Multi-element system composite oxygen carrier, preparation method and application
The desulfurization ash of metallurgical solid waste is treated with sulfuric acid acidolysis and combined with blast furnace gas mud to prepare a multi-system composite oxygen carrier, which solves the problem of difficult utilization of metallurgical solid waste and achieves the preparation of high-efficiency oxygen carrier and environmental protection and energy saving goals.
Patent Information
- Application Number
- CN202410844165.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-29
AI Technical Summary
In the existing technology, it is difficult to achieve unified treatment and efficient utilization of metallurgical solid waste desulfurization ash, leading to resource waste and environmental pollution, and the modification cost based on primary resource materials is high.
The desulfurization ash of metallurgical solid waste is treated by sulfuric acid acidolysis and converted into CaSO4 form to improve its oxygen-carrying capacity and porosity. A multi-component system composite oxygen carrier is prepared, which is combined with blast furnace gas mud and oxidant to form Fe2O3/Al2O3/CaSO4/ZnO, etc. Oxygen carrier, improve oxygen carrying capacity and combustion conversion rate.
It achieves high value-added utilization of metallurgical solid waste, reduces enterprise costs, improves the oxygen-carrying capacity and combustion conversion rate of the oxygen carrier, and meets the requirements of energy conservation, environmental protection, and circular economy.
Smart Images

Figure CN118853253A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of oxygen carrier preparation, and relates to a multi-component system composite oxygen carrier, a preparation method and application. Background Art
[0002] Chemical chaining combustion is a process of decomposing the traditional reaction of direct contact between fuel and air into two gas-solid reactions with the help of oxygen carriers, and transferring oxygen to the fuel with the help of oxygen carriers. Compared with conventional combustion, this new combustion technology can increase the CO2 concentration, thereby facilitating CO2 enrichment and recovery, and improve energy utilization efficiency through the cascade utilization of energy grades, and can also effectively control the generation of NOx and reduce pollution.
[0003] During the chemical chain combustion process, the oxygen carrier can not only provide heat and be received by the fuel reactor, but also output oxygen and realize the conversion of fuel, thereby effectively controlling CO2 emissions.
[0004] At present, the main classification forms of oxygen carriers are metals and non-metals. Metal oxygen carriers are mainly iron-based, copper-based, cobalt-based, manganese-based and nickel-based. For non-metal oxygen carriers, calcium-based (CaSO4 / CaS), barium-based (BaSO4 / BaS) and strontium-based (SrSO4 / SrS) oxygen carriers are their main components. Among them, calcium-based oxygen carriers have the widest application. Unlike metal oxides, they have greater oxygen carrying capacity and good environmental protection. Among them, CaSO4 has excellent oxygen transfer properties and can reach a theoretical oxygen carrying rate of 0.471, and will not cause heavy metal pollution in the environment. Therefore, calcium sulfate is widely used in the field of chemical chain combustion.
[0005] After searching, it was found that the CaSO4 oxygen carrier materials based on experimental research and commercialization at home and abroad are all prepared with chemical reagents or primary mineral resources as raw materials. The technology of preparing Ca-based oxygen carriers and composite oxygen carriers based on metallurgical solid waste-desulfurization ash has not been reported.
