A method for selectively separating thallium from thallium-containing waste
By grinding and mixing calcium oxide and baking the thallium-containing waste, the problems of poor application and high cost in the prior art are solved, and the selective separation and recycling of thallium are realized, thereby reducing environmental risks and treatment costs.
Patent Information
- Application Number
- CN202310205228.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-02
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-03-02
AI Technical Summary
The prior art has poor application and high cost when dealing with thallium-containing waste, making it difficult to selective separation of thallium, resulting in low resource utilization and high environmental pollution risk.
By grinding the thallium-containing waste and mixing it with calcium oxide and then roasting, the thallium-containing phase structure is destroyed by high temperatures around 700°C, volatilization of other metals is inhibited, and the selective separation and recovery of thallium is achieved.
It effectively avoids environmental pollution, reduces treatment costs, improves the resource reuse rate of thallium, realizes selective separation and recycling of thallium, and reduces the environmental risks of waste.
Smart Images

Figure CN116287731B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to waste treatment, in particular to a method for selectively separating thallium from thallium-containing waste. Background Art
[0002] Thallium-containing wastes generated in the production processes of nonferrous metallurgy, steel metallurgy and chemical industry have brought great risks to the ecological environment and reduced the resource utilization rate of thallium. In the prior art, in order to achieve the separation and enrichment of thallium, wet treatment is often used to recover thallium from thallium-containing wastes.
[0003] For example, the Chinese invention patent with publication number CN112981124A has developed a method for separating and enriching thallium from thallium-containing oxidized waste residues, which involves slurrying, dissolution, liquid-solid separation and precipitation. In the specific operation, alkali must be added first and then acid to achieve cobalt-thallium separation. Although the patent has a certain thallium separation effect, it has the disadvantages of a wide variety of additives, large consumption and high cost. It is not a better choice for selectively separating thallium from thallium-containing wastes in industry. Therefore, the applicability of the prior art to treat thallium-containing wastes is poor.
[0004] In view of this, it is necessary to provide a method for selectively separating thallium from thallium-containing wastes to solve or alleviate the technical defect of the above-mentioned prior art in treating thallium-containing wastes with poor applicability. Summary of the invention
[0005] The main purpose of the present invention is to provide a method for selectively separating thallium from thallium-containing waste, aiming to solve the technical problem that the above-mentioned prior art has poor applicability in treating thallium-containing waste.
[0006] To achieve the above object, the present invention provides a method for selectively separating thallium from thallium-containing waste, comprising the steps of:
[0007] S1, grinding the thallium-containing waste to obtain a grinding product;
[0008] Wherein, the thallium-containing waste is a solid, and the thallium-containing waste includes zinc sulfate;
[0009] S2, mixing the ground product and calcium oxide to obtain a pretreated product;
[0010] S3, calcining the pretreated product to obtain thallium-containing volatiles and thallium-removing slag;
[0011] Wherein, the temperature of the calcination treatment is 650-750°C, and the duration of the calcination treatment is not less than 1 hour.
[0012] Furthermore, the thallium-containing waste includes thallium-containing smoke generated during zinc smelting.
[0013] Furthermore, the content of thallium in the thallium-containing smoke is 0.5-0.7wt%.
[0014] Furthermore, the particle size of the ground product is not greater than 100 mesh.
[0015] Furthermore, the thallium-containing solid waste also includes valuable metal fluorine-chloride compounds, and the valuable metal fluorine-chloride compounds include one or more of lead fluorine-chloride compounds, zinc fluorine-chloride compounds and cadmium fluorine-chloride compounds.
[0016] Furthermore, the mass proportion of the calcium oxide in the pretreated material is not less than 5%.
[0017] Furthermore, the mass proportion of the calcium oxide in the pretreated material is not less than 10%.
[0018] Furthermore, the step S1 further comprises: drying the thallium-containing waste before grinding the thallium-containing waste.
[0019] Furthermore, in the step S2, the mixing process includes: grinding the ground product and the calcium oxide together to obtain a primary mixture; and then, oscillating the primary mixture to obtain the pretreated product.
