroxide in the sodium hydroxide solution is 0.1 to 2 mol / L.
[0039] Preferably, the temperature of the neutralization reaction is 30°C to 70°C.
[0040] Preferably, the neutralization reaction time is 30 min to 90 min.
[0041] Preferably, the sodium sulfate solution is used to precipitate the leaching solution containing tin and lead to achieve the recycling of sodium sulfate.
[0042] Among them, the sodium sulfate solution obtained by neutralization reaction of the aluminum-containing leachate can be directly used for precipitation treatment of the tin- and lead-containing leachate in the silicon wafer-welding strip mixture treatment system, which not only realizes the recycling of sodium sulfate, but also reduces production costs and reduces pollution to the environment.
[0043] Preferably, the concentration of hydrochloric acid in the hydrochloric acid solution is 0.05 to 1 mol / L.
[0044] Preferably, the silver-containing silicon powder-welding strip (Cu / Pb / Sn) and the hydrochloric acid solution are in a ratio of 1kg:1 to 5L in kg:L.
[0045] Preferably, the silver-containing silicon powder-welding strip (Cu / Pb / Sn) is treated with a hydrochloric acid solution at a temperature of 30° C. to 70° C.
[0046] Preferably, the silver-containing silicon powder-welding strip (Cu / Pb / Sn) is treated with the hydrochloric acid solution for 20 minutes to 90 minutes.
[0047] Preferably, the acid treatment of the silver-containing silicon powder comprises: treating the silver-containing silicon powder with a nitric acid solution.
[0048] Preferably, the concentration of nitric acid in the nitric acid solution is 0.2-1 mol / L.
[0049] Preferably, the silver-containing silicon powder and nitric acid solution are in a kg:L ratio of 1kg:1 to 3L.
[0050] Preferably, the temperature for treating the silver-containing silicon powder with the nitric acid solution is 50°C to 90°C.
[0051] Preferably, the time for treating the silver-containing silicon powder with the nitric acid solution is 20 minutes to 90 minutes.
[0052] Preferably, the oxidation treatment of the tin-containing leaching solution comprises: introducing oxygen into the tin-containing leaching solution for treatment.
[0053] Preferably, the method for recovering metals from retired photovoltaic laminates comprises the following steps:
[0054] S1, pre-processing the retired photovoltaic laminate to obtain initial silicon wafers, initial welding strips, photovoltaic glass and backplane;
[0055] S2, physically sorting the initial silicon wafer and the initial soldering strip to obtain silicon wafers, soldering strips and a silicon wafer-soldering strip mixture respectively;
[0056] S3, leaching the silicon wafer with a sulfuric acid solution, and filtering to obtain an aluminum-containing leaching solution and silver-containing silicon powder;
[0057] After the aluminum-containing leachate is neutralized and concentrated, the product aluminum hydroxide is obtained;
[0058] The silver-containing silicon powder is treated with a nitric acid solution, and after filtering, a silver-containing leaching solution and silicon powder are obtained, and the obtained silicon powder can be directly used in production applications;
[0059] Adding sodium chloride solution to the silver-containing leaching solution, filtering to obtain product silver chloride;
[0060] S4, placing the solder strip in a sulfuric acid-copper sulfate mixed solution for replacement reaction, and introducing nitrogen to keep the mixed solution in an oxygen-free atmosphere, and filtering to obtain the product lead sulfate and copper strips, as well as tin-containing leaching solution, and the copper strips can be used directly;
[0061] The tin-containing leaching solution is oxidized to obtain the product tin dioxide;
[0062] S5, leaching the silicon wafer-welding strip mixture with a sulfuric acid solution, and filtering to obtain an aluminum-containing leaching solution and a silver-containing silicon powder-welding strip (Cu / Pb / Sn);
[0063] The aluminum-containing leachate is directly sent to the aluminum-containing leachate treatment process of the silicon wafer;
[0064] Silver-containing silicon powder-welding strip (Cu / Pb / Sn) is treated with hydrochloric acid solution, and after filtration, copper strips, leaching solution containing tin and lead, and silver-containing silicon powder are obtained. The copper strips can be used directly;
[0065] The silver-containing silicon powder is directly sent to the silver-containing silicon powder processing process of the silicon wafer;
[0066] The leaching solution containing tin and lead is precipitated with sulfate, and filtered to obtain product lead sulfate and tin-containing leaching solution;
[0067] The tin-containing leaching solution is directly sent to the tin-containing leaching solution treatment process of the solder strip system.
[0068] The purity of the copper strip obtained by the above method is greater than 99%, and can be directly recycled.
[0069] Preferably, the pretreatment of the retired photovoltaic laminates comprises: treating the retired photovoltaic laminates by mechanical separation, heat treatment and solvent leaching.
[0070] Since retired photovoltaic laminates are a "glass-EVA film-silicon wafer-EVA film-TPT backplane" structure, the EVA film is very sticky. If it is not pre-treated and removed, it will directly affect the recycling of valuable materials such as photovoltaic glass, silicon wafers, and metals. Therefore, before recycling valuable metals, retired photovoltaic laminates are pre-treated by mechanical separation, heat treatment, and solvent leaching to ensure efficient and high-quality recycling of valuable metals.
[0071] Preferably, the retired photovoltaic laminate is selected from at least one of a polycrystalline silicon retired photovoltaic laminate, a monocrystalline silicon retired photovoltaic laminate, a double-glass retired photovoltaic laminate and a single-glass retired photovoltaic laminate.
