High-flux preparation method suitable for high-density energetic composite material

High-density energetic composite materials are prepared under multi-wetting conditions through 3D printing and laser scanning technology, which solves the problem of alloy preparation of W/Mo elements and BCC matrix systems, realizes composition gradient changes and interface structure optimization, and meets different impact damage The performance of the target matches the requirements.

CN118848014APending Publication Date: 2024-10-29BEIJING INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410937361.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively prepare high-density energy-containing composite materials with high-quality proportions of W/Mo elements and BCC matrix systems. Moreover, alloy preparation is difficult and cannot meet the performance matching needs of different targets for hitting and damaging.

Method used

3D printing coaxial powder feeding technology and layer-by-layer printing are used, combined with rapid solidification and adjustable powder ratio, to prepare wide-component alloy samples with composition gradient changes, and complete the two-phase transition under multi-wetting conditions through multi-pass laser scanning. Through the combination of materials, we can study the interface reaction behavior and establish the relationship between high-density metal and energetic component system-wetting conditions-interface structure-performance.

Benefits of technology

It achieves high-throughput preparation of high-density energy-containing composite materials, provides a reference for the expansion of composite material components and preparation processes, introduces wetting conditions in the composite process through different laser process parameters, analyzes the reaction behavior of the two-phase interface, and quickly obtains good results. Interface structure improves the performance of composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118848014A_ABST
    Figure CN118848014A_ABST
Patent Text Reader

Abstract

The invention relates to a high-flux preparation method suitable for a high-density energetic composite material, and belongs to the technical field of composite materials. A wide-component alloy sample with component gradient change is prepared by utilizing a 3D printing coaxial powder feeding technology and the characteristics of layer-by-layer printing, rapid solidification and adjustable powder proportion, high-density metal powder is scanned on the sample by adopting different laser process parameters in a multi-pass manner, combination between two phases is completed under multiple wetting conditions, and the high-density metal powder is obtained. The high-throughput preparation of the multi-component and multi-wetting-condition alloy sample for researching the interface reaction behavior between the two phases is completed. Establishing a relationship between the high-density metal and the energetic component system-wetting condition-interface structure-performance; and a reference is provided for expanding the components of the high-density energetic composite material and a composite material preparation process through additive manufacturing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high-throughput preparation method suitable for high-density energetic composite materials, belonging to the technical field of composite materials. Background Art

[0002] High-density energetic composite materials are mainly composed of high-density W and Mo elements with high mass ratio and energetic elements with high combustion calorific value such as Ti, Zr, V, Nb, Al, Hf, Ta, etc. W-Zr alloy has high density, high strength and energy release characteristics, but it generates more W 2 The Zr phase makes the alloy lack macroscopic plasticity, and performs poorly in mechanical processing and anti-detonation loading capabilities. By learning from the method of replacing the matrix phase of W-Zr alloy, a high-density energetic composite material with good plasticity is prepared. Among them, energetic alloys rich in elements such as Ti, Zr, and Nb are mainly BCC structures, such as TiZrNb, TiZrVNbAl, etc. However, due to the large differences in physical and chemical properties such as melting points between W / Mo elements and elements such as Ti, Zr, and Nb, and the large mutual diffusion coefficient between W / Mo and BCC matrix, the alloy preparation is difficult. At present, there is little research on the W / Mo element and BCC matrix system.

