Lithium secondary battery
By using a non-aqueous electrolyte with a high content of cyclic phosphite organic solvents and fluorinated ethylene carbonate in lithium secondary batteries, a stable SEI film is formed, which solves the problem of the negative electrode of lithium secondary batteries under high temperature and long-term use. Deterioration and expansion issues significantly improve battery durability and stability.
Patent Information
- Application Number
- CN202380024362.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-09-29
- Filing Date
- 2023-09-26
- Publication Date
- 2024-10-15
Smart Images

Figure CN118786553A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of Korean Patent Application No. 10-2022-0124727 filed on September 29, 2022 in the Korean Intellectual Property Office, the contents of which are incorporated herein by reference. Technical Field
[0003] The invention relates to a lithium secondary battery. Background Art
[0004] Recently, as the application fields of secondary batteries are rapidly expanding to power storage supplies for large devices such as vehicles and power storage systems and power supplies for electrical, electronic, telecommunication and computer electronic equipment, the demand for secondary batteries with high capacity, high output and high stability is increasing.
[0005] In particular, in lithium secondary batteries for vehicles, high capacity, high output and long life characteristics are becoming increasingly important. In order to achieve high capacity of secondary batteries, nickel-rich positive electrode active materials or silicon-based negative electrode active materials with high energy density but low stability can be used.
[0006] When a secondary battery with this condition is operated, the electrolyte deteriorates as charge and discharge proceed, causing side reactions to occur, and the coating film formed on the positive / negative electrode surface or the surface structure of the electrode deteriorates, so transition metal ions may be dissolved from the positive electrode surface. The transition metal ions dissolved in this way may be electrodeposited on the negative electrode, and the passivation ability of the SEI may be reduced, thereby causing defects that deteriorate the negative electrode.
[0007] If the potential of the positive electrode increases, or the battery is exposed to high temperature, the deterioration phenomenon of the secondary battery tends to be further accelerated.
[0008] Furthermore, if a lithium secondary battery is continuously used for a long time or left at a high temperature, gas may be generated, resulting in an increase in the thickness of the battery, a so-called swelling phenomenon, and it is known that the amount of gas generation depends on the state of SEI.
[0009] Therefore, in order to solve these defects, research and development are underway to reduce the swelling phenomenon of secondary batteries and improve high temperature stability by forming a stable SEI film on the negative electrode. Summary of the invention
[0010] Technical issues
[0011] According to the research conducted from various angles to solve these tasks, the present invention provides a lithium secondary battery, which contains a non-aqueous electrolyte organic solvent that can form a stable SEI film by strong reductive decomposition at the negative electrode containing a silicon-based negative electrode active material. The lithium secondary battery of the present invention provides improved high-temperature cycle characteristics and high-temperature storage characteristics, thereby improving overall performance.
[0012] Technical Solution
[0013] To achieve this object, the present invention provides a lithium secondary battery comprising: a positive electrode comprising a lithium nickel cobalt manganese oxide as a positive electrode active material; a negative electrode comprising a negative electrode active material composed of Si; and a non-aqueous electrolyte comprising a lithium salt, an organic solvent and an additive, wherein the organic solvent comprises a compound of formula 1 and fluoroethylene carbonate, and the content of the compound of formula 1 is greater than 15 weight % of the total amount of the non-aqueous electrolyte.
[0014] [Formula 1]
[0015]
[0016] In Formula 1, A is a cyclic phosphite having 2 or 3 carbon atoms, R is an alkylene group having 1 to 5 carbon atoms, and X is a perfluoroalkyl group having 1 to 5 carbon atoms.
[0017] Beneficial Effects
[0018] The present invention relates to a lithium secondary battery including a positive electrode and a negative electrode having high energy density but poor stability, wherein a compound represented by Formula 1 is included as a non-aqueous organic solvent. If the compound represented by Formula 1 is used, a SEI layer that polymerizes with strong reductive decomposition can be formed, especially in a Si negative electrode, thereby improving the durability of the negative electrode even under high voltage and high temperature conditions.