[0072] The method of the present invention considers the metal recovery under three reaction systems of silicon wafer (Si-Ag-Al), solder strip (Cu-Pb-Sn) and silicon wafer-solder strip (Si-Ag-Al-Cu-Pb-Sn) respectively according to the metal distribution in retired photovoltaic laminates, and proposes different metal recovery schemes for different systems, which not only realizes the selective separation and directional enrichment of metals under each system, but also avoids the influence of different material components on subsequent metal recovery. The process has a wide range of application, can realize the recovery of multiple valuable metals, and has a high metal recovery rate.
[0073] The method of the present invention utilizes the difference in redox potential of each metal to effectively realize the selective separation and enrichment of metals, reduce the use of strong acids and alkalis, improve the production environment, reduce production costs and wastewater volume, and most of the waste liquid generated in the process can be recycled.
[0074] After testing, the copper obtained by the method of the present invention meets the No. 2 standard copper (Cu>99.90%) of GB / T 467-2010, and the product has high purity and value. The obtained silicon wafer can be returned to the battery production process as a raw material, and the product lead sulfate, aluminum hydroxide, silver chloride and tin dioxide can be directly sold or used in the production of subsequent products, thereby realizing the comprehensive recovery and recycling of various valuable metals in retired photovoltaic laminates.
[0075] Beneficial effects of the present invention:
[0076] The method of recovering metals from retired photovoltaic laminates of the present invention realizes the selective separation and recovery of valuable metals in retired photovoltaic laminates by cleverly using the different redox potentials of the metals in the silicon wafers and solder strips of the retired photovoltaic laminates. For silicon wafers (Si-Ag-Al), the selective separation of metal aluminum is effectively realized by simply and cleverly using acid leaching treatment, and the product silicon wafers and silver chloride are obtained by using nitric acid leaching-sodium chloride precipitation method. For the solder strip (Cu-Pb-Sn) system, the selective separation of copper, lead and tin is effectively realized by simply and cleverly using the copper sulfate-sulfuric acid system, and the product copper and lead sulfate can be directly used, and the tin-containing solution can be directly oxidized to obtain the product tin oxide. For the silicon wafer-welding strip (Si-Ag-Al-Cu-Pb-Sn) system, the selective separation of metallic aluminum is effectively achieved by simply and cleverly using sulfuric acid leaching; the selective separation of copper and silver as well as lead and tin is achieved by using hydrochloric acid leaching; the further separation and purification of lead and tin solutions are effectively achieved by chemical precipitation; the silver-containing silicon powder can be directly sent to the silicon wafer system, and the product silicon wafer and silver chloride are obtained by the same nitric acid leaching-sodium chloride precipitation method. The above method not only effectively realizes the efficient recovery of various valuable metals, but also realizes the use of multiple process production lines, reduces production costs, has the advantages of low energy consumption, high product value and environmental friendliness, and conforms to the concept of circular economy. In addition, the method of the present invention fully considers the recovery of multiple metals under different systems in the industrial recycling process, has a wide range of process applications, has promotion and application value, and is suitable for industrial promotion in the field of photovoltaic module recycling technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0077] Figure 1 is a process flow chart of the present invention for recovering valuable metals from retired photovoltaic laminates;
[0078] Figure 2 is a retired photovoltaic laminate structure to be processed according to an embodiment of the present invention;
[0079] Figure 3 This is the XRD pattern of the pure silicon wafer obtained in Example 1 of the present invention;
[0080] Figure 4 This is a photo of the welding strip in Example 1 of the present invention, wherein: Figure 4 A is the welding strip before reaction, Figure 4 B is the welding strip after reaction;
[0081] Figure 5 This is a physical picture of the welding strip after reaction obtained in Comparative Example 1 of the present invention;
[0082] Figure 6 This is the XRD diagram of the solder strip after reaction obtained in Comparative Example 1 of the present invention;
[0083] Figure 7This is the redox potential diagram of the metals recovered in the present invention. DETAILED DESCRIPTION
[0084] The following will describe the embodiments of the present invention with reference to the preferred embodiments, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are only for illustrating the present invention, not for limiting the scope of protection of the present invention.
[0085] The present invention intends to disclose a method for recovering metals from retired photovoltaic laminates, so as to achieve the recovery of valuable metals in solder ribbons and silicon wafers in retired photovoltaic laminates.
[0086] A method for recovering metals from retired photovoltaic laminates, comprising the steps of:
[0087] Pre-treating the retired photovoltaic laminate to obtain a mixture of initial silicon wafers and initial solder strips;
[0088] Physically sorting the mixture of the initial silicon wafer and the initial solder strip to obtain silicon wafers, solder strips and a silicon wafer-solder strip mixture;
[0089] The silicon wafer is subjected to acid leaching treatment to obtain an aluminum-containing leaching solution and silver-containing silicon powder;
[0090] In an oxygen-free atmosphere, the solder strip is placed in a sulfuric acid-copper sulfate mixed solution to undergo a replacement reaction to obtain lead sulfate, tin-containing leaching solution and copper strips;
[0091] The silicon wafer-welding strip mixture is subjected to acid leaching to obtain an aluminum-containing leaching solution and a silver-containing silicon powder-welding strip (Cu / Pb / Sn);
[0092] The aluminum-containing leachate is subjected to a neutralization reaction to obtain aluminum hydroxide;
[0093] The silver-containing silicon powder-welding strip (Cu / Pb / Sn) is treated with a hydrochloric acid solution to obtain a copper element, a leaching solution containing tin and lead, and a silver-containing silicon powder;
[0094] The silver-containing silicon powder is treated with acid to obtain a silver-containing leaching solution and silicon powder, and a chloride salt is added to the silver-containing leaching solution to obtain silver chloride;
[0095] The leaching solution containing tin and lead is subjected to sulfate precipitation to obtain lead sulfate and tin-containing leaching solution;
[0096] The tin-containing leaching solution is oxidized to obtain tin dioxide.