[0003] In order to quickly expand the composition selection of the energetic matrix phase, high-density energetic composite materials with different compositions and properties are prepared to achieve performance matching for different strike damage targets. Chinese patent CN115152060B discloses a high-throughput preparation method for alloy samples suitable for different solidification kinetics research. Through the characteristics of 3D printing coaxial powder feeding technology and layer-by-layer printing, rapid solidification, and adjustable powder ratio, the preparation of wide-composition samples is completed, and the wide-composition samples are laser scanned twice to analyze the influence of laser process parameters on the organizational structure of wide-composition samples. However, the W / Mo elements with a high mass proportion (>50wt%) cannot be prepared into alloy powders with energetic elements, and the method cannot be used as a guide for the preparation of composite materials. It is necessary to find a new method to provide a reference for the preparation of composite materials. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a high-throughput preparation method suitable for high-density energetic composite materials. By utilizing the coaxial powder feeding technology of 3D printing and the characteristics of layer-by-layer printing, rapid solidification, and adjustable powder ratio, a wide-component alloy sample with a gradient composition change is prepared, and high-density metal powder is scanned multiple times on the sample using different laser process parameters to complete the combination of the two phases under multiple wetting conditions, that is, to complete the high-throughput preparation of multi-component, multi-wetting condition alloy samples for studying the interface reaction behavior between the two phases. Establish the relationship between high-density metal and energetic component system-wetting conditions-interface structure-performance; provide a reference for expanding the composition of high-density energetic composite materials and the process of preparing composite materials by additive manufacturing.

[0005] To achieve the above objectives, the technical solution of the present invention is as follows.

[0006] A high-throughput preparation method for high-density energetic composite materials, the method steps comprising:

[0007] (1) Using two energetic alloy powders A and B as matrix materials, the 3D printing coaxial powder feeding technology is used to adjust the feeding ratio of the two powders, and a wide-composition alloy block with a gradient change in the volume ratio of the two energetic alloys A and B along the deposition direction is deposited on the substrate;

[0008] (2) removing the alloy block from the substrate and uniformly cutting it along the direction of composition change to obtain a plurality of small alloy blocks;

[0009] (3) Using high-density metal as the reinforcement phase, multiple passes of laser scanning of high-density metal powder are performed on the surface of each alloy block. The laser scanning parameters are as follows: laser diameter is 2 to 6 mm, laser power is 500 to 1500 W, laser scanning speed is 2 to 10 mm / s, and powder feeding speed is 4 to 20 r / min. The scanning parameters are different for each pass.

[0010] (4) After the laser scanning is completed, cutting is performed along a direction perpendicular to the direction of composition change of the base material and at the composition change interface.

[0011] Preferably, in step (1), the two energetic alloys A and B are M x N y One of the energetic alloys in the system, with a theoretical energy density ≥10KJ / g; wherein, 85≤x≤100, 0≤y≤15, x+y=100; M is selected from one or more of Ti, Zr, Hf, V, Nb and Ta; and N is selected from one or more of Al, Cr, Mn, Fe, Co, Ni and Cu.

[0012] Preferably, in step (1), the two energetic alloy powders A and B are spherical powders with a particle size of 45 to 150 μm.

[0013] Preferably, in step (1), during 3D printing, the laser spot diameter is 2 to 6 mm, the laser power is 800 to 1400 W, the laser scanning speed is 2 to 10 mm / s, the deposition thickness of each layer is 0.5 to 1 mm, and the fixed spacing between layers is 1.6 to 3.2 mm.

[0014] Preferably, in step (1), the volume ratio of the two energetic alloy powders A and B is changed every 2 to 3 layers of deposition.

[0015] Preferably, in step (1), based on the total volume of the two energetic alloy powders A and B being 100%, the volume content of the energetic alloy powder A is reduced by 10% each time, and the volume content of the energetic alloy powder B is increased by 10% each time.

[0016] Preferably, in step (2), the thickness of the small alloy block is ≥5 mm.

[0017] Preferably, in step (3), the ratio of the powder feeding speed to the scanning speed in each pass is the same.

[0018] Preferably, in step (3), the spacing between two adjacent paths is ≥6 mm.

[0019] Preferably, in step (3), the high-density metal is W powder or Mo powder, and the particle size is 5 to 25 μm.