[0019] Specifically, if a small amount of the compound of formula 1 is used at the level of an additive, a polymer may not be formed between the compounds of formula 1, and it is difficult to form a dense SEI layer. However, if a high content of the compound of formula 1 is included at the level of an organic solvent as in the lithium secondary battery of the present invention, a dense and uniform SEI layer with a high proportion of monomers derived from the compound of formula 1 can be formed, and the durability of the negative electrode can be improved. The lithium secondary battery with improved durability of the negative electrode of the present invention exhibits the following effect: even if it is exposed to high voltage and high temperature for a long time and operates, the overall performance will not deteriorate. DETAILED DESCRIPTION
[0020] It will be understood that the words or terms used in the present invention and claims should not be interpreted as the meanings defined in commonly used dictionaries. It will also be understood that based on the inventors can appropriately define the meanings of the words or terms to best explain the principles of the present invention, the words or terms should be interpreted as having a meaning consistent with the technical ideas of the present invention.
[0021] It will also be understood that when used in this specification, the terms "comprising", "providing" or "having" specify the presence of stated features, numbers, steps, elements or a combination thereof, but do not exclude the presence or addition of one or more other features, numbers, steps, elements or a combination thereof.
[0022] In addition, in the term "a to b carbon atoms" in the specification, "a" and "b" represent the number of carbon atoms contained in a specific functional group. That is, the functional group may contain "a" to "b" carbon atoms. For example, "an alkylene group having 1 to 5 carbon atoms" means an alkylene group containing 1 to 5 carbon atoms, i.e., -CH2-, -CH2CH2-, -CH2CH2CH2-, -CH2(CH3)CH-, -CH(CH3)CH2-, -CH(CH3)CH2CH2-, etc.
[0023] Furthermore, in the specification, the term "alkylene group" means a branched or unbranched divalent hydrocarbon group.
[0024] Furthermore, in the specification, alkyl groups, alkylene groups, etc. may all be substituted or unsubstituted.
[0025] In addition, in the specification, alkyl and the like may be substituted or unsubstituted. "Substituted" means that at least one or more hydrogens bonded to carbon are replaced by elements other than hydrogen, unless otherwise defined separately, such as alkyl having 1 to 20 carbon atoms, alkenyl having 2 to 20 carbon atoms, alkynyl having 2 to 20 carbon atoms, alkoxy having 1 to 20 carbon atoms, cycloalkyl having 3 to 12 carbon atoms, cycloalkenyl having 3 to 12 carbon atoms, heterocycloalkyl having 3 to 12 carbon atoms, heterocycloalkenyl having 3 to 12 carbon atoms, aryloxy having 6 to 12 carbon atoms, halogen atoms, nitro, aryl having 6 to 20 carbon atoms, heteroaryl having 2 to 20 carbon atoms, halogenated aryl having 6 to 20 carbon atoms, etc.
[0026] Hereinafter, the present invention will be explained in more detail.
[0027] The lithium secondary battery of the present invention comprises: a positive electrode comprising a positive electrode active material, a negative electrode comprising a negative electrode active material, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte. In this case, the lithium secondary battery of the present invention can be manufactured according to a common method known in the art. For example, the positive electrode, the negative electrode, and the separator between the positive electrode and the negative electrode can be stacked to form an electrode assembly, the electrode assembly can be placed in a battery case, and a non-aqueous electrolyte can be injected.
[0028] Specifically, the lithium secondary battery of the present invention may include: a positive electrode including lithium nickel cobalt manganese oxide as a positive electrode active material; a negative electrode including a silicon-based active material as a negative electrode active material; and a non-aqueous electrolyte including a lithium salt, an organic solvent and an additive.
[0029] The nonaqueous electrolyte contained in the lithium secondary battery of the present invention may include the compound of Formula 1 as an organic solvent.
[0030] [Formula 1]
[0031]
[0032] In Formula 1, A is a cyclic phosphite having 2 to 3 carbon atoms, and in consideration of a smooth ring-opening reaction for forming an SEI layer, A is preferably a cyclic phosphite having 2 carbon atoms.
[0033] In Formula 1, R is an alkylene group having 1 to 5 carbon atoms, preferably an alkylene group having 1 to 3 carbon atoms.
[0034] In Formula 1, X is a perfluoroalkyl group having 1 to 5 carbon atoms, and preferably, X is CF3 or CF2CF3.
[0035] Specifically, the compound of Formula 1 may be a compound of Formula 1-1.
[0036] [Formula 1-1]
[0037]
[0038] In Formula 1-1, R is an alkylene group having 1 to 5 carbon atoms, preferably an alkylene group having 1 to 3 carbon atoms.
[0039] In Formula 1-1, R1 and R2 may each independently be H or an alkyl group of 1 to 3 carbon atoms.