[0097] By cleverly using the different redox potentials of the metals in the silicon wafers and solder strips of retired photovoltaic laminates, elements with more negative redox potentials can replace elements with higher redox potentials, thereby achieving selective separation and recovery of valuable metals in retired photovoltaic modules. Therefore, for silicon wafers (Si-Ag-Al), by simply and cleverly using acid leaching treatment, the selective separation of metallic aluminum is effectively achieved, and the product silicon wafers and silver chloride are obtained by nitric acid leaching-sodium chloride precipitation. For the solder strip (Cu-Pb-Sn) system, by simply and cleverly using the copper sulfate-sulfuric acid system, the selective separation of copper, lead and tin is effectively achieved, and the product copper and lead sulfate can be directly used, while the tin-containing solution can be directly oxidized to obtain the product tin oxide. For the silicon wafer-welding strip (Si-Ag-Al-Cu-Pb-Sn) system, the selective separation of metal aluminum is effectively achieved by simply and cleverly using sulfuric acid leaching; the selective separation of copper and silver as well as lead and tin is achieved by using hydrochloric acid leaching; the further separation and purification of lead and tin solutions are effectively achieved through chemical precipitation; the silver-containing silicon powder can be directly sent to the silicon wafer processing system, and the product silicon wafer and silver chloride are obtained by the same nitric acid leaching-sodium chloride precipitation method. The above method not only effectively realizes the efficient recovery of various valuable metals, but also realizes the use of multiple process production lines, reduces production costs, has the advantages of low energy consumption, high product value and environmental friendliness, and is in line with the concept of circular economy.
[0098] In some embodiments, the acid leaching treatment of the silicon wafer includes: leaching the silicon wafer with a sulfuric acid solution.
[0099] In some embodiments, subjecting the silicon wafer-welding ribbon mixture to acid leaching treatment includes: subjecting the silicon wafer-welding ribbon mixture to leaching treatment using a sulfuric acid solution.
[0100] In some embodiments, the concentration of sulfuric acid in the sulfuric acid solution is 0.1-2 mol / L.
[0101] In some embodiments, the ratio of silicon wafer to sulfuric acid solution is 1kg:2-6L in kg:L.
[0102] In some embodiments, the temperature of the sulfuric acid solution for leaching the silicon wafer is 20°C to 80°C.
[0103] In some embodiments, the time for leaching the silicon wafer-welding ribbon mixture with the sulfuric acid solution is 30 minutes to 90 minutes.
[0104] In some embodiments, the temperature of the sulfuric acid solution for leaching the silicon wafer-welding ribbon mixture is 20° C. to 80° C.
[0105] In some embodiments, the silicon wafer-ribbon mixture and the sulfuric acid solution are calculated in kg:L at 1kg:1-5L.
[0106] Exemplarily, the ratio of the silicon wafer-ribbon mixture to the sulfuric acid solution is 1 kg:5 L.
[0107] In some embodiments, in the sulfuric acid-copper sulfate mixed solution, the concentration of copper sulfate is 0.1-1 mol / L, and the concentration of sulfuric acid is 0.1-2 mol / L.
[0108] Exemplarily, in the sulfuric acid-copper sulfate mixed solution, the concentration of copper sulfate is 0.5 mol / L, and the concentration of sulfuric acid is 0.1 mol / L.
[0109] In some embodiments, the ratio of the soldering tape to the sulfuric acid-copper sulfate mixed solution is 1 kg:1 to 10 L.
[0110] Exemplarily, the ratio of the solder strip to the sulfuric acid-copper sulfate mixed solution is 1kg:5L.
[0111] In some embodiments, the temperature of the replacement reaction is 30°C to 80°C.
[0112] In some embodiments, the replacement reaction time is 10 min to 60 min.
[0113] In some embodiments, the aluminum-containing leachate is subjected to a neutralization reaction to obtain aluminum hydroxide by neutralizing the aluminum-containing leachate with a sodium hydroxide solution to obtain aluminum hydroxide and a sodium sulfate solution.
[0114] In some embodiments, the concentration of sodium hydroxide in the sodium hydroxide solution is 0.1-2 mol / L.
[0115] Exemplarily, the concentration of sodium hydroxide in the sodium hydroxide solution is 0.1 mol / L.
[0116] In some embodiments, the temperature of the neutralization reaction is 30°C to 70°C.
[0117] In some embodiments, the neutralization reaction time is 30 min to 90 min.
[0118] In some embodiments, in order to realize the recycling of sodium sulfate, reduce production costs and reduce environmental pollution, the sodium sulfate solution obtained by neutralizing the aluminum-containing leachate is directly used to precipitate the tin- and lead-containing leachate.
[0119] In some embodiments, the concentration of hydrochloric acid in the hydrochloric acid solution is 0.05-0.1 mol / L.
[0120] Exemplarily, the concentration of hydrochloric acid in the hydrochloric acid solution is 0.1 mol / L.
[0121] In some embodiments, the silver-containing silicon powder-welding strip (Cu / Pb / Sn) and the hydrochloric acid solution are calculated in kg:L at 1kg:1-5L.
[0122] Exemplarily, the ratio of silver-containing silicon powder-solder strip (Cu / Pb / Sn) to hydrochloric acid solution is 1kg:5L.
[0123] In some embodiments, the silver-containing silicon powder-welding strip (Cu / Pb / Sn) is treated with the hydrochloric acid solution for a time period of 30° C. to 70° C.
[0124] In some embodiments, the silver-containing silicon powder-welding strip (Cu / Pb / Sn) is treated with the hydrochloric acid solution for 20 minutes to 90 minutes.