[0020] Beneficial Effects

[0021] The present invention provides a high-throughput preparation method suitable for high-density energetic composite materials, which utilizes the 3D printing coaxial powder feeding technology and the characteristics of layer-by-layer printing, rapid solidification, and adjustable powder ratio to prepare a wide-composition alloy sample with a composition gradient change, and uses different laser process parameters to scan multiple high-density metal powders on the sample twice to complete the control of the wetting conditions between the two-phase materials, that is, to complete the preparation of multi-component and multi-wetting condition samples for analyzing the interface reaction behavior between the two phases. It provides a reference for expanding the composition of high-density energetic composite materials and the preparation process of composite materials.

[0022] The present invention provides a high-throughput preparation method suitable for high-density energetic composite materials. A good two-phase interface structure is a prerequisite for good performance of the composite block. Different wetting conditions are introduced in the composite process through different laser processes, and the interface reaction behavior between the reinforcement phase and the matrix phase is analyzed, so as to quickly obtain the matrix component material and the process forming window with a good interface structure. The operation is simple and practical. Specifically: the interface structure is an important influencing factor of the performance of the composite material. The molten pool is the smallest processing unit for preparing composite materials by laser instantaneous liquid phase sintering technology. The molten pool formed by the high-density metal and the energetic alloy has a direct effect on the interface wetting, element diffusion / reaction and two-phase combination behavior of the high-density metal and the energetic alloy solution during the rapid heating / cooling and heat preservation process. The interface structure after forming; in addition, the symmetry and regularity of the molten pool have an important influence on the forming of the composite block. The uneven distribution of the solidified structure on both sides of the melt channel will lead to different material and energy transfer conditions in the subsequent cyclic deposition process. There are differences in different tissue locations and components, and it is also easy to cause insufficient fusion and severe heat accumulation, thus affecting the forming quality of the block. Therefore, taking the molten pool as the research object, by introducing different wetting conditions, the influence of different conditions on the two-phase interface behavior in the molten pool is observed; the organizational morphology and properties of the molten pool provide a reference basis for the preparation of bulk alloys.

[0023] The present invention provides a high-throughput preparation method suitable for high-density energetic composite materials. In order to quickly obtain a series of wetting kinetic conditions (the core is the molten pool heating and cooling rate and the liquid phase residence time) in a wide-composition energetic matrix sample, a high-throughput method can be used to efficiently and quickly study the high-density metal-energetic alloy interface reaction behavior, thereby establishing a high-density metal-energetic alloy component system-wetting condition-interface structure-performance relationship. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Schematic diagram of the powder feeding process of single-pass laser secondary scanning in Example 1 and Example 2.

[0025] Figure 2 This is a quantitative schematic diagram of the morphology of the high-density energetic material molten pool in Example 1.

[0026] Figure 3 This is the microstructure morphology of the tungsten-energetic alloy sample prepared in Example 1 under different wetting conditions with the same matrix composition.

[0027] Figure 4 This is the hardness curve at different positions of molten pool No. 2 in Example 1. DETAILED DESCRIPTION

[0028] The present invention is further described below with reference to the accompanying drawings and specific implementation methods. The implementation methods are conventional methods unless otherwise specified, and the raw materials are all available from public commercial channels unless otherwise specified.

[0029] Example 1

[0030] Metal powder W powder, A (Ti 30 Zr 25 V 15 Nb 20 Al 10 )、B(Ti 50 Zr 30 Nb 20 ) as an example, the specific steps of the high-throughput preparation method for high-density energetic composite materials are as follows:

[0031] (1) Select 45-150 μm Ti 30 Zr 25 V 15 Nb 20 Al 10 、Ti 50 Zr 30 Nb 20 The powder is used as the raw material for preparing the alloy matrix. The laser beam works through the laser parameter values ​​and scanning paths pre-set by the machine tool (laser spot diameter 6mm, laser power 1400W, laser scanning speed 10mm / s, deposition thickness of each layer 1mm, fixed spacing between layers 3.2mm), and the alloy powder is sprayed to the center of the molten pool generated by the substrate and the laser beam through the carrier gas in the powder feeding device, overlapping one by one to form a deposition layer connected to the substrate, and then the processing head is lifted by a deposition layer thickness and continues to work along the scanning path to complete the melting deposition layer by layer and complete the Ti 30 Zr 25 V 15 Nb 20 Al 10 To Ti 50 Zr 30 Nb 20 Preparation of wide composition alloy samples. During the deposition process, the coaxial powder feeding technology was used to change the composition ratio every 2 deposition layers, and the powder volume ratio was controlled from A to 10 B 0 , A 9 B 1 , A 8 B 2 Change to A 2 B 8 , A 1 B 9 , A 0 B 10 .