[0006] The main components of desulfurization ash of metallurgical solid waste are calcium sulfate, calcium carbonate, calcium hydroxide and calcium sulfite, which contain trace elements such as Fe, Si, Al and Mg. Since the proportions of these components in desulfurization ash are not fixed, it is difficult to achieve unified treatment of them. The properties of calcium sulfite in desulfurization ash are extremely unstable during utilization, so most of them are mainly piled up and discarded, which not only has low utilization efficiency but also easily causes environmental pollution. At present, the material utilization of solid waste has become a new mainstream of energy conservation and emission reduction, which can realize the high added value utilization of metallurgical solid waste. Therefore, the present invention combines the fact that Ca in the desulfurization ash of metallurgical solid waste is the main element required for preparing Ca-based oxygen carriers, controls the existence form of Ca by modifying the desulfurization ash, thereby converting it into an oxygen carrier with the main component existing in CaSO4, removes most harmful components, increases the porosity and specific surface area of the desulfurization ash to improve its oxygen carrying capacity, thereby, the desulfurization ash has the basic elements for preparing Ca-based oxygen carriers, the present invention not only realizes the high added value recycling of metallurgical solid waste, but also opens up a new way in the field of energy conservation and emission reduction, and reduces enterprise costs. Summary of the invention
[0007] The present invention aims to provide a multi-component composite oxygen carrier, preparation method and application, which can remove part of the alkali metal elements and increase the porosity through sulfuric acid hydrolysis to expand the specific surface area, so that CaSO3, CaCO3 and Ca(OH)2 in the desulfurization ash are converted into CaSO4, and the component concentration of CaSO4 is increased, so as to expand the single limitation of calcium-based oxygen carrier raw materials and provide a new way for the high added value utilization of desulfurization ash. On the other hand, the prepared multi-component composite oxygen carrier meets the current development requirements of energy conservation, environmental protection and circular economy.
[0008] In order to solve the above technical problems, the inventors have obtained the technical solution of the present invention through practice and summary. The present invention discloses that the basic concept of the technical solution adopted by the present invention to solve the above technical problems is:
[0009] A method for preparing a multi-component composite oxygen carrier, wherein the raw materials for preparing the multi-component composite oxygen carrier are as follows in terms of weight percentage:
[0010] Blast furnace gas mud 3%~6%
[0011] Desulfurization ash 10%~15%
[0012] Oxidant 0.2%~0.6%
[0013] Water 80%~86%
[0014] Among them, the Fe content in the blast furnace gas mud is greater than 35%, the Al2O3 content is greater than 5%, and the Zn content is greater than 2%; the desulfurization ash is semi-dry desulfurization ash;
[0015] First, CaSO4 is enriched by acid hydrolysis at high temperature, washed, and a neutral active Ca-based oxygen carrier precursor is obtained; then a multi-component composite oxygen carrier is prepared by mixing. The desulfurized ash of the present invention is a material for post-treatment of metallurgical solid waste, and can realize the recycling and utilization of waste materials.
[0016] In a further technical solution, the oxidant is of industrial grade and the water is distilled water.
[0017] In a further technical solution, the oxidant is potassium permanganate or hydrogen peroxide.
[0018] In a further technical solution, the raw materials for preparing the multi-component composite oxygen carrier are as follows by weight percentage:
[0019]
[0020] Among them, the Fe content in the blast furnace gas mud is greater than 35%, the Al2O3 content is greater than 5%, and the Zn content is greater than 2%.
[0021] In a further technical solution, the raw materials for preparing the multi-component composite oxygen carrier are as follows by weight percentage:
[0022]
[0023] The blast furnace gas mud has an Fe content of 42.2%, an Al2O3 content of 6.9% and a Zn content of 3.6%.
[0024] In a further technical solution, the following steps are included:
[0025] A. Preparation of CaSO4 oxygen carrier precursor;
[0026] Step 1: Raw material preparation
[0027] Grind the desulfurized ash and pass it through a 100-500 mesh sieve; then dry it in an oven for 6-36 hours, remove the deionized water, weigh 10g of the dried desulfurized ash and dissolve it in a beaker, and add water to 100mL;
[0028] Prepare sulfuric acid with a concentration of 2 to 7 mol / L, add it dropwise into a beaker to adjust the pH to 1 to 9;
[0029] Step 2: Precursor preparation
[0030] Place on a magnetic stirrer, adjust the speed to 200r / min-450r / min, heat the solution to 50-100°C, and react for 1-3h;
[0031] The obtained solution was filtered and washed with deionized water until neutral, and then dried for 6 to 12 hours;
[0032] A CaSO4 oxygen carrier precursor is obtained; the CaSO4 oxygen carrier precursor here refers to the removal of internal components such as calcium sulfite, calcium carbonate, calcium hydroxide, etc. to increase the content of CaSO4, and what is obtained is not pure CaSO4.