[0040] More specifically, the compound of Formula 1 may be a compound of Formula 1-2.
[0041] [Formula 1-2]
[0042]
[0043] The content of the compound of formula 1 in the lithium secondary battery of the present invention may be greater than 15% by weight of the total amount of the non-aqueous electrolyte, preferably 20% to 50% by weight of the total amount of the non-aqueous electrolyte, and more preferably 30% to 50% by weight. If the content of the compound of formula 1 satisfies the above range, a dense and uniform SEI layer with a high proportion of monomers derived from the compound of formula 1 can be formed, and the durability of the negative electrode can be improved. The lithium secondary battery of the present invention with improved negative electrode durability can show the following effect: even if it is exposed to high voltage and high temperature for a long time and operates, the overall performance will not deteriorate.
[0044] The lithium secondary battery of the present invention comprises a compound represented by Formula 1 and fluoroethylene carbonate (FEC) in a non-aqueous electrolyte. The lithium secondary battery of the present invention comprises a compound of Formula 1 and fluoroethylene carbonate as an organic solvent, and a fluorine-based solid polymer coating film can be formed, and a durable coating film can be formed on the negative electrode. In addition, the coating film derived from phosphite has excellent lithium ion permeability and has a low resistance effect. In the lithium secondary battery of the present invention, the organic solvent contained in the non-aqueous electrolyte is most preferably composed of a compound of Formula 1 and fluoroethylene carbonate.
[0045] The content of fluoroethylene carbonate (FEC) of the lithium secondary battery of the present invention can account for 5% to 80% by weight of the total amount of the non-aqueous electrolyte, preferably 10% to 70% by weight, and more preferably 20% to 50% by weight. If the FEC content meets the above range, a durable coating film can be formed on the negative electrode.
[0046] The non-aqueous electrolyte of the present invention may further include at least one organic solvent selected from the group consisting of cyclic carbonate organic solvents, linear carbonate organic solvents, linear ester organic solvents, and cyclic ester organic solvents.
[0047] Preferably, in addition to the compound represented by Formula 1 as an organic solvent, the non-aqueous electrolyte of the present invention may further include a linear carbonate organic solvent. The linear carbonate organic solvent is an organic solvent with low viscosity and low dielectric constant, and generally, at least one organic solvent selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate and ethyl propyl carbonate can be used, specifically diethyl carbonate (DEC).
[0048] The cyclic carbonate organic solvent is an organic solvent with high viscosity and an organic solvent with a high dielectric constant and which dissociates lithium salts well in the electrolyte, and may specifically include at least one selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), fluoroethylene carbonate (FEC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate and vinylene carbonate.
[0049] Furthermore, the organic solvent may further include at least one or more ester organic solvents selected from the group consisting of linear ester organic solvents and cyclic ester organic solvents in order to prepare an electrolyte having high ion conductivity.
[0050] The linear ester organic solvent may specifically include at least one organic solvent selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate and butyl propionate.
[0051] In addition, the cyclic ester organic solvent may include at least one organic solvent selected from the group consisting of γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone.
[0052] Meanwhile, the organic solvent may be an organic solvent generally used for non-aqueous electrolytes as needed, but is not limited thereto. For example, at least one organic solvent selected from ether organic solvents, glyme organic solvents, and nitrile organic solvents may be further included.
[0053] The ether solvent may include any one selected from the group consisting of dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether, ethyl propyl ether, 1,3-dioxolane (DOL) and 2,2-bis(trifluoromethyl)-1,3-dioxolane (TFDOL), or a mixture of two or more thereof, but is not limited thereto.
[0054] Compared with linear carbonate organic solvents, glycol dimethyl ether solvents have a higher dielectric constant and a lower surface tension, have almost no reactivity with metals, and may include at least one selected from the group consisting of dimethoxyethane (glycol dimethyl ether, DME), diethoxyethane, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether and tetraethylene glycol dimethyl ether (TEGDME), but are not limited thereto.
[0055] The nitrile solvent may be one or more selected from the group consisting of acetonitrile, propionitrile, butyronitrile, valeronitrile, octanonitrile, heptanenitrile, cyclopentanenitrile, cyclohexanenitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, benzyl cyanide, 2-fluorophenyl cyanide and 4-fluorophenyl cyanide, but is not limited thereto.