[0032] (2) The block alloy was removed from the substrate by electrospark cutting technology and the 3D printing marks on the surface were removed. The block alloy sample was then cut into two sheet alloy samples with a length × width × thickness = 30 × 20 × 5 mm along the direction of composition change. The samples were then polished (240# sandpaper) and ultrasonically cleaned for 20 minutes and dried to obtain the pretreated sheet alloy samples.

[0033] (3) A laser beam with a diameter of 6 mm was selected and moved along the direction of composition change on the pre-treated sheet alloy sample. After each scan, the process parameters were changed. The center distance between two adjacent cladding molten pools was 10 mm. Three W powders were scanned and deposited on each sheet alloy sample, thus completing the introduction of different wetting conditions at different composition positions. The schematic diagram is shown in FIG. Figure 1 shown.

[0034] Among them, the six specific process parameters on the two sheet alloy samples are as follows: sample No. 1 (laser power 500W, scanning speed 2mm / s, powder feeding speed 4r / min), sample No. 2 (laser power 700W, scanning speed 4mm / s, powder feeding speed 8r / min), sample No. 3 (laser power 800W, scanning speed 4mm / s, powder feeding speed 8r / min), sample No. 4 (laser power 1000W, scanning speed 5mm / s, powder feeding speed 10r / min), sample No. 5 (laser power 1200W, scanning speed 10mm / s, powder feeding speed 20r / min), sample No. 6 (laser power 1500W, scanning speed 10mm / s, powder feeding speed 20r / min).

[0035] (4) The sheet alloy sample that has completed three W powder scans is cut into 10 long thin slices with a thickness of 2 mm (the deposition thickness is changed each time the powder volume ratio is changed) perpendicular to the direction of composition change. Different long thin slices have different compositions and wetting conditions, thus completing the high-throughput preparation of high-density energetic materials.

[0036] (5) 10 long thin slices were sanded and polished with diamond polishing liquid to prepare metallographic samples for morphological structure and composition characterization. The morphological structure of the alloy samples was then observed by optical microscopy (OM) and scanning electron microscopy (SEM); the actual composition of each component inside the alloy was analyzed by X-ray energy spectrum analyzer (XPS); the hardness of different parts of the alloy was measured by Vickers hardness tester, completing the integrated characterization of different matrix components, different wetting conditions, interface structure, and organizational properties.

[0037] The composition of the wide-composition alloy sample in step (1) was scanned every 2 mm in the height direction. It was found that the content of V and Al in the alloy decreased linearly, and the total mass percentage of V and Al decreased from 12% to 9% to 3%, and finally to 0%, indicating that the composition of the wide-composition sample was Ti. 30 Zr25 V 15 Nb 20 Al 10 To Ti 50 Zr 30 Nb 20 .

[0038] Quantitative schematic diagram of melt pool morphology Figure 2 As shown, where W is the weld width, h is the weld depth, H 1 : Melting height 1, H 2 :Melting height 2, S 1 : Molten pool area, S 2 : Weak edge area, asymmetry ratio = (H 1 -H 2 ) / H 2 , weak edge = S 2 / (S 1 +S 2 ).