[0125] In some embodiments, the acid treatment of the silver-containing silicon powder includes: treating the silver-containing silicon powder with a nitric acid solution.
[0126] In some embodiments, the concentration of nitric acid in the nitric acid solution is 0.2-1 mol / L.
[0127] In some embodiments, the ratio of silver-containing silicon powder to nitric acid solution is 1 kg:1 to 3 L.
[0128] In some embodiments, the temperature for treating the silver-containing silicon powder with the nitric acid solution is 50° C. to 90° C.
[0129] In some embodiments, the time for treating the silver-containing silicon powder with the nitric acid solution is 20 minutes to 90 minutes.
[0130] In some embodiments, the oxidation treatment of the tin-containing leachate comprises: introducing oxygen into the tin-containing leachate for treatment.
[0131] In some embodiments, a method of recovering metals from retired photovoltaic laminates comprises the following steps:
[0132] S1, pre-processing the retired photovoltaic laminate to obtain initial silicon wafers, initial welding strips, photovoltaic glass and backplane;
[0133] S2, physically sorting the initial silicon wafer and the initial soldering strip to obtain silicon wafers, soldering strips and a silicon wafer-soldering strip mixture respectively;
[0134] S3, leaching the silicon wafer with a sulfuric acid solution, and filtering to obtain an aluminum-containing leaching solution and silver-containing silicon powder;
[0135] After the aluminum-containing leachate is neutralized and concentrated, the product aluminum hydroxide is obtained;
[0136] The silver-containing silicon powder is treated with a nitric acid solution, and after filtering, a silver-containing leaching solution and silicon powder are obtained, and the obtained silicon powder can be directly used in production applications;
[0137] Adding sodium chloride solution to the silver-containing leaching solution, filtering to obtain product silver chloride;
[0138] S4, placing the solder strip in a sulfuric acid-copper sulfate mixed solution for replacement reaction, and introducing nitrogen to keep the mixed solution in an oxygen-free atmosphere, and filtering to obtain the product lead sulfate and copper strips, as well as tin-containing leaching solution, and the copper strips can be used directly;
[0139] The tin-containing leaching solution is oxidized to obtain the product tin dioxide;
[0140] S5, leaching the silicon wafer-welding strip mixture with a sulfuric acid solution, and filtering to obtain an aluminum-containing leaching solution and a silver-containing silicon powder-welding strip (Cu / Pb / Sn);
[0141] The aluminum-containing leachate is directly sent to the aluminum-containing leachate treatment process of the silicon wafer;
[0142] Silver-containing silicon powder-welding strip (Cu / Pb / Sn) is treated with hydrochloric acid solution, and after filtration, copper strips, leaching solution containing tin and lead, and silver-containing silicon powder are obtained. The copper strips can be used directly;
[0143] The silver-containing silicon powder is directly sent to the silver-containing silicon powder processing process of the silicon wafer;
[0144] The leaching solution containing tin and lead is precipitated with sulfate, and filtered to obtain product lead sulfate and tin-containing leaching solution;
[0145] The tin-containing leaching solution is directly sent to the tin-containing leaching solution treatment process of the solder strip system.
[0146] The above method achieves the selective separation and directional enrichment of multiple metals in retired photovoltaic laminates when recovering valuable metals, and further realizes the high-value comprehensive utilization of retired photovoltaic laminates.
[0147] In some embodiments, since the retired photovoltaic laminate is a "glass-EVA film-silicon wafer-EVA film-TPT backplane" structure, the EVA film has a high viscosity. If it is not pre-treated and removed, it will directly affect the recycling of valuable materials such as photovoltaic glass, silicon wafers, and metals. Therefore, mechanical separation, heat treatment, and solvent leaching are used to pre-treat the retired photovoltaic laminate.
[0148] In some embodiments, the retired photovoltaic laminate is selected from at least one of a multicrystalline silicon retired photovoltaic laminate, a monocrystalline silicon retired photovoltaic laminate, a double-glass retired photovoltaic laminate, and a single-glass retired photovoltaic laminate.
[0149] Exemplarily, the retired photovoltaic laminate is selected from a multicrystalline silicon retired photovoltaic laminate, a monocrystalline silicon retired photovoltaic laminate, a double-glass retired photovoltaic laminate or a single-glass retired photovoltaic laminate.
[0150] Among them, retired photovoltaic laminates contain copper (Cu), silver (Ag), aluminum (Al), lead (Pb) and tin (Sn). Taking the redox potential of copper (Cu), lead (Pb) and tin (Sn) as an example, the relationship between their redox potentials is as follows: Figure 7 As shown. Figure 7 It can be seen that the redox potential of tin (Sn) and lead (Pb) is more negative, and can replace metallic copper from the copper-containing solution, thereby realizing the recovery of metal on the solder tape in retired photovoltaic laminates.
[0151] In order to make the technical problems, technical solutions and beneficial effects solved by the present application clearer, the method for recovering metals from retired photovoltaic laminates of the present invention will be further described in detail below in conjunction with specific embodiments and drawings. Obviously, the specific embodiments described are only part of the embodiments of the present application, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present application and its applications. Based on the specific embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work belong to the scope of protection of the present application.