[0020] Furthermore, the calcination process is performed in an air atmosphere.
[0021] Compared with the prior art, the present invention has at least the following advantages:
[0022] The invention provides a method for selectively separating thallium from thallium-containing wastes, which can effectively avoid the pollution of the environment by the thallium-containing wastes, and at the same time selectively separate thallium from the thallium-containing wastes to reuse resources to the greatest extent.
[0023] Specifically, the present invention uses calcium oxide as a phase conversion agent and is assisted by high-temperature treatment at about 700°C to destroy the structure of the thallium-containing phase, inhibit the volatilization of other metals, and achieve selective separation of thallium. Compared with other treatment methods, the present invention avoids the twists and turns of the wet method, has a lower treatment cost and a higher volatilization efficiency. The thallium-free slag obtained after volatilization can be returned to the lead-zinc smelting system for secondary utilization, achieving the separation and recovery of thallium, while greatly reducing the environmental risk of thallium-containing waste. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0025] Figure 1 is the XRD diagram of the thallium-containing soot in Example 1 of the present invention;
[0026] Figure 2 The chemical phase analysis results of water-soluble zinc and oxidized zinc as the roasting temperature changes in Example 2 of the present invention, and the variation law diagram of thallium volatility;
[0027] Figure 3 The chemical phase analysis results of lead chloride, lead sulfate and lead oxidation as the roasting temperature changes in Example 2 of the present invention, and the variation regularity diagram of thallium volatility;
[0028] Figure 4 The chemical phase analysis results of water-soluble zinc and oxidized zinc as the oxygen concentration changes in Example 3 of the present invention, and the variation law diagram of thallium volatility;
[0029] Figure 5 The chemical phase analysis results of lead chloride, lead sulfate and lead oxidation as the oxygen concentration changes in Example 3 of the present invention, and the variation law of thallium volatilization rate are shown.
[0030] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0033] It should be understood that thallium is a typical rare dispersed element in nature, widely found in primary metal minerals. Thallium has many characteristics such as improving alloy strength, improving alloy hardness, and enhancing alloy corrosion resistance. Thallium-containing alloys have potential application value in optical fibers, superconducting materials, infrared optical materials, radiation shielding materials, catalysts, etc.
[0034] At present, smelting enterprises are faced with the problems of high pollution, high disposal costs and selective separation and recovery of thallium in slag caused by thallium-containing waste. However, the existing technology for the treatment of thallium-containing waste is not fully suitable for industrial applications, and is not very targeted for specific thallium-containing waste (the existing treatment of thallium-containing waste slag does not involve thallium-containing smoke).
[0035] Based on this, in order to achieve the selective separation of thallium from thallium-containing waste under the premise of being applicable to industrial applications, complete the enrichment of thallium and the harmlessness and resource utilization of roasted materials, the present invention provides a method for selectively separating thallium from thallium-containing waste, comprising the steps of:
[0036] S1, grinding the thallium-containing waste to obtain a grinding product.
[0037] The ground product may be in granular form. For example, the particle size of the ground product may be no greater than 100 mesh, and may specifically be 100-400 mesh.
[0038] The thallium-containing waste contains thallium element; the thallium-containing waste may also contain one or more of lead element, zinc element and cadmium element.
[0039] In terms of specific phase types, the thallium-containing solid waste includes zinc sulfate, in which thallium element is present, that is, the phase of thallium present includes or is zinc sulfate; the thallium-containing solid waste may also include one or more of lead sulfate and cadmium sulfate.
[0040] Furthermore, the thallium-containing solid waste may also include valuable metal fluorine and chlorine compounds; and the thallium-containing solid waste may also include valuable metal oxides. It should be noted that the valuable metal in the present invention refers to other metals except thallium.
[0041] The valuable metal fluorine-chloride compound may include or be one or more of lead fluorine-chloride compounds, zinc fluorine-chloride compounds and cadmium fluorine-chloride compounds; the fluorine-chloride compound may contain one or both of fluorine and chlorine, or may contain both fluorine and chlorine. The metal oxide may include or be one or more of lead oxide, zinc oxide and cadmium oxide.