[0039] The microstructures of all alloy samples obtained in step (4) were observed to quickly obtain the alloy forming conditions and the microstructure relationships between different components and different wetting conditions. The molten pool morphologies of six different processes under the same component position were selected, such as Figure 3 As shown. The results show that laser power plays a major role in the forming of the alloy. With the increase of laser power, the molten width and depth in the molten pool gradually increase. However, the asymmetry of the alloy morphology is greater when the laser power is too low or too high. This is because when the power is too low, the input energy is low, which will cause the matrix alloy to be partially unmelted, and uneven accumulation distribution will occur, resulting in poor alloy forming; when the power is too high, the matrix alloy will be over-melted, affecting the powder fluidity, increasing the temperature gradient, and aggravating the Marangoni effect, resulting in unevenness at both ends of the molten pool.

[0040] Sample No. 2, which has good alloy forming performance, was selected to conduct composition scanning at its interface under different matrix compositions. The results show that as the matrix composition changes from Ti 30 Zr 25 V 15 Nb 20 Al 10 Change into Ti 50 Zr 30 Nb 20 , W content is kept within a certain range (±5%), V, Al, Zr, Nb content decreases linearly, and Ti content increases linearly. Select position 6 (volume ratio 4Ti 30 Zr 25 V 15 Nb 20 Al 10 :6Ti 50 Zr 30 Nb20 ) and position 10(10Ti 50 Zr 30 Nb 20 ) observed its structure and found that with the increase of Ti content, there was an obvious gauze-like structure (reaction layer) near the W particles, and the content of the reaction layer gradually increased. This is because there is a high mutual diffusion coefficient between W and Ti, and mutual diffusion behavior is very easy to occur in the molten pool.

[0041] The hardness test was carried out on the top, weak edge area and base of sample No. 2 respectively. Figure 4 As shown in the figure, it is found that the hardness at the interface between the two phases is similar to that of the energetic matrix, which indicates that the melted W particles at the interface between the two phases do not strengthen the matrix. This may be due to the Hall-Petch effect. Under the action of laser power, the grains grow and the microhardness of the alloy decreases.

[0042] In summary, when the laser power is 700W-1000W and the scanning speed is 3-10m / s, scanning W powder has a good forming effect, thereby further narrowing the process range, and the structure, composition and hardness of the well-formed sample No. 2 are tested to screen out the matrix composition of all Ti 50 Zr 30 Nb 20 May have stronger comprehensive performance.

[0043] Example 2

[0044] Metal powder Mo powder, B (Ti 40 Zr 30 V 10 Nb 20 ), C(Ti) as an example, the specific steps of the high-throughput preparation method for high-density energetic composite materials are as follows:

[0045] (1) Select 45-150 μm Ti 40 Zr 30 V 10 Nb 20 , Ti powder is used as the raw material for preparing the alloy matrix. The laser beam works with the scanning path through the laser parameter values ​​pre-set by the machine tool (laser spot diameter 2mm, laser power 800W, laser scanning speed 2mm / s, deposition thickness of each layer 0.5mm, fixed spacing between layers 1.6mm), and the alloy powder is sprayed to the center of the molten pool generated by the substrate and the laser beam through the carrier gas in the powder feeding device, and overlaps one by one to form a deposition layer connected to the substrate. Then the processing head is lifted by a deposition layer thickness and continues to work along the scanning path to complete the melting deposition layer by layer and complete the Ti 40 Zr 30 V 10 Nb 20During the deposition process, the coaxial powder feeding technology was used to change the composition ratio every 2 deposition layers, and the powder volume ratio was controlled from B to 10 C 0 , B 9 C 1 , B 8 C 2 Change to B 2 C 8 , B 1 C 9 , B 0 C 10 .

[0046] (2) The block alloy was removed from the substrate by electrospark cutting technology and the 3D printing marks on the surface were removed. The block alloy sample was then cut into two sheet alloy samples with a length × width × thickness = 30 × 20 × 5 mm along the direction of composition change. The samples were then polished (240# sandpaper) and ultrasonically cleaned for 30 minutes and dried to obtain the pretreated sheet alloy samples.