[0152] If no specific techniques or conditions are specified in the specific embodiments, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0153] Example 1
[0154] like Figure 1 As shown, a method for recovering metals from retired photovoltaic laminates comprises the following steps:
[0155] S1. Decommissioned photovoltaic laminates (such as Figure 2 As shown) are mechanically separated to obtain a mixture of initial silicon wafers and initial solder strips, as well as photovoltaic glass and backplane;
[0156] S2, subjecting the mixture of the initial silicon wafer and the initial solder strip obtained in S1 to color sorting and optical sorting, and obtaining silicon wafers and solder strips (such as Figure 4 A) and silicon wafer-welding ribbon mixture, the sorting efficiency can reach 95%;
[0157] S3, take 500g of the silicon wafer obtained in S2 and place it in a reactor, add 2L of 0.5mol / L sulfuric acid solution, heat it to 60°C, start stirring and react for 30min, filter to obtain aluminum-containing leaching solution and silver-containing silicon powder, wherein the aluminum leaching rate can reach more than 98%;
[0158] The aluminum-containing leachate is neutralized and hydrolyzed, and the temperature is controlled at 65°C to promote the hydrolysis of aluminum ions to obtain the product aluminum hydroxide, wherein the hydrolysis efficiency is as high as 99.5%;
[0159] The silver-containing silicon powder is treated with 100 mL of 0.5 mol / L nitric acid solution, and filtered to obtain a silver-containing leaching solution and silicon powder, wherein the silver leaching rate is 99.3%, and the grade of the obtained silicon powder is greater than 99%, so that the silicon powder can be directly used for production applications;
[0160] Add 20mL of 1mol / L sodium chloride solution to the silver-containing leaching solution, and obtain the product silver chloride after filtering, wherein the silver recovery rate is as high as 98%;
[0161] S4, put 500g solder strip (such as Figure 4 A) was placed in a reaction kettle and 4 L of 0.2 mol / L CuSO 4 and 0.5 mol / LH 2 SO 4 The mixed solution is subjected to a replacement reaction, the temperature is controlled at 60°C, the rotation speed is 600rpm, and nitrogen is introduced to keep the mixed solution in an oxygen-free atmosphere. After filtration, the products of lead sulfate and copper strips, as well as tin-containing leaching solution are obtained, wherein the lead recovery rate is greater than 98%, the copper strip grade is greater than 99%, and the copper strip can be used directly. The copper strip is the welding strip after the reaction, such as Figure 4 As shown in B;
[0162] The tin-containing leaching solution is placed in the air for 2 hours, and the product tin dioxide is obtained through air oxidation treatment, and the tin recovery rate can reach more than 95%;
[0163] S5. Put 100g of silicon wafer-welding strip mixture in a reactor, add 500mL of 0.25mol / L sulfuric acid solution, and filter to obtain aluminum-containing leaching solution and silver-containing silicon powder-welding strip (Cu / Pb / Sn), and the aluminum leaching rate can reach more than 98%;
[0164] The aluminum-containing leachate is directly sent to the aluminum-containing leachate treatment process of the silicon wafer, and the product aluminum hydroxide is obtained by neutralization and hydrolysis;
[0165] Silver-containing silicon powder-welding strip (Cu / Pb / Sn) is treated with 200mL 0.1mol / L hydrochloric acid solution, and after filtration, copper strips, leaching solutions containing tin and lead, and silver-containing silicon powder are obtained. The grade of the copper strips is greater than 99%, and the copper strips can be used directly;
[0166] The silver-containing silicon powder is directly sent to the silver-containing silicon powder treatment process of silicon wafers, and is leached with nitric acid and precipitated with sodium chloride to obtain product silicon powder and silver chloride;
[0167] The leaching solution containing tin and lead was treated with 20 mL of 0.5 mol / L sodium sulfate (Na 2SO 4 ) solution precipitation, after filtering, the product lead sulfate and tin-containing leaching solution are obtained. During the process, nitrogen is always introduced to keep the solution in an oxygen-free atmosphere. The recovery rate of lead is 98.5%;
[0168] The tin-containing leaching solution is directly sent to the tin-containing leaching solution treatment process of the solder strip, and the product tin dioxide is obtained after air oxidation, and the tin recovery rate can reach 90%.
[0169] Example 2
[0170] like Figure 1 As shown, a method for recovering metals from retired photovoltaic laminates comprises the following steps:
[0171] S1. Decommissioned photovoltaic laminates (such as Figure 2 As shown) are mechanically separated to obtain a mixture of initial silicon wafers and initial solder strips, photovoltaic glass and backplane;
[0172] S2, subjecting the mixture of the initial silicon wafer and the initial solder strip obtained in S1 to optical sorting, and obtaining silicon wafers, solder strips and a silicon wafer-solder strip mixture after sorting, respectively, with a sorting efficiency of up to 90%;
[0173] S3, take 500g of the silicon wafer obtained in S2 and place it in a reactor, add 2L of 0.1mol / L sulfuric acid solution, heat it to 60°C, start stirring and react for 30min, filter to obtain aluminum-containing leaching solution and silver-containing silicon powder, wherein the aluminum leaching rate can reach more than 90%;
[0174] The aluminum-containing leachate is neutralized and hydrolyzed, and the temperature is controlled at 65°C to promote the hydrolysis of aluminum ions to obtain the product aluminum hydroxide, with a hydrolysis efficiency of up to 99.5%;
[0175] The silver-containing silicon powder is treated with 100 mL of 0.1 mol / L nitric acid solution, and a silver-containing leaching solution and silicon powder are obtained after filtration, wherein the silver leaching rate is 85%, and the grade of the obtained silicon powder is greater than 90%. The silver-containing silicon powder needs to be further treated;
[0176] Add 20mL of 1mol / L sodium chloride solution to the silver-containing leaching solution, and obtain the product silver chloride after filtration, with a silver recovery rate of up to 98%;