[0042] The thallium-containing waste is a solid material, and specifically may include or be thallium-containing smoke generated during zinc smelting. The thallium-containing smoke may include or be thallium-containing high-fluorine and chlorine smoke. The thallium content in the thallium-containing high-fluorine and chlorine smoke (thallium-containing smoke) may be 0.5-0.7wt%, usually 0.6-0.7wt%. The thallium in the thallium-containing high-fluorine and chlorine smoke is basically present in zinc sulfate. The thallium element in the thallium-containing high-fluorine and chlorine smoke includes or is monovalent thallium.
[0043] It should be noted that when the thallium-containing high-fluorine and chlorine smoke or other waste contains thallium in other valence states, it does not affect the implementation of the present application.
[0044] In order to facilitate the treatment of the thallium-containing waste, the step S1 may further include: before grinding the thallium-containing waste, drying the thallium-containing waste to a constant weight; the drying temperature may be 60-100°C, such as 80°C.
[0045] S2, mixing the ground product and calcium oxide to obtain a pretreated product.
[0046] In order to ensure the release of thallium and the conversion of valuable metals, the mass proportion of calcium oxide in the pretreatment material may be no less than 5%; preferably, the mass proportion of calcium oxide in the pretreatment material may be no less than 10%, illustratively, it may be 10-20%.
[0047] In order to ensure that the thallium-containing waste and the calcium oxide are in full contact, in the step S2, the mixing process includes: grinding the ground product and the calcium oxide together to obtain a primary mixture; then, oscillating the primary mixture to obtain the pre-treated product. The particle size standard of the primary mixture can be consistent with that of the ground product, and the oscillation time can be not less than 0.5h, preferably 0.5-3h.
[0048] S3, calcining the pretreated product to obtain separated thallium-containing volatiles and thallium-free slag (calcined slag). Specifically, during the calcining process, the thallium-containing volatiles generated during the calcining process can be collected synchronously to recover the separated thallium.
[0049] The collection process may be: conveying the volatiles to a condenser or other condensation device to condense the volatiles, thereby obtaining thallium-containing recovered materials.
[0050] In order to ensure the selective separation of thallium, the temperature of the roasting treatment is 650-750°C, preferably 700°C; the duration of the roasting treatment is not less than 1 hour, preferably 1-3 hours. In addition, the roasting treatment is generally carried out in a furnace, and the temperature increase of the pretreated material and the temperature decrease of the residue can be carried out in a furnace-associated manner.
[0051] In order to ensure the progress of the reaction during the calcination process, the calcination treatment cannot be carried out in a reducing atmosphere, and the calcination treatment can usually be carried out in an air atmosphere or an inert atmosphere.
[0052] The main principles of the present invention include:
[0053] In order to achieve the selective volatilization of thallium, the volatilization conditions of thallium compounds must be met in thermodynamics and kinetics, that is, the critical temperature for the volatilization of thallium-containing compounds must be reached, and at the same time, the thallium contained in other compounds must be released. Therefore, it is necessary to regulate the reaction, roasting temperature and roasting time in the thallium-containing smoke, and control the relevant conditions and parameters to achieve the selective volatilization of thallium.
[0054] 1. The main reasons why the additive is CaO in the present invention include:
[0055] 1) There is a strong correlation between the thallium in the thallium-containing high-fluorine and chlorine smoke (thallium-containing waste) and the zinc sulfate phase. The release and selective volatilization of thallium can be achieved by destroying the zinc sulfate structure. CaO can react with the zinc sulfate phase to convert it into zinc oxide and calcium sulfate, thereby releasing thallium.
[0056] Although other substances may also exist in the thallium-containing high-fluorine and chlorine smoke, since zinc sulfate has a strong correlation with the thallium in the thallium-containing smoke (zinc sulfate and thallium), the thallium in the thallium-containing high-fluorine and chlorine smoke is basically stored in zinc sulfate. Therefore, zinc sulfate needs to be converted to efficiently release thallium.
[0057] 2) Valuable metal fluorine and chlorine compounds have a low volatility point. CaO can react with valuable metal fluorine and chlorine compounds to convert them into oxides, thereby reducing the volatility of valuable metals during the roasting process.