[0047] (3) A laser beam with a diameter of 2 mm was selected and moved along the direction of composition change on the pre-treated sheet alloy sample. After each scan, the process parameters were changed. The center distance between two adjacent cladding molten pools was 6 mm. Three Mo powders were scanned and deposited on each sheet alloy sample, thus completing the introduction of different wetting conditions at different composition positions. The schematic diagram is shown in FIG. Figure 1 shown.

[0048] Among them, the six specific process parameters on the two sheet alloys are as follows: sample No. 1 (laser power 500W, scanning speed 2mm / s, powder feeding speed 2r / min), sample No. 2 (laser power 700W, scanning speed 4mm / s, powder feeding speed 4r / min), sample No. 3 (laser power 800W, scanning speed 5mm / s, powder feeding speed 5r / min), sample No. 4 (laser power 1000W, scanning speed 5mm / s, powder feeding speed 10r / min), sample No. 5 (laser power 1200W, scanning speed 8mm / s, powder feeding speed 8r / min), sample No. 6 (laser power 1500W, scanning speed 10mm / s, powder feeding speed 10r / min).

[0049] (1) The sheet alloy sample that has completed three Mo powder scans is cut into 10 long thin slices with a thickness of 2 mm (the deposition thickness is changed each time the powder volume is changed) perpendicular to the direction of composition change. Different long thin slices have different compositions and wetting conditions, thus completing the high-throughput preparation of high-density energetic materials.

[0050] (2) 10 long thin slices were sanded and polished with diamond polishing liquid to prepare metallographic samples for morphology, structure and composition characterization. The morphology and structure of the alloy samples were then observed by optical microscopy (OM) and scanning electron microscopy (SEM); the actual composition of each component in the alloy was analyzed by X-ray energy spectrum analyzer (XPS); the hardness of different parts of the alloy was measured by Vickers hardness tester, completing the integrated characterization of different matrix components, different wetting conditions, interface structure and structure performance.

[0051] The composition of the wide-composition alloy sample in step (1) was scanned every 2 mm in the height direction. It was found that the content of Zr, V, and Nb in the alloy decreased linearly, and the total mass percentage of Zr, V, and Nb decreased from 60% to 30% to 10%, and finally to 0%, indicating that the composition of the wide-composition sample was Ti 40 Zr 30 V 10 Nb 20 Become Ti.

[0052] The microstructures of all alloy samples obtained in step (4) were observed to quickly obtain the alloy forming conditions and the microstructure relationships of different components and different wetting conditions. The results show that with the increase of laser power, the molten width, molten depth and asymmetry rate in the molten pool gradually increase. The laser power plays a major role in the forming of the alloy. This is because too low power will cause the matrix alloy to be partially unmelted and the alloy forming is poor; too high power will cause the matrix alloy to be over-melted, affecting fluidity.

[0053] Sample No. 3, which has good alloy forming performance, was selected to conduct composition scanning at its interface under different matrix compositions. The results show that as the matrix composition changes from Ti 40 Zr 30 V 10 Nb 20 The content of Zr, V and Nb gradually decreases, and the content of Ti gradually increases. 40 Zr 30 V 10 Nb 20 The microstructures of position 5Ti) and position 10 (10Ti alloy) were observed and it was found that with the increase of Ti content, the content of reaction layer near Mo particles did not change much. This is because at the same temperature, with the increase of Mo content, the mutual diffusion coefficient decreased; but under the same matrix composition, comparing sample No. 3 and sample No. 6, with the increase of laser power, the content of reaction layer near Mo particles increased. This is because with the increase of molten pool temperature, the mutual diffusion coefficient between Mo and Ti increased.

[0054] Hardness tests were performed on different components at different composition positions of sample 3. It was found that the hardness at the interface between the two phases was similar to that of the energetic matrix, which indicated that the melted Mo particles at the interface between the two phases did not strengthen the matrix, which may be due to the decrease in microhardness caused by grain growth under the action of laser power.

[0055] In summary, when the laser power is 800W-1200W and the scanning speed is 5-8m / s, the scanning Mo powder has a good forming effect. The process range is further determined, and the organization, composition and hardness of the well-formed sample No. 3 are tested. It is screened that the matrix composition in the middle (55% Ti, 25% Zr, 15% Nb, 5% V) may have stronger comprehensive performance.