[0177] S4, take 500g of solder strip and place it in a reactor, add 4L 0.2mol / L CuSO 4 -0.2 mol / L H 2 SO 4The mixture is subjected to a replacement reaction, the temperature is controlled at 60°C, the rotation speed is 600rpm, and nitrogen is introduced to keep the mixed solution in an oxygen-free atmosphere. After filtration, lead sulfate and copper bars are obtained, as well as a tin-containing leaching solution. The lead recovery rate is greater than 90%, and the copper bar grade is greater than 85%, and the copper bar needs to be further impurity-removed;
[0178] The tin-containing leaching solution is placed in the air for 1 hour, and after being oxidized by air, the product tin dioxide is obtained by filtration, and the recovery rate of tin can reach more than 90%;
[0179] S5. Take 100g of silicon wafer-welding strip mixture into a reactor, add 500mL of 0.1mol / L sulfuric acid solution, and filter to obtain aluminum-containing leaching solution and silver-containing silicon powder-welding strip (Cu / Pb / Sn). The aluminum leaching rate can reach more than 90%;
[0180] The aluminum-containing leachate is directly sent to the aluminum-containing leachate treatment process of silicon wafers, and the product aluminum hydroxide is obtained through neutralization and hydrolysis;
[0181] Silver-containing silicon powder-welding strip (Cu / Pb / Sn) is treated with 200mL 0.1mol / L hydrochloric acid solution, and after filtration, copper strips, leaching solutions containing tin and lead, and silver-containing silicon powder are obtained. The grade of the copper strips is greater than 99%, and the copper strips can be used directly;
[0182] The silver-containing silicon powder is directly sent to the silicon wafer for treatment, and the product silicon powder and silver chloride are obtained through nitric acid leaching and sodium chloride precipitation;
[0183] The leaching solution containing tin and lead was treated with 20 mL of 0.25 mol / L sodium sulfate (Na 2 SO 4 ) solution precipitation, after filtering, the product lead sulfate and tin-containing leaching solution were obtained. During the process, nitrogen was introduced at all times to keep the solution in an oxygen-free atmosphere. The lead recovery rate was 88.5%;
[0184] The tin-containing leaching solution is directly sent to the tin-containing leaching solution treatment process of the solder strip, and the product tin dioxide is obtained after air oxidation, and the tin recovery rate can reach 90%.
[0185] Example 3
[0186] like Figure 1 As shown, a method for recovering metals from retired photovoltaic laminates comprises the following steps:
[0187] S1. Decommissioned photovoltaic laminates (such as Figure 2 As shown) are mechanically separated to obtain a mixture of initial silicon wafers and initial solder strips, as well as photovoltaic glass and backplane;
[0188] S2, subjecting the mixture of the initial silicon wafer and the initial solder strip obtained in S1 to color sorting, and obtaining silicon wafers, solder strips and a silicon wafer-solder strip mixture after sorting, respectively, with a sorting efficiency of 80%;
[0189] S3, take 500g of the silicon wafer obtained in S2 and place it in a reactor, add 2L of 0.1mol / L sulfuric acid solution, heat it to 60°C, start stirring and react for 30min, filter to obtain aluminum-containing leaching solution and silver-containing silicon powder, and the aluminum leaching rate can reach more than 90%;
[0190] The aluminum-containing leachate is neutralized and hydrolyzed, the temperature is controlled at room temperature, and the hydrolysis efficiency is 70%;
[0191] The silver-containing silicon powder is treated with 100 mL of 0.1 mol / L nitric acid solution, and a silver-containing leaching solution and silicon powder are obtained after filtration, wherein the silver leaching rate is 85%, and the grade of the obtained silicon powder is greater than 90%. The silver-containing silicon powder needs to be further treated;
[0192] Add 20mL of 0.5mol / L sodium chloride solution to the silver-containing leaching solution, and obtain the product silver chloride after filtering, with a silver recovery rate of 80%;
[0193] S4, take 500g of solder strip and place it in a reactor, add 4L 0.5mol / L CuSO 4 and 0.2mol / LH 2 SO 4 The mixture is subjected to a replacement reaction, the temperature is controlled at room temperature, the rotation speed is 600 rpm, and nitrogen is introduced to keep the mixed solution in an oxygen-free atmosphere. After filtration, the products of lead sulfate and copper strips, as well as a tin-containing leaching solution are obtained. The lead recovery rate is 80%, of which the copper strip grade is 70%, and the copper strip needs to be further impurity-removed;
[0194] The tin-containing leaching solution is placed in the air for 1 hour, and then filtered to obtain the product tin dioxide after air oxidation. The recovery rate of tin can reach more than 90%;
[0195] S5, take 100g of silicon wafer-welding strip mixture into a reactor, add 500mL of 0.1mol / L sulfuric acid solution, filter to obtain aluminum-containing leaching solution and silver-containing silicon powder-welding strip (Cu / Pb / Sn), and the aluminum leaching rate can reach more than 90%;
[0196] The aluminum-containing leachate is directly sent to the aluminum-containing leachate treatment process of silicon wafers, and the product aluminum hydroxide is obtained through neutralization and hydrolysis;
[0197] Silver-containing silicon powder-welding strip (Cu / Pb / Sn) is treated with 100mL 0.1mol / L hydrochloric acid solution, and after filtration, copper strips, leaching solutions containing tin and lead, and silver-containing silicon powder are obtained. The grade of the copper strips is 85%, and further impurity removal is required;
[0198] The silver-containing silicon powder is directly sent to the silicon wafer for treatment, and the product silicon powder and silver chloride are obtained through nitric acid leaching and sodium chloride precipitation;
[0199] The leaching solution containing tin and lead was treated with 20 mL of 0.25 mol / L Na 2 SO 4 The solution was precipitated and filtered to obtain the product lead sulfate and tin-containing leaching solution. Nitrogen was introduced at all times during the process to keep the solution in an oxygen-free atmosphere. The lead recovery rate was 88.5%;
[0200] The tin-containing leaching solution is directly sent to the tin-containing leaching solution treatment process of the solder strip, and the product tin dioxide is obtained after air oxidation, and the tin recovery rate can reach 90%.