[0058] 2. The main reasons for determining the roasting temperature to be 650-750°C in the present invention include:
[0059] 1) Thallium begins to volatilize at temperatures above 600°C and volatilizes in large quantities at 700°C.
[0060] 2) Valuable metals such as lead, zinc, and cadmium are converted into oxides, and a large amount of volatilization occurs when the temperature is higher than 700°C (the specific volatilization effect is subject to the examples and comparative examples).
[0061] In order to facilitate those skilled in the art to understand the present invention in detail, examples are given below:
[0062] Example 1
[0063] Sampling and Analysis of Thallium-Containing Dust
[0064] Take the thallium-containing high-fluorine and chlorine smoke (thallium-containing smoke) generated in the zinc smelting process, dry (80°C forced air drying oven) to constant weight and then grind (grind until it can pass through a 100-mesh sieve), digest the ground thallium-containing smoke, measure the element content in the thallium-containing smoke, and perform phase analysis.
[0065] In this embodiment, the thallium content in the thallium-containing smoke was measured to be 0.66wt%. It should be noted that the thallium element is unevenly distributed in the thallium-containing high-fluorine and chlorine smoke, and the thallium content of the smoke as a whole is between 0.6 and 0.7wt%. The volatilization rate of thallium in the subsequent embodiments and comparative examples is calculated based on the content obtained by this digestion.
[0066] The specific analysis results are as follows:
[0067] 1. See Figure 1 According to the chemical phase analysis, in this embodiment, the main phases of the thallium-containing smoke include zinc oxide, lead oxide, zinc sulfate (water-soluble zinc), lead sulfate, lead chloride, and zinc chloride, and the existing forms include crystalline and amorphous states.
[0068] 2. In this embodiment, the mass percentages of the main elements in the thallium-containing smoke are shown in the following table:
[0069] element Zn Pb S Cd Fe F Tl Cl O content(%) 38.1 17.75 6.135 1.98 3.22 0.93 0.66 4.87 22.5
[0070] It can be seen from the above table that thallium-containing smoke mainly contains valuable metal elements such as Zn and Pb.
[0071] 3. In this embodiment, the chemical phase analysis results (mass percentage) of Zn are shown in the following table:
[0072]
[0073] 4. In this embodiment, the chemical phase analysis results (mass percentage) of Pb are shown in the following table:
[0074]
[0075] Example 2
[0076] Temperature single factor test
[0077] Take 1 kg of a sample of thallium-containing smoke (same as in Example 1) dried (in a blast drying oven at 80° C.) to constant weight and grind it (grind until it can pass through a 100-mesh sieve) to obtain a grinding product.
[0078] The ground products were calcined at temperatures of 600°C, 700°C, 800°C, 900°C, 1000°C and 1100°C, respectively.
[0079] The process of each roasting is as follows: 15 g of the ground product is placed in a vertical tube furnace for roasting under air atmosphere; the temperature of each roasting is controlled to be the above-mentioned temperatures, the insulation time of each roasting is 1 hour, and after roasting, the roasted slag is cooled to room temperature along with the furnace.
[0080] In this embodiment, the chemical phase analysis results of the water-soluble zinc and oxidized zinc in the roasted slag as a function of the roasting temperature (the mass proportion in the roasted slag), and the variation law of the thallium volatility (as a function of the roasting temperature) are all referred to Figure 2 shown.
[0081] The chemical phase analysis results of lead chloride, lead sulfate and lead oxide in the roasted slag (mass proportion in the roasted slag) and the variation law of thallium volatility (varies with roasting temperature) are shown in Figure 3 shown.
[0082] Example 3
[0083] Oxygen concentration single factor experiment
[0084] Take 1 kg of a sample of thallium-containing smoke (same as in Example 1) dried (in a blast drying oven at 80° C.) to constant weight and grind it (grind until it can pass through a 100-mesh sieve) to obtain a grinding product.
[0085] The ground products were calcined at oxygen concentrations of 0%, 10%, 20%, 30%, 40% and 50%, respectively.