[0056] The lithium salt contained in the non-aqueous electrolyte of the present invention is used as an electrolyte salt in a lithium secondary battery and as a medium for transmitting ions. Generally, the lithium salt includes Li + As the cation, and as the anion, at least one selected from the group consisting of: F-, Cl-, Br - 、I-、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - , B 10 Cl 10 - 、AlCl4 - 、AlO2 - PF6 - CF3SO3 - 、CH3CO2 - CF3CO2 - 、AsF6 - 、SbF6 - 、CH3SO3 - 、(CF3CF2SO2)2N - 、(CF3SO2)2N - 、(FSO2)2N - 、BF2C2O4 - , BC4O8 - PF4C2O4 - PF2C4O8 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - 、C4F9SO3 - CF3CF2SO3 - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - CF3(CF2)7SO3 - and SCN - .
[0057] Specifically, the lithium salt may include a single material selected from the group consisting of LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10, LiAlCl4, LiAlO2, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, lithium bis(fluorosulfonyl)imide (LiFSI, LiN(SO2F)2), lithium bis(perfluoroethanesulfonyl)imide (LiBETI, LiN(SO2CF2CF3)2) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI, LiN(SO2CF3)2), or a mixture of two or more thereof. In addition, lithium salts commonly used in electrolytes for lithium secondary batteries can be used, but there is no limitation.
[0058] The concentration of the lithium salt can be appropriately changed within the range of common use, but in order to obtain the best formation effect of the coating film for preventing corrosion of the electrode surface, its concentration in the electrolyte can be 0.1 M to 5.0 M, preferably 0.5 M to 3.0 M, and more preferably 1.0 M to 2.0 M. If the concentration of the lithium salt satisfies the above range, the improvement effect of the cycle characteristics of the lithium secondary battery when stored at high temperature can be sufficient, and the viscosity of the non-aqueous electrolyte can be appropriate, and therefore, the impregnation property of the electrolyte can be improved.
[0059] In addition, the non-aqueous electrolyte of the present invention may further contain known electrolyte additives in the non-aqueous electrolyte as needed to prevent the disintegration of the negative electrode caused by the decomposition of the non-aqueous electrolyte in a high-output environment, or to further improve the high-rate discharge properties at low temperatures, stability at high temperatures, prevent overcharging, and inhibit the expansion of the battery at high temperatures.
[0060] Other electrolyte additives may include at least one additive for forming a SEI layer selected from the group consisting of cyclic carbonate compounds, sultone compounds, sulfate compounds, phosphate compounds, borate compounds, nitrile compounds, benzene compounds, amine compounds, silane compounds and lithium salt compounds.
[0061] The cyclic carbonate-based compound may include vinylene carbonate (VC) or vinyl ethylene carbonate.
[0062] The sultone compound may be at least one selected from the group consisting of 1,3-propane sultone (PS), 1,4-butane sultone, ethylene sultone, 1,3-propene sultone (PRS), 1,4-butene sultone, and 1-methyl-1,3-propene sultone.
[0063] The sulfate compound may include ethylene sulfate (Esa), trimethylene sulfate (TMS) or methyl trimethylene sulfate (MTMS).
[0064] The phosphate compound may include one or more compounds selected from the group consisting of lithium difluoro(bisoxalato)phosphate, lithium difluorophosphate, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, tris(2,2,2-trifluoroethyl)phosphate and tris(2,2,2-trifluoroethyl)phosphite.
[0065] The borate ester / salt compounds may include tetraphenylborate, lithium difluorooxalatoborate (LiODFB), and lithium bis(oxalatoborate) (LiB(C2O4)2, LiBOB).
[0066] The nitrile compound may include at least one compound selected from the group consisting of succinonitrile, adiponitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, octanonitrile, heptanenitrile, cyclopentanenitrile, cyclohexanenitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzyl, benzyl cyanide, 2-fluorophenylacetonitrile and 4-fluorophenylacetonitrile.
[0067] The benzene compound may include fluorobenzene, the amine compound may include triethanolamine or ethylenediamine, and the silane compound may include tetravinylsilane.
[0068] The lithium salt-based compound is a compound other than a lithium salt contained in the non-aqueous electrolyte, and may include lithium difluorophosphate (LiDFP), LiPO 2 F 2 , or LiBF 4 .