[0033] B. Preparation of multi-component composite oxygen carrier;
[0034] Step 3: Preparation of composite solution
[0035] The CaSO4 oxygen carrier precursor is mixed and ground with blast furnace gas mud, and after drying for 18 to 24 hours, a mixed fine powder of 250 to 350 mesh is obtained;
[0036] After mixing the mixed micropowder with water, the pH of the mixed micropowder solution is adjusted to 1 using sulfuric acid with a concentration of 3 to 5 mol / L to obtain an acidic mixed micropowder solution;
[0037] Step 4, using a magnetic stirrer at a temperature of 100 to 150° C. and a rotation speed of 300 to 500 r / min to stir the acidic mixed micropowder solution and the oxidant for 1 to 2 hours, and then drying to obtain a multi-system composite oxygen carrier precursor;
[0038] Step 5: calcining the multi-component composite oxygen carrier precursor in a tubular furnace at a temperature of 400 to 600° C. for 2.5 to 3.5 hours to obtain the multi-component composite oxygen carrier.
[0039] In a further technical solution, when the oxidant is potassium permanganate, the multi-component composite oxygen carrier is Fe2O3-Al2O3-CaSO4-ZnO oxygen carrier.
[0040] In a further technical solution, when the oxidant is hydrogen peroxide, the multi-component composite oxygen carrier is Fe2O3-Al2O3-CaSO4-ZnO oxygen carrier.
[0041] In a further technical solution, during the heating process of steps 1-5, a thermogravimetric mass spectrometer is used to perform oxygen carrier weight loss and gas release tests to obtain its lattice oxygen release characteristics;
[0042] During the test, argon was used as the protective gas, nitrogen was used as the reaction atmosphere, the gas flow rate was 30 mL / min, the heating time was 2 h, and the temperature was raised from 42 ° C to 850 ° C; and it is suitable for measuring changes in the gas concentrations of O2, N2, CO2, CO, SO2, and H2O.
[0043] On the one hand, the CaCO3 and Ca(OH)2 contained in the desulfurized ash are modified by chemical reaction using sulfuric acid solution to achieve the purpose of high purity of CaSO4 in the oxygen carrier.
[0044] On the other hand, desulfurized ash contains trace amounts of CaSO3, which is converted into CaSO4 after roasting, thereby increasing the oxygen carrying capacity of the calcium-based oxygen carrier.
[0045] Compared with the prior art, the present invention has the following beneficial effects:
[0046] Blast furnace gas mud contains a high total Fe content and a certain content of Al2O3. In the process of preparing Ca-based oxygen carriers, Fe2O3 / Al2O3 oxygen carriers are formed, which can improve the oxygen transfer capacity and reduction reaction rate, and maintain good reactivity during the first combustion cycle.
[0047] Secondly, blast furnace gas mud contains a certain amount of Zn. Zn is a transition metal oxide with catalytic function. In the process of preparing Ca-based oxygen carrier, it combines to form Zn oxygen carrier, catalyzing the combustion process, so that the reaction performance of the oxygen carrier during the combustion process is improved.
[0048] The Fe2O3 / Al2O3 oxygen carrier and the Zn oxygen carrier play a synergistic role in improving the combustion conversion rate of the Ca-based oxygen carrier.
[0049] During the heating process, hydrogen peroxide provides the O2 needed in the roasting process, which promotes the more complete conversion of calcium sulfite in the desulfurized ash into calcium sulfate. Blast furnace gas mud contains Zn and potassium permanganate contains Mn. Zn and Mn are transition metal oxides. In the process of preparing Ca-based oxygen carriers, Zn / Mn oxygen carriers are formed, which can alleviate the sintering degree of the oxygen carrier, disperse the active components, and maintain the reaction performance of the oxygen carrier during long-term cyclic use.