[0086] Each roasting process is as follows: 15 g of the ground product is roasted in a vertical tube furnace under the above oxygen concentration; the roasting temperature is controlled to be 900° C., the holding time for each roasting is 1 hour, and after roasting, the roasted slag is cooled to room temperature along with the furnace.
[0087] In this embodiment, the chemical phase analysis results of the water-soluble zinc and oxidized zinc in the roasted slag as a function of oxygen concentration (mass proportion in the roasted slag), and the variation law of the thallium volatilization rate (as a function of oxygen concentration) are all referred to Figure 4 shown.
[0088] The chemical phase analysis results of the change of lead chloride, lead sulfate and lead oxide in the roasted slag with oxygen concentration (mass proportion in the roasted slag), and the change law of thallium volatility (change with oxygen concentration) are shown in Figure 5 shown.
[0089] Example 4
[0090] Water immersion test
[0091] Take 1 kg of a sample of thallium-containing smoke (same as in Example 1) dried (in a blast drying oven at 80° C.) to constant weight and grind it (grind until it can pass through a 100-mesh sieve) to obtain a grinding product.
[0092] Weigh 0.2000 g of the ground product and place it in a centrifuge tube. Add 50 ml of deionized water to the centrifuge tube, place it in a water bath shaker (150 r / min) at room temperature and shake for 2 hours. Take it out and centrifuge it to separate the solid and liquid. Take the supernatant to test the thallium and zinc content.
[0093] The leaching rate is calculated by combining the two. The mass leaching rate is shown in the following table:
[0094] Thallium leaching rate (%) Water-soluble zinc leaching rate (%) 98.61 100
[0095] Analysis example 1
[0096] Combined with Examples 1-4, the presence of thallium was analyzed
[0097] 1. See Figure 2-5 It can be seen that in the analytical test results of the two groups of single-factor experiments, the thallium volatilization rate showed a significant correlation with the zinc-containing phase, but a weaker correlation with the lead-containing phase, and the regularity was not obvious. Therefore, it is speculated that there is a certain correlation between the occurrence of thallium and the zinc-containing phase.
[0098] For further details, see Figure 2 As the temperature increases, the water-soluble zinc phase decreases, the oxidized zinc phase increases, and the thallium volatilization rate increases. It is speculated that during the heating process, the water-soluble zinc phase is transformed into the oxidized zinc phase and thallium is released at the same time.
[0099] See Figure 4 In the single-factor experiment of oxygen concentration, the water-soluble zinc phase first increased and then decreased, while the oxidized zinc phase and thallium volatilization first decreased and then increased. It is also speculated that this is caused by the mutual transformation between the water-soluble zinc phase and the oxidized zinc phase.
[0100] Combined with the data from the water immersion experiment, it can be seen that during the water immersion process, the water-soluble zinc is completely dissolved, and the thallium is almost completely dissolved. Analysis shows that since the physical structure of the water-soluble zinc is destroyed during the water immersion process, the thallium contained in it is released, resulting in the simultaneous dissolution of both.
[0101] Since there is a strong correlation between the dissolution relationship of water-soluble zinc and thallium, as well as the change law during the roasting process, it is believed that there is a strong correlation between the occurrence of thallium and the water-soluble zinc phase.
[0102] 2. Combined with the main elements involved in thallium-containing dust, the water-soluble zinc involved in the present invention should be zinc chloride and zinc sulfate. Among them, the volatilization temperature of zinc chloride is relatively low (it will volatilize significantly at about 500°C), and the decomposition temperature of zinc sulfate is relatively high (it will start to dissociate at 500-600°C and will dissociate violently at about 930°C).
[0103] In the temperature single-factor experiment, as the temperature increases, the water-soluble zinc phase continues to decrease after exceeding 500°C, and the water-soluble zinc phase decreases significantly in the range of 900-1000°C (the violent dissociation temperature of zinc sulfate), while the thallium volatilization rate increases significantly.
[0104] Therefore, it is believed that the occurrence of thallium is correlated with the zinc sulfate phase, and the occurrence phase of thallium in thallium-containing smoke is zinc sulfate.