[0069] Among other electrolyte additives, if a combination of vinylene carbonate (VC), 1,3-propane sultone and 1,3-propylene sultone (PRS) is additionally included, a stronger SEI coating film can be formed on the negative electrode surface during the initial activation process of the secondary battery, the generation of gas due to decomposition of the electrolyte at high temperature can be suppressed, and the stability of the secondary battery at high temperature can be improved.
[0070] Meanwhile, the additional electrolyte additive can be used by mixing two or more additives at 0.1 wt % to 10 wt %, specifically 0.2 wt % to 8 wt %, preferably 0.5 wt % to 8 wt % of the total weight of the non-aqueous electrolyte. If the content of the additional electrolyte additive satisfies the above range, the improvement effect of ion conductivity and cycle characteristics will be better.
[0071] The positive electrode contained in the lithium secondary battery of the present invention may be manufactured by applying a positive electrode mixture slurry including a positive electrode active material, a binder, a conductive agent, and a solvent to a positive electrode collector.
[0072] There is no particular limitation on the positive electrode current collector as long as it does not cause chemical changes in the battery and has conductivity, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used.
[0073] The positive electrode contained in the lithium secondary battery of the present invention may include a lithium nickel cobalt manganese oxide having a high nickel content as a positive electrode active material to increase the energy density. Specifically, the lithium nickel cobalt manganese oxide may have a composition represented by Formula 2.
[0074] [Formula 2]
[0075] Li a Ni b Co c M 1 d M 2 e O2
[0076] In Formula 2, M 1 may be Mn or a combination of Mn and Al, and a combination of Mn and Al is preferred in consideration of enhancing the structural stability.
[0077] M 2 may be one or more selected from the group consisting of Zr, W, Y, Ba, Ca, Ti, Mg, Ta, and Nb.
[0078] a represents the atomic fraction of lithium in the lithium nickel cobalt manganese oxide and may satisfy 0.90 ≤ a ≤ 1.1, preferably 0.95 ≤ a ≤ 1.08, more preferably 1.0 ≤ a ≤ 1.08.
[0079] b represents the atomic fraction of nickel among the metal elements other than lithium in the lithium nickel cobalt manganese oxide and may satisfy 0.80 ≤ b < 1.0, preferably 0.80 ≤ b ≤ 0.95, more preferably 0.80 ≤ b ≤ 0.90. If the nickel content satisfies the above range, high capacity can be achieved.
[0080] c represents the atomic fraction of cobalt among the metal elements other than lithium in the lithium nickel cobalt manganese oxide and may satisfy 0 < c < 0.2, 0 < c ≤ 0.15, or 0.01 ≤ c ≤ 0.10.
[0081] d represents the atomic fraction of M among the metal elements other than lithium in the lithium nickel cobalt manganese oxide 1 and may satisfy 0 < d < 0.2, 0 < d ≤ 0.15, or 0.01 ≤ d ≤ 0.10.
[0082] e represents the atomic fraction of M among the metal elements other than lithium in the lithium nickel cobalt manganese oxide 2 and may satisfy 0 ≤ e ≤ 0.1 or 0 ≤ e ≤ 0.05.
[0083] The content of the positive electrode active material may account for 60 to 99 wt %, preferably 70 to 99 wt %, and more preferably 80 to 98 wt % of the total weight of the solid matter excluding the solvent in the positive electrode mixture slurry.
[0084] The binder is a component that assists bonding of an active material, a conductive agent, etc., and bonding with a current collector.
[0085] The binder may include, for example, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene (PE), polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, various copolymers, and the like.
[0086] Generally, the content of the binder may account for 1 to 20 wt %, preferably 1 to 15 wt %, and more preferably 1 to 10 wt % of the total weight of the solid matter excluding the solvent in the positive electrode mixture slurry.
[0087] The conductive agent is a component for further improving the conductivity of the positive electrode active material, and its addition amount may account for 1 wt % to 20 wt % of the total weight of the solids in the positive electrode mixture slurry. The conductive agent is not specifically limited as long as it does not cause chemical changes in the battery and has conductivity, and may include, for example, carbon powders such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; graphite powders such as natural graphite, artificial graphite, and graphite with a very developed crystal structure; conductive fibers such as carbon fibers and metal fibers; fluorocarbon powders; conductive powders such as aluminum powder and nickel powder; conductive whiskers such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0088] Generally, the content of the conductive agent may account for 1 to 20 wt %, preferably 1 to 15 wt %, and more preferably 1 to 10 wt % of the total weight of the solid matter excluding the solvent in the positive electrode mixture slurry.