[0050] The Fe2O3 / Al2O3 oxygen carrier and the Zn / Mn oxygen carrier play a synergistic role in improving the cyclic combustion characteristics of the Ca-based oxygen carrier.
[0051] During the heating process, potassium permanganate and Mn play a catalytic and oxygen-carrying role in the oxygen-carrying process. Therefore, potassium permanganate not only provides the O2 required in the roasting process, promoting the conversion of calcium sulfite in the desulfurized ash into calcium sulfate; it also participates in the combustion of the oxygen carrier.
[0052] The present invention solves the problem of high cost in the prior art of using primary resource materials for modification. In addition, the method of the present invention is simple in preparing the oxygen carrier, has low investment cost, and can effectively improve its market competitiveness.
[0053] The present invention utilizes metallurgical solid waste desulfurization ash to prepare Ca-based oxygen carriers, which not only opens up a new way to utilize metallurgical solid waste, but also realizes the high value-added application of metallurgical solid waste, expands the utilization of metallurgical iron-containing solid waste, achieves the purpose of "using waste to treat pollution", and complies with relevant energy conservation, environmental protection, and circular economy policy requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0055] Figure 1 The XRD spectrum of the original sample of desulfurized ash prepared by the present invention;
[0056] Figure 2 To change the acid modification time, the CaSO4 oxygen carrier XRD spectrum was 0.5h, 1h, 1.5h, 2h, and 2.5h, respectively, and the pH was 5, while the other conditions remained unchanged;
[0057] Figure 3 To change the solution pH to 1, 3, 5, 7, 9, the XRD spectrum of CaSO4 oxygen carrier when other conditions remain unchanged;
[0058] Figure 4 This is the thermogravimetric diagram of the combustion process of calcium sulfate oxygen carrier in nitrogen atmosphere.
[0059] Figure 5 This is the oxygen carrier stability test curve. DETAILED DESCRIPTION
[0060] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0061] The application principle of the present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0062] Example 1
[0063] First, grind the desulfurized ash through a 100-500 mesh sieve, place it in an oven to dry for 6 hours to remove deionized water, weigh 10g of dry desulfurized ash and dissolve it in a beaker, add water to 100mL, prepare 2mol / L sulfuric acid, add sulfuric acid to adjust the pH to 1, place it on a magnetic stirrer, adjust the speed to 200r / min, heat the solution to 50℃ and react for 0.5h. Filter the resulting solution and wash it with deionized water until it is neutral, and dry it for 6 hours to obtain the CaSO4 oxygen carrier precursor;
[0064] The CaSO4 oxygen carrier precursor is mixed and ground with blast furnace gas mud, and after drying for 24 hours, a mixed fine powder of 250-350 mesh is obtained;
[0065] After mixing the mixed micropowder with water, the pH of the mixed micropowder solution was adjusted to 1 using sulfuric acid with a concentration of 3 mol / L to obtain an acidic mixed micropowder solution;
[0066] The acidic mixed micro-powder solution and the oxidant were stirred for 2 hours using a magnetic stirrer at a temperature of 120° C. and a rotation speed of 300 r / min, and then dried to obtain a multi-system composite oxygen carrier precursor;
[0067] The multi-component composite oxygen carrier precursor was calcined in a tubular furnace at a temperature of 600° C. for 3 hours to obtain the multi-component composite oxygen carrier.
[0068] Finally, a thermogravimetric mass spectrometer was used to test the oxygen carrier weight loss and gas release, so as to obtain its lattice oxygen release characteristics. During the test, argon was used as the protective gas, nitrogen was used as the reaction atmosphere, the gas flow rate was 30mL / min, the heating time was 2h, and the temperature was raised from 42℃ to 850℃. The changes in gases such as O2, N2, CO2, CO, SO2, and H2O were measured.