[0105] Example 5
[0106] Take 1 kg of a sample of thallium-containing smoke (same as in Example 1) dried (in a blast drying oven at 80° C.) to constant weight and grind it (grind until it can pass through a 100-mesh sieve) to obtain a grinding product.
[0107] Weigh 13.5 g of the ground product (thallium-containing dust after grinding) and 1.5 g of calcium oxide, add the weighed ground product and calcium oxide into a mortar and grind and mix to obtain a primary mixture (the primary mixture can pass a 100-mesh sieve); put the primary mixture into a plastic bottle with a cover, place it on a tumbling oscillator (30 r / min) and oscillate for 2 hours to obtain a pretreated product.
[0108] The obtained pre-treated product was placed in a corundum crucible and placed in a vertical tube furnace for roasting in an air atmosphere. During the roasting process, the roasting temperature was controlled to be 700°C and the holding time was 1 hour. After roasting, the roasted slag was cooled to room temperature along with the furnace.
[0109] The roasted residue is digested and the contents of thallium, lead, zinc and cadmium in the digestion solution are determined.
[0110] According to calculation, in this embodiment, the mass volatilization rate of thallium is 90.06%, and the mass volatilization rates of lead, zinc and cadmium are 2.42%, 10.20% and 10.35% respectively.
[0111] Example 6
[0112] Compared with Example 5, in this example, only the weighing amount of the ground product is adjusted to 12 g, and the weighing amount of calcium oxide is adjusted to 3 g, and other conditions remain unchanged.
[0113] According to calculation, in this embodiment, the mass volatilization rate of thallium is 95%, and the mass volatilization rates of lead, zinc and cadmium are 1.51%, 5.21% and 4.13% respectively.
[0114] Comparative Example 1
[0115] Compared with Example 5, in this comparative example, only the calcination temperature is adjusted to 900° C., and other conditions remain unchanged.
[0116] According to calculation, in this comparative example, the mass volatilization rate of thallium is 98.39%, and the mass volatilization rates of lead, zinc and cadmium are 2.30%, 59.41% and 56.79% respectively.
[0117] Comparative Example 2
[0118] Compared with Example 5, in this comparative example, only the calcination temperature is adjusted to 800° C., and other conditions remain unchanged.
[0119] According to calculation, in this comparative example, the mass volatilization rate of thallium is 94.51%, and the mass volatilization rates of lead, zinc and cadmium are 3.79%, 42.12% and 32.53% respectively.
[0120] Analysis example 2
[0121] Based on Comparative Examples 1-2, it can be seen that:
[0122] When the temperature is too high, although the structure of the thallium-containing phase is destroyed and thallium is completely released, the valuable metals evaporate severely under high temperature conditions, making selective separation impossible.
[0123] Therefore, ensuring the calcination temperature at around 700°C is critical for destroying the structure of the thallium-containing phase and achieving selective volatilization of thallium.
[0124] Comparative Example 3
[0125] Compared with Example 5, in this comparative example, only the calcination temperature is adjusted to 600° C., and other conditions remain unchanged.
[0126] According to calculation, in this comparative example, the mass volatilization rate of thallium is 29.40%, and the mass volatilization rates of lead, zinc and cadmium are 2.64%, 7.41% and 9.35% respectively.
[0127] Comparative Example 4
[0128] Compared with Example 5, in this comparative example, only the calcination temperature was adjusted to 500° C., and other conditions remained unchanged.
[0129] According to calculation, in this comparative example, the mass volatilization rate of thallium is 8.53%, and the mass volatilization rates of lead, zinc and cadmium are 2.18%, 2.45% and 2.53% respectively.
[0130] Analysis example 3
[0131] Based on Comparative Examples 3-4, it can be seen that:
[0132] When the temperature is too low, the structure of the thallium-containing phase is not destroyed and thallium cannot be completely released, resulting in a low thallium volatilization rate.
[0133] Therefore, it is necessary to ensure that the calcination temperature is around 700°C in order to destroy the structure of the thallium-containing phase and achieve the selective volatilization of thallium.