[0089] The solvent may include an organic solvent such as N-methyl-2-pyrrolidone (NMP), and when used with the positive electrode active material and the optional binder and the conductive agent, the amount used may provide a preferred viscosity. For example, the content of the solvent may be such that the concentration of the solids containing the positive electrode active material and the optional binder and the conductive agent may be 50% to 95% by weight, preferably 70% to 95% by weight, and more preferably 70% to 90% by weight.
[0090] The negative electrode contained in the lithium secondary battery of the present invention can be manufactured by applying a negative electrode mixture slurry containing a negative electrode active material, a binder, and a solvent to a negative electrode current collector.
[0091] There is no specific limitation on the negative electrode current collector as long as it does not cause chemical changes in the battery and has conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum cadmium alloy, etc. can be used. In addition, similar to the positive electrode current collector, fine irregularities can be formed on its surface to enhance the binding force of the negative electrode active material, and various types such as films, sheets, foils, meshes, porous bodies, foams, and non-woven fabrics can be used.
[0092] The negative electrode contained in the lithium secondary battery of the present invention can contain a silicon-based active material as the negative electrode active material to increase the energy density. The silicon-based active material can include Si, SiO x (0 < x < 2), etc. The negative electrode active material of the present invention may not include conventional negative electrode active materials such as graphite, but may be composed of silicon (Si), etc.
[0093] The content of the negative electrode active material can account for 60% to 99% by weight, preferably 70% to 99% by weight, and more preferably 80% to 98% by weight of the total weight of the solids other than the solvent in the negative electrode mixture slurry.
[0094] The binder is a component that aids in the binding between the conductive agent, the active material, and the current collector. The binder can include, for example, polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, various copolymers, etc.
[0095] Generally, the content of the binder can account for 1% to 20% by weight, preferably 1% to 15% by weight, and more preferably 1% to 10% by weight of the total weight of the solids other than the solvent in the negative electrode mixture slurry.
[0096] The conductive agent is a component for further improving the conductivity of the negative electrode active material, and its content may account for 1% to 20% by weight of the total weight of the solid content of the negative electrode mixture slurry. The conductive agent is not specifically limited as long as it does not cause chemical changes in the battery and has conductivity, and may include, for example, carbon powders such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal carbon black; graphite powders such as natural graphite, artificial graphite, and graphite with a very developed crystal structure; conductive fibers such as carbon fibers and metal fibers; fluorocarbon powders; conductive powders such as aluminum powder and nickel powder; conductive whiskers such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0097] The content of the conductive agent may account for 1 to 20 wt %, preferably 1 to 15 wt %, and more preferably 1 to 10 wt % of the total weight of the solid matter excluding the solvent in the negative electrode mixture slurry.
[0098] The solvent may include water or an organic solvent such as N-methyl-2-pyrrolidone (NMP), and when used together with the negative electrode active material and the optional binder and conductive agent, the amount of the solvent used may provide a preferred viscosity. For example, the content of the solvent may be such that the concentration of the solids containing the negative electrode active material and the optional binder and conductive agent may be 50 wt % to 95 wt %, preferably 70 wt % to 90 wt %.
[0099] As the separator contained in the lithium secondary battery of the present invention, the porous polymer film used as a conventional separator can be used, for example, it can be used alone or as its laminated structure using a porous polymer film formed by polyolefin polymers such as ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer and ethylene / methacrylate copolymer. In addition, commonly used porous nonwovens can be used, such as nonwovens of glass fiber, polyethylene terephthalate fiber with high melting point, but there is no restriction. In addition, in order to ensure heat resistance and mechanical strength, a coated separator comprising a ceramic component or a polymer material can be optionally used with a single layer or multilayer structure.
[0100] The appearance of the lithium secondary battery of the present invention is not particularly limited, but may be a cylindrical type using a can, a prismatic type, a pouch type, or a coin type.
[0101] Hereinafter, the present invention will be explained in more detail with reference to specific embodiments. However, the embodiments are only explanations that help to understand the present invention, and do not limit the scope of the present invention. It is obvious to those skilled in the art that various changes and modifications can be made within the scope and technical spirit of this specification, and these changes and modifications are included in the appended claims.