[0069] Embodiment 2:
[0070] First, grind the desulfurized ash through a 100-500 mesh sieve, place it in an oven to dry for 10 hours to remove deionized water, weigh 10g of dry desulfurized ash and dissolve it in a beaker, add water to 100mL, prepare 3mol / L sulfuric acid, add sulfuric acid to adjust the pH to 2, place it on a magnetic stirrer, adjust the speed to 250r / min, heat the solution to 60℃ and react for 1h; filter the resulting solution and wash it with deionized water until it is neutral, dry it for 7h to obtain a CaSO4 oxygen carrier precursor; mix and grind the CaSO4 oxygen carrier precursor with blast furnace gas mud, and after drying for 24h, obtain a mixed micro powder of 250-350 mesh;
[0071] After mixing the mixed micropowder with water, the pH of the mixed micropowder solution was adjusted to 1 using sulfuric acid with a concentration of 3 mol / L to obtain an acidic mixed micropowder solution;
[0072] The acidic mixed micro-powder solution and the oxidant were stirred for 2 hours using a magnetic stirrer at a temperature of 120° C. and a rotation speed of 300 r / min, and then dried to obtain a multi-system composite oxygen carrier precursor;
[0073] The multi-component composite oxygen carrier precursor was calcined in a tubular furnace at a temperature of 600° C. for 3 hours to obtain the multi-component composite oxygen carrier.
[0074] Finally, a thermogravimetric mass spectrometer was used to test the oxygen carrier weight loss and gas release, so as to obtain its lattice oxygen release characteristics. During the test, argon was used as the protective gas, nitrogen was used as the reaction atmosphere, the gas flow rate was 30mL / min, the heating time was 2h, and the temperature was raised from 42℃ to 850℃. The changes in gases such as O2, N2, CO2, CO, SO2, and H2O were measured.
[0075] Embodiment 3:
[0076] First, grind the desulfurized ash through a 100-500 mesh sieve, place it in an oven to dry for 14 hours to remove deionized water, weigh 10g of dry desulfurized ash and dissolve it in a beaker, add water to 100mL, prepare 4mol / L sulfuric acid, add sulfuric acid to adjust the pH to 3, place it on a magnetic stirrer, adjust the speed to 300r / min, heat the solution to 70℃ and react for 1.5h; filter the resulting solution and wash it with deionized water until it is neutral, dry it for 8h to obtain a CaSO4 oxygen carrier precursor; mix and grind the CaSO4 oxygen carrier precursor with blast furnace gas mud, and after drying for 24h, obtain a mixed micro powder of 250-350 mesh;
[0077] After mixing the mixed micropowder with water, the pH of the mixed micropowder solution was adjusted to 1 using sulfuric acid with a concentration of 3 mol / L to obtain an acidic mixed micropowder solution;
[0078] The acidic mixed micro-powder solution and the oxidant were stirred for 2 hours using a magnetic stirrer at a temperature of 120° C. and a rotation speed of 300 r / min, and then dried to obtain a multi-system composite oxygen carrier precursor;
[0079] The multi-component composite oxygen carrier precursor was calcined in a tubular furnace at a temperature of 600° C. for 3 hours to obtain the multi-component composite oxygen carrier.
[0080] Finally, a thermogravimetric mass spectrometer was used to test the oxygen carrier weight loss and gas release, so as to obtain its lattice oxygen release characteristics. During the test, argon was used as the protective gas, nitrogen was used as the reaction atmosphere, the gas flow rate was 30mL / min, the heating time was 2h, and the temperature was raised from 42℃ to 850℃. The changes in gases such as O2, N2, CO2, CO, SO2, and H2O were measured.