[0056] Based on the high-throughput preparation method described in the present invention, the relationship between matrix composition, wetting conditions, interface structure and microstructure performance of high-density energetic composite materials is established, and a basis is provided for studying the two-phase interface behavior of the high-density energetic composite material by scanning W / Mo powder with different laser process parameters in a wide composition space.

[0057] In summary, the invention includes but is not limited to the above embodiments. Any equivalent substitution or partial improvement made under the spirit and principle of the invention shall be deemed to be within the protection scope of the invention.

Claims

1. A high-throughput preparation method for high-density energetic composite materials, characterized in that: The method steps include: (1) Using two energetic alloy powders A and B as matrix materials, the 3D printing coaxial powder feeding technology is used to adjust the feeding ratio of the two powders, and a wide-composition alloy block with a gradient change in the volume ratio of the two energetic alloys A and B along the deposition direction is deposited on the substrate; (2) removing the alloy block from the substrate and uniformly cutting it along the direction of composition change to obtain a plurality of small alloy blocks; (3) Using high-density metal as the reinforcement phase, multiple passes of laser scanning of high-density metal powder are performed on the surface of each alloy block. The laser scanning parameters are as follows: laser diameter is 2 to 6 mm, laser power is 500 to 1500 W, laser scanning speed is 2 to 10 mm / s, and powder feeding speed is 4 to 20 r / min. The scanning parameters are different for each pass. (4) After the laser scanning is completed, cutting is performed along a direction perpendicular to the direction of composition change of the base material and at the composition change interface.

2. A high-throughput preparation method for high-density energetic composite materials according to claim 1, characterized in that: In step (1), the two energetic alloys A and B are M x N y One of the energetic alloys in the system, with a theoretical energy density ≥10KJ / g; wherein, 85≤x≤100, 0≤y≤15, x+y=100; M is selected from one or more of Ti, Zr, Hf, V, Nb and Ta; and N is selected from one or more of Al, Cr, Mn, Fe, Co, Ni and Cu.

3. A high-throughput preparation method for high-density energetic composite materials according to claim 1, characterized in that: In step (1), the two energetic alloy powders A and B are spherical powders with a particle size of 45 to 150 μm.

4. A high-throughput preparation method for high-density energetic composite materials according to claim 1, characterized in that: In step (1), during 3D printing, the laser spot diameter is 2 to 6 mm, the laser power is 800 to 1400 W, the laser scanning speed is 2 to 10 mm / s, the deposition thickness of each layer is 0.5 to 1 mm, and the fixed spacing between layers is 1.6 to 3.2 mm.

5. A high-throughput preparation method for high-density energetic composite materials according to claim 1, characterized in that: In step (1), the volume ratio of the two energetic alloy powders A and B is changed every 2 to 3 layers of deposition.

6. A high-throughput preparation method for high-density energetic composite materials according to any one of claims 1 to 5, characterized in that: Taking the total volume of the energetic alloy powders A and B as 100%, the volume content of the energetic alloy powder A is reduced by 10% each time, and the volume content of the energetic alloy powder B is increased by 10% each time.

7. A high-throughput preparation method for high-density energetic composite materials according to claim 1, characterized in that: In step (2), the thickness of the small alloy block is ≥5 mm.

8. A high-throughput preparation method for high-density energetic composite materials as claimed in claim 1, characterized in that: In step (3), the ratio of the powder feeding speed to the scanning speed in each pass is the same.

9. A high-throughput preparation method for high-density energetic composite materials as claimed in claim 1, characterized in that: In step (3), the spacing between two adjacent paths is ≥6 mm.

10. A high-throughput preparation method for high-density energetic composite materials according to claim 1, 8 or 9, characterized in that: In step (3), the high-density metal is W powder or Mo powder, and the particle size is 5 to 25 μm.