[0134] Comparative Example 5
[0135] Compared with Example 5, in this comparative example, only the weighing amount of the ground product is adjusted to 14.5 g, and the weighing amount of calcium oxide is adjusted to 0.5 g, and other conditions remain unchanged.
[0136] According to calculation, in this comparative example, the mass volatilization rate of thallium is 20.79%, and the mass volatilization rates of lead, zinc and cadmium are 2.10%, 13.79% and 12.73% respectively.
[0137] Based on this comparative example, it can be seen that:
[0138] When the addition ratio of calcium oxide is low, the structure of the thallium-containing phase is not destroyed and thallium cannot be completely released, resulting in a low thallium volatilization rate.
[0139] Therefore, ensuring the proportion of calcium oxide is very necessary to destroy the structure of the thallium-containing phase and achieve the selective volatilization of thallium.
[0140] Comparative Example 6
[0141] Compared with Example 5, this comparative example only replaces calcium oxide with sodium carbonate, and other conditions remain unchanged.
[0142] According to calculation, in this comparative example, the mass volatilization rate of thallium is 75.23%, and the mass volatilization rates of lead, zinc and cadmium are 9.11%, 0.86% and 11.66% respectively.
[0143] Based on this comparative example, it can be seen that:
[0144] Calcium oxide has a specific reaction mechanism in the present application. Under the condition of a roasting temperature of 700° C., if calcium oxide is replaced by sodium carbonate, the volatilization rate of thallium will be reduced.
[0145] The above technical solutions of the present invention are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the contents of the present invention specification under the technical concept of the present invention, or directly / indirectly applied in other related technical fields, are included in the patent protection scope of the present invention.
Claims
1. A method for selectively separating thallium from thallium-containing waste, characterized in that: Includes steps: S1, grinding the thallium-containing waste to obtain a grinding product; Wherein, the thallium-containing waste is solid matter, and the thallium-containing waste includes zinc sulfate; the thallium-containing waste includes thallium-containing smoke generated during zinc smelting; S2, mixing the ground product and calcium oxide to obtain a pretreated product; S3, calcining the pretreated product to obtain thallium-containing volatiles and thallium-removing slag; Wherein, the temperature of the calcination treatment is 650-750°C, and the duration of the calcination treatment is not less than 1 hour.
2. The method for selectively separating thallium from thallium-containing waste according to claim 1, characterized in that: The content of thallium in the thallium-containing smoke is 0.5-0.7wt%.
3. The method for selectively separating thallium from thallium-containing waste according to claim 1, characterized in that: The particle size of the ground product is not greater than 100 meshes.
4. The method for selectively separating thallium from thallium-containing waste according to claim 1, characterized in that: The thallium-containing waste also includes valuable metal fluorine-chloride compounds, and the valuable metal fluorine-chloride compounds include one or more of lead fluorine-chloride compounds, zinc fluorine-chloride compounds and cadmium fluorine-chloride compounds.
5. The method for selectively separating thallium from thallium-containing waste according to claim 1, characterized in that: The mass proportion of the calcium oxide in the pretreated material is not less than 5%.
6. The method for selectively separating thallium from thallium-containing waste according to claim 5, characterized in that: The mass proportion of the calcium oxide in the pretreated material is not less than 10%.
7. The method for selectively separating thallium from thallium-containing waste according to claim 1, characterized in that: The step S1 further includes: drying the thallium-containing waste before grinding the thallium-containing waste.
8. The method for selectively separating thallium from thallium-containing waste according to claim 1, characterized in that: In the step S2, the mixing process includes: grinding the ground product and the calcium oxide together to obtain a primary mixture; and then oscillating the primary mixture to obtain the pretreated product.
9. The method for selectively separating thallium from thallium-containing waste according to any one of claims 1 to 8, characterized in that: The calcination treatment is performed in an air atmosphere.
Citation Information
Patent Citations
Method of separating and enriching thallium from thallium-contained cobalt oxide waste residues
CN112981124A
Method for extracting Zn, In, Cd and Tl from lead and zinc smelting smoke dust
CN104060099A
Thallium-containing wastewater strongly oxidizing, coagulating, adsorbing and recovering process
CN104310672A