[0102] Example
[0103] Example 1
[0104] (Preparation of non-aqueous electrolyte)
[0105] The compound of formula 1-2 is mixed with fluoroethylene carbonate (FEC) in a volume ratio of 20:80 to prepare a non-aqueous solvent. 1.5M LiPF6, 0.5 wt% vinylene carbonate (VC), 0.5 wt% 1,3-propane sultone (PS), and 0.5 wt% 1,3-propylene sultone (PRS) are dissolved therein to prepare a non-aqueous electrolyte. In the non-aqueous electrolyte prepared in this way, the content of the compound of formula 1-2 accounts for 16 wt% of the total amount of the non-aqueous electrolyte, and the content of FEC accounts for 71 wt% of the total amount of the non-aqueous electrolyte.
[0106] [Formula 1-2]
[0107]
[0108] (Manufacturing of lithium secondary batteries)
[0109] The positive electrode active material (LiNi 0.86 Co 0.05 Mn 0.07 Al 0.02 O2): Conductive agent (carbon black): Binder (polyvinylidene fluoride) was added to N-methyl-2-pyrrolidone (NMP) solvent to prepare positive electrode slurry (solid content of 50 wt%). The positive electrode slurry was applied to one side of a positive electrode current collector (Al film) with a thickness of 12 μm, dried and rolled to manufacture a positive electrode.
[0110] The negative electrode slurry (solid content of 60 wt%) was prepared by adding negative electrode active material (Si): conductive agent (carbon black): binder (SBR-CMC) in a weight ratio of 95:1.5:3.5 to N-methyl-2-pyrrolidone (NMP) solvent. The negative electrode slurry was applied on one side of a negative electrode current collector (Cu film) with a thickness of 6 μm, dried and rolled to manufacture a negative electrode.
[0111] In a dry room, a polyolefin-based porous separator coated with Al2O3 inorganic particles was placed between the positive electrode and the negative electrode thus formed, and the prepared nonaqueous electrolyte was injected, thereby manufacturing a secondary battery.
[0112] Example 2
[0113] A secondary battery was manufactured by the same method as in Example 1, except that a non-aqueous solvent prepared by mixing a compound of Formula 1-2 with fluoroethylene carbonate (FEC) in a volume ratio of 30:70 was used. In the non-aqueous electrolyte thus prepared, the content of the compound of Formula 1-2 accounted for 25% by weight of the total amount of the non-aqueous electrolyte, and the content of FEC accounted for 62% by weight of the total amount of the non-aqueous electrolyte.
[0114] Example 3
[0115] A secondary battery was manufactured by the same method as in Example 1, except that a non-aqueous solvent prepared by mixing a compound of Formula 1-2 with fluoroethylene carbonate (FEC) in a volume ratio of 50:50 was used. In the non-aqueous electrolyte thus prepared, the content of the compound of Formula 1-2 accounted for 42% by weight of the total amount of the non-aqueous electrolyte, and the content of FEC accounted for 45% by weight of the total amount of the non-aqueous electrolyte.
[0116] Comparative Example 1
[0117] A secondary battery was manufactured by the same method as in Example 1, except that a non-aqueous solvent prepared by mixing a compound of Formula 1-2 with fluoroethylene carbonate (FEC) in a volume ratio of 18:82 was used. In the non-aqueous electrolyte thus prepared, the content of the compound of Formula 1-2 accounted for 15% by weight of the total amount of the non-aqueous electrolyte, and the content of FEC accounted for 72% by weight of the total amount of the non-aqueous electrolyte.
[0118] Comparative Example 2
[0119] A secondary battery was manufactured by the same method as in Example 1, except that graphite was used as the negative electrode active material.
[0120] Comparative Example 3
[0121] A secondary battery was manufactured by the same method as in Example 1, except that a non-aqueous solvent prepared by mixing the compound of Formula 1-2 with ethylene carbonate (EC) at a volume ratio of 20:80 was used. In the non-aqueous electrolyte thus prepared, the content of the compound of Formula 1-2 accounted for 18% by weight of the total amount of the non-aqueous electrolyte, and the content of EC accounted for 66% by weight of the total amount of the non-aqueous electrolyte.
[0122] Experimental Example 1-Evaluation of High Temperature Cycle Characteristics
[0123] For the secondary batteries manufactured in Examples 1 to 3 and Comparative Examples 1 to 3, cycle characteristics were evaluated.
[0124] Specifically, when 1 cycle includes charging at a constant current of 0.33C at 45°C to 4.2V and discharging at a constant current of 0.33C to 3.0V, each battery manufactured in Examples 1 to 3 and Comparative Examples 1 to 3 was charged and discharged for 250 cycles, and after 250 cycles, the capacity retention rate relative to the initial capacity was measured. The results are shown in Table 1.