[0081] Embodiment 4:
[0082] First, grind the desulfurized ash through a 100-500 mesh sieve, place it in an oven to dry for 18 hours to remove deionized water, weigh 10g of dry desulfurized ash and dissolve it in a beaker, add water to 100mL, prepare 5mol / L sulfuric acid, add sulfuric acid to adjust the pH to 4, place it on a magnetic stirrer, adjust the speed to 350r / min, heat the solution to 80℃ and react for 2h; filter the resulting solution and wash it with deionized water until it is neutral, dry it for 9h to obtain a CaSO4 oxygen carrier precursor; mix and grind the CaSO4 oxygen carrier precursor with blast furnace gas mud, and after drying for 24h, obtain a mixed micro powder of 250-350mesh;
[0083] After mixing the mixed micropowder with water, the pH of the mixed micropowder solution was adjusted to 1 using sulfuric acid with a concentration of 3 mol / L to obtain an acidic mixed micropowder solution;
[0084] The acidic mixed micro-powder solution and the oxidant were stirred for 2 hours using a magnetic stirrer at a temperature of 120° C. and a rotation speed of 300 r / min, and then dried to obtain a multi-system composite oxygen carrier precursor;
[0085] The multi-component composite oxygen carrier precursor was calcined in a tubular furnace at a temperature of 600° C. for 3 hours to obtain the multi-component composite oxygen carrier.
[0086] Finally, a thermogravimetric mass spectrometer was used to test the oxygen carrier weight loss and gas release, so as to obtain its lattice oxygen release characteristics. During the test, argon was used as the protective gas, nitrogen was used as the reaction atmosphere, the gas flow rate was 30mL / min, the heating time was 2h, and the temperature was raised from 42℃ to 850℃. The changes in gases such as O2, N2, CO2, CO, SO2, and H2O were measured.
[0087] Embodiment 5:
[0088] First, grind the desulfurized ash through a 100-500 mesh sieve, place it in an oven and dry it for 22 hours to remove the deionized water, weigh 10g of the dry desulfurized ash and dissolve it in a beaker, add water to 100mL, prepare 6mol / L sulfuric acid, add sulfuric acid to adjust the pH to 5, place it on a magnetic stirrer, adjust the speed to 400r / min, heat the solution to 90℃ and react for 2.5 hours; filter the obtained solution and wash it with deionized water until it is neutral, dry it for 10 hours to obtain a CaSO4 oxygen carrier precursor; mix and grind the CaSO4 oxygen carrier precursor with blast furnace gas mud, and after drying for 24 hours, obtain a mixed micro powder of 250-350 mesh;
[0089] After mixing the mixed micropowder with water, the pH of the mixed micropowder solution was adjusted to 1 using sulfuric acid with a concentration of 3 mol / L to obtain an acidic mixed micropowder solution;
[0090] The acidic mixed micro-powder solution and the oxidant were stirred for 2 hours using a magnetic stirrer at a temperature of 120° C. and a rotation speed of 300 r / min, and then dried to obtain a multi-system composite oxygen carrier precursor;
[0091] The multi-component composite oxygen carrier precursor was calcined in a tubular furnace at a temperature of 600° C. for 3 hours to obtain the multi-component composite oxygen carrier.
[0092] Finally, a thermogravimetric mass spectrometer was used to test the oxygen carrier weight loss and gas release, so as to obtain its lattice oxygen release characteristics. During the test, argon was used as the protective gas, nitrogen was used as the reaction atmosphere, the gas flow rate was 30mL / min, the heating time was 2h, and the temperature was raised from 42℃ to 850℃. The changes in gases such as O2, N2, CO2, CO, SO2, and H2O were measured.
[0093] Embodiment 6:
[0094] First, grind the desulfurized ash through a 100-500 mesh sieve, place it in an oven to dry for 26 hours to remove deionized water, weigh 10g of dry desulfurized ash and dissolve it in a beaker, add water to 100mL, prepare 7mol / L sulfuric acid, add sulfuric acid to adjust the pH to 6, place it on a magnetic stirrer, adjust the speed to 450r / min, heat the solution to 100℃ and react for 3 hours. Filter the resulting solution and wash it with deionized water until it is neutral, dry it for 12 hours to obtain a CaSO4 oxygen carrier precursor; mix and grind the CaSO4 oxygen carrier precursor with blast furnace gas mud, and after drying for 24 hours, obtain a mixed micro powder of 250-350 mesh;
[0095] After mixing the mixed micropowder with water, the pH of the mixed micropowder solution was adjusted to 1 using sulfuric acid with a concentration of 3 mol / L to obtain an acidic mixed micropowder solution;
[0096] The acidic mixed micro-powder solution and the oxidant were stirred for 2 hours using a magnetic stirrer at a temperature of 120° C. and a rotation speed of 300 r / min, and then dried to obtain a multi-system composite oxygen carrier precursor;
[0097] The multi-component composite oxygen carrier precursor was calcined in a tubular furnace at a temperature of 600° C. for 3 hours to obtain the multi-component composite oxygen carrier.