[0201] Comparative Example 1
[0202] A method for recovering metals from retired photovoltaic laminates comprises the following steps:
[0203] S1, mechanically separating the retired photovoltaic laminates to obtain initial silicon wafers, initial solder strips, photovoltaic glass and backplane;
[0204] S2, take 500g of the initial silicon wafer and initial solder strip obtained in S1 and place them in a reactor, add 2L of 0.1mol / L sodium hydroxide solution, heat to 60°C, start stirring and react for 30min, filter to obtain aluminum-containing leaching solution, copper-lead-tin soldering rod and silver-containing silicon powder, and the aluminum leaching rate is 85%;
[0205] Add water of the same proportion to the aluminum-containing leachate for neutralization and hydrolysis, and control the temperature at 65°C to promote the hydrolysis of aluminum ions to obtain the product aluminum hydroxide, with a hydrolysis efficiency of up to 99.5%;
[0206] Silver-containing silicon powder and copper-lead-tin welding rods are treated with 200mL 0.1mol / L hydrochloric acid solution, and after multiple filtrations, copper strips, leaching solutions containing tin and lead, and silver-containing silicon powder are obtained. The grade of the copper strips is 90%, and further impurity removal is required. The copper strips are the welding strips after the reaction, such as Figure 5 As shown, the XRD test diagram of the solder strip after the reaction is as follows Figure 6 As shown;
[0207] The silver-containing silicon powder is leached with nitric acid and precipitated with calcium chloride to obtain silicon powder and silver chloride. The silicon powder grade is 80% and the silver recovery rate is 85%.
[0208] The leaching solution containing tin and lead was treated with 20mL 0.5mol / LNa 2 SO 4 After precipitation and filtration, the product lead sulfate and tin-containing leaching solution are obtained, and the lead recovery rate is 90%;
[0209] The tin-containing leaching solution is oxidized by air to obtain the product tin dioxide, and the tin recovery rate can reach 60%.
[0210] Detection and analysis
[0211] 1) After dilution and filtration, the liquid sample in the implementation case was tested for the metal ion concentration by inductively coupled plasma ICP-AES (iCAP6300, Thermo), and the results are shown in Table 1;
[0212] After testing, the composition of the tin-containing leaching solution obtained in Example 1 is shown in Table 1.
[0213] Table 1 Composition of solder strip leaching solution
[0214] element Cu(mol / L) Pb(ppm) Sn(ppm) content 0.14 1.54 10.11
[0215] 2) The solid sample of the retired photovoltaic laminate used in Example 1 was digested, diluted and filtered, and the metal ion concentration contained therein was detected by ICP-AES (iCAP6300, Thermo). The results are shown in Table 2.
[0216] After testing, the components of the retired photovoltaic laminate in Example 1 are shown in Table 2.
[0217] Table 2 Composition of retired photovoltaic laminates
[0218] type Glass Organic matter Silicon Wafer copper silver aluminum lead tin wt / % 83.54 10.69 3.65 1.22 0.06 0.61 0.09 0.15
[0219] 3) The silicon powder obtained in S3 of Example 1 was subjected to qualitative analysis by XRD analysis. The specific working parameters were: scanning speed of 5° / min and scanning range of 10-80°. The results are shown in FIG. Figure 3 shown.
[0220] From the analysis in 3, it can be seen that the main component of the product silicon powder is silicon, and the removal effect of copper and aluminum is good. The product silicon powder can be directly recycled.
[0221] In summary, the method of recovering metals from retired photovoltaic laminates of the present invention realizes the selective separation and recovery of various metals in retired photovoltaic modules by cleverly using the different redox potentials of various metals in silicon wafers and solder strips of retired photovoltaic laminates. For silicon wafers (Si-Ag-Al), by simply and cleverly using acid leaching treatment, the selective separation of metallic aluminum is effectively achieved, and the product silicon wafers and silver chloride are obtained by using nitric acid leaching-sodium chloride precipitation method. For the solder strip (Cu-Pb-Sn) system, by simply and cleverly using the copper sulfate-sulfuric acid system, the selective separation of copper, lead and tin is effectively achieved, and the product copper and lead sulfate can be directly used, and the tin-containing solution can be directly oxidized to obtain the product tin oxide. For the silicon wafer-welding strip (Si-Ag-Al-Cu-Pb-Sn) system, the selective separation of metallic aluminum is effectively achieved by simply and cleverly using sulfuric acid leaching; the selective separation of copper and silver as well as lead and tin is achieved by using hydrochloric acid leaching; the further separation and purification of lead and tin solutions are effectively achieved by chemical precipitation; the silver-containing silicon powder can be directly sent to the silicon wafer system, and the product silicon wafer and silver chloride are obtained by the same nitric acid leaching-sodium chloride precipitation method. The above method not only effectively realizes the efficient recovery of various valuable metals, but also realizes the use of multiple process production lines, reduces production costs, has the advantages of low energy consumption, high product value and environmental friendliness, and conforms to the concept of circular economy. In addition, the method of the present invention fully considers the recovery of multiple metals under different systems in the industrial recycling process, has a wide range of process applications, has promotion and application value, and is suitable for industrial promotion in the field of photovoltaic module recycling technology.
[0222] The above embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Any equivalent substitution or change made by a person skilled in the art based on the present invention is within the protection scope of the present invention.