[0125] [Table 1]
[0126] Capacity retention rate (%) Example 1 83.6 Example 2 85.4 Example 3 90.8 Comparative Example 1 70.4 Comparative Example 2 72.8 Comparative Example 3 78.2
[0127] As shown in Table 1, the secondary batteries of Examples 1 to 3 exhibited higher capacity retention rates and better lifespan characteristics than those of Comparative Examples 1 to 3.
[0128] Experimental Example 2-Evaluation of High Temperature Storage Characteristics
[0129] For the secondary batteries manufactured in Examples 1 to 3 and Comparative Examples 1 to 3, high-temperature storage performance was evaluated.
[0130] Specifically, each of the batteries manufactured in Examples 1 to 3 and Comparative Examples 1 to 3 was fully charged to 4.2 V and then stored at 60° C. for 8 weeks.
[0131] Before storage, the capacity of the fully charged secondary battery was measured and set as the initial capacity of the secondary battery.
[0132] After 8 weeks, the capacity retention rate of the stored secondary battery relative to the initial capacity before storage was measured. The percentage of the secondary battery capacity retention rate relative to the initial capacity of the secondary battery was calculated, and the capacity retention rate after 8 weeks was calculated. The results are shown in Table 2.
[0133] [Table 2]
[0134] Capacity retention rate (%) Example 1 88.9 Example 2 91.2 Example 3 95.4 Comparative Example 1 73.2 Comparative Example 2 75.7 Comparative Example 3 83.1
[0135] As shown in Table 2, compared with the secondary batteries of Comparative Examples 1 to 3, the secondary batteries of Examples 1 to 3 showed higher capacity retention rates and stable high-temperature performance after 8 weeks.
Claims
1. A lithium secondary battery comprising: A positive electrode comprising a lithium nickel cobalt manganese-based oxide as a positive electrode active material; a negative electrode comprising a negative electrode active material composed of Si; and a non-aqueous electrolyte comprising a lithium salt, an organic solvent and an additive, in, The organic solvent comprises a compound of the following formula 1 and fluoroethylene carbonate, and The content of the compound of Formula 1 is greater than 15% by weight of the total amount of the non-aqueous electrolyte: [Formula 1] In Formula 1, A is a cyclic phosphite having 2 or 3 carbon atoms, R is an alkylene group having 1 to 5 carbon atoms, and X is a perfluoroalkyl group having 1 to 5 carbon atoms.
2. The lithium secondary battery according to claim 1, in, The lithium nickel cobalt manganese oxide has a composition represented by the following formula 2: [Formula 2] Li a Ni b Co c M 1 d M 2 e O 2 In Formula 2, M 1 is Mn or a combination of Mn and Al, and M 2 is one or more selected from the group consisting of Zr, W, Y, Ba, Ca, Ti, Mg, Ta, and Nb, 0.8 ≤ a ≤ 1.2, 0.80 ≤ b < 1, 0 < c < 0.2, 0 < d < 0.2, and 0 ≤ e ≤ 0.
1.
3. The lithium secondary battery according to claim 1, in, The organic solvent consists of the compound of Formula 1 and fluoroethylene carbonate.
4. The lithium secondary battery according to claim 1, in, The lithium salt comprises LiPF 6 .
5. The lithium secondary battery according to claim 1, in, R of Formula 1 is an alkylene group having 1 to 3 carbon atoms.
6. The lithium secondary battery according to claim 1, in, X is CF 3 or CF 2 CF 3 .
7. The lithium secondary battery according to claim 1, in, The compound of formula 1 is a compound of the following formula 1-1: [Formula 1-1] In Formula 1-1, R is an alkylene group having 1 to 5 carbon atoms, and R 1 and R 2 Each is independently H or an alkyl group having 1 to 3 carbon atoms.
8. The lithium secondary battery according to claim 1, in, The compound of formula 1 is a compound of the following formula 1-2: [Formula 1-2] 9. The lithium secondary battery according to claim 1, in, The content of the compound of Formula 1 accounts for 20 wt % to 50 wt % of the total amount of the non-aqueous electrolyte.
10. The lithium secondary battery according to claim 1, in, The content of fluoroethylene carbonate is 5 to 80 weight % of the total amount of the non-aqueous electrolyte.