Claims
1. A method for recovering metals from retired photovoltaic laminates, It is characterized in that The following steps are involved: Pre-treating the retired photovoltaic laminate to obtain a mixture containing initial silicon wafers and initial solder strips; Physically sorting the mixture of the initial silicon wafer and the initial solder strip to obtain silicon wafers, solder strips and a silicon wafer-solder strip mixture; The silicon wafer is subjected to acid leaching treatment to obtain an aluminum-containing leaching solution and silver-containing silicon powder; In an oxygen-free atmosphere, the solder strip is placed in a sulfuric acid-copper sulfate mixed solution to undergo a replacement reaction to obtain lead sulfate, tin-containing leaching solution and pure copper strip; The silicon wafer-welding strip mixture is subjected to acid leaching to obtain an aluminum-containing leaching solution and a silver-containing silicon powder-welding strip; The aluminum-containing leachate is subjected to a neutralization reaction to obtain aluminum hydroxide; The silver-containing silicon powder-welding strip is treated with a hydrochloric acid solution to obtain a copper strip, a leaching solution containing tin and lead, and a silver-containing silicon powder; The silver-containing silicon powder is treated with acid to obtain a silver-containing leaching solution and silicon powder, and a chloride salt is added to the silver-containing leaching solution to obtain silver chloride; The leaching solution containing tin and lead is subjected to sulfate precipitation to obtain lead sulfate and tin-containing leaching solution; The tin-containing leaching solution is oxidized to obtain tin dioxide.
2. The method for recovering metals from retired photovoltaic laminates according to claim 1, It is characterized in that The acid leaching treatment of the silicon wafer comprises: leaching the silicon wafer with a sulfuric acid solution; And / or, the acid leaching treatment of the silicon wafer-welding strip mixture is: leaching the silicon wafer-welding strip mixture with a sulfuric acid solution.
3. The method for recovering metals from retired photovoltaic laminates according to claim 2, It is characterized in that The concentration of sulfuric acid in the sulfuric acid solution is 0.1-2 mol / L; and / or, the silicon wafer and sulfuric acid solution are calculated in kg:L at 1kg:2-6L; And / or, the leaching treatment temperature is 20°C to 80°C; And / or, the leaching treatment time is 30min to 90min; And / or, the silicon wafer-welding ribbon mixture and the sulfuric acid solution are in a ratio of 1kg:1 to 5L in terms of kg:L.
4. The method for recovering metals from retired photovoltaic laminates according to claim 1, It is characterized in that In the sulfuric acid-copper sulfate mixed solution, the concentration of copper sulfate is 0.1-1 mol / L, and the concentration of sulfuric acid is 0.1-2 mol / L; and / or, the welding strip and the sulfuric acid-copper sulfate mixed solution are calculated in kg:L as 1kg:1 to 10L; And / or, the temperature of the replacement reaction is 30°C to 80°C; And / or, the replacement reaction time is 10 min to 60 min.
5. The method for recovering metals from retired photovoltaic laminates according to claim 1, It is characterized in that The aluminum-containing leachate is subjected to a neutralization reaction to obtain aluminum hydroxide: the aluminum-containing leachate is subjected to a neutralization reaction using a sodium hydroxide solution to obtain aluminum hydroxide and a sodium sulfate solution; The concentration of sodium hydroxide in the sodium hydroxide solution is 0.1-2 mol / L; The temperature of the neutralization reaction is 30°C to 70°C; The neutralization reaction time is 30min to 90min; The sodium sulfate solution is used to precipitate the leaching solution containing tin and lead, so as to realize the recycling of sodium sulfate.
6. The method for recovering metals from retired photovoltaic laminates according to claim 1, It is characterized in that The concentration of hydrochloric acid in the hydrochloric acid solution is 0.05-1 mol / L; and / or, the silver-containing silicon powder-welding strip and hydrochloric acid solution are calculated in kg:L as 1kg:1-5L; And / or, the silver-containing silicon powder-welding strip is treated with a hydrochloric acid solution for a time period of 30° C. to 70° C.; And / or, the silver-containing silicon powder-welding strip is treated with the hydrochloric acid solution for 20 minutes to 90 minutes.
7. The method for recovering metals from retired photovoltaic laminates according to claim 1, It is characterized in that The acid treatment of the silver-containing silicon powder comprises: treating the silver-containing silicon powder with a nitric acid solution; The concentration of nitric acid in the nitric acid solution is 0.2-1 mol / L; The silver-containing silicon powder and nitric acid solution are calculated in kg:L at 1kg:1-3L; The temperature for treating the silver-containing silicon powder with the nitric acid solution is 50° C. to 90° C.; The time for treating the silver-containing silicon powder with the nitric acid solution is 20 minutes to 90 minutes.
8. The method for recovering metals from retired photovoltaic laminates according to claim 1, It is characterized in that The oxidation treatment of the tin-containing leaching solution comprises: introducing oxygen into the tin-containing leaching solution for treatment.
9. The method for recovering metals from retired photovoltaic laminates according to claim 1, It is characterized in that The pretreatment of the retired photovoltaic laminates comprises: treating the retired photovoltaic laminates by mechanical separation, heat treatment and solvent leaching.
10. The method for recovering metals from retired photovoltaic laminates according to claim 1, It is characterized in that The retired photovoltaic laminate is selected from at least one of a polycrystalline silicon retired photovoltaic laminate, a monocrystalline silicon retired photovoltaic laminate, a double-glass retired photovoltaic laminate and a single-glass retired photovoltaic laminate.
Citation Information
Patent Citations
Method for comprehensively recovering all components of waste crystalline silicon photovoltaic module
CN114833176A
Comprehensive recovery method of waste photovoltaic module
CN115647007A
Method for recycling all components of scrapped photovoltaic module
CN116371879A
Cited By
Step recovery method for key components of core laminated structure of waste photovoltaic module
CN121446807A