[0098] Finally, a thermogravimetric mass spectrometer was used to test the oxygen carrier weight loss and gas release, so as to obtain its lattice oxygen release characteristics. During the test, argon was used as the protective gas, nitrogen was used as the reaction atmosphere, the gas flow rate was 30mL / min, the heating time was 2h, and the temperature was raised from 42℃ to 850℃. The changes in gases such as O2, N2, CO2, CO, SO2, and H2O were measured.
[0099] Example 7
[0100] First, grind the desulfurization ash through a 100-500 mesh sieve, place it in an oven to dry for 6 hours to remove deionized water, weigh 10g of dry desulfurization ash and dissolve it in a beaker, add water to 100mL, prepare 2mol / L sulfuric acid, add sulfuric acid to adjust the pH to 1, place it on a magnetic stirrer, adjust the speed to 200r / min, heat the solution to 50℃ and react for 0.5h. Filter the resulting solution and wash it with deionized water until it is neutral, and dry it for 6 hours to obtain the CaSO4 oxygen carrier precursor; the desulfurization ash is semi-dry desulfurization ash, the hydrogen peroxide is industrial grade, and the water is distilled water.
[0101] Then the quality ratio of raw materials is limited:
[0102] Taking the preparation of 100g of the product of the present invention as an example, the components and their mass ratios are as follows:
[0103]
[0104] The blast furnace gas mud has a total Fe content of 42.2%, an Al2O3 content of 6.9%, and a Zn content of 3.6%.
[0105] (1) The CaSO4 oxygen carrier precursor is mixed and ground with blast furnace gas mud, and a 300-mesh mixed micropowder is obtained after drying for 24 hours; the mixed micropowder is mixed with water, and the pH of the mixed micropowder solution is adjusted to 1 using sulfuric acid with a concentration of 3 mol / L to obtain an acidic mixed micropowder solution.
[0106] (2) The acidic mixed micropowder solution and hydrogen peroxide were stirred for 1.5 h using a magnetic stirrer at a temperature of 110° C. and a rotation speed of 500 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier precursor.
[0107] (3) The Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier precursor was calcined in a tubular furnace at a temperature of 400°C for 3.5 hours to obtain a Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier.
[0108] Example 8
[0109] Based on Example 7, the components and their mass ratios used in this example for preparing 100 g of the product of the present invention are as follows:
[0110]
[0111] The blast furnace gas mud has a total Fe content of 42.2%, an Al2O3 content of 6.9%, and a Zn content of 3.6%.
[0112] The desulfurization ash is semi-dry desulfurization ash; the hydrogen peroxide is industrial grade; and the water is distilled water.
[0113] (1) The CaSO4 oxygen carrier precursor is mixed and ground with blast furnace gas mud, and after drying for 18 hours, a 350-mesh mixed micropowder is obtained; after the mixed micropowder is mixed with water, the pH of the mixed micropowder solution is adjusted to 1 using sulfuric acid with a concentration of 5 mol / L to obtain an acidic mixed micropowder solution.
[0114] (2) The acidic mixed micropowder solution and hydrogen peroxide were stirred for 2 h using a magnetic stirrer at a temperature of 150° C. and a rotation speed of 300 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier precursor.
[0115] (3) The Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier precursor was calcined in a tubular furnace at a temperature of 500°C for 2.5 hours to obtain a Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier.
[0116] Example 9
[0117] Based on Example 7, the components and their mass ratios used in this example for preparing 100 g of the product of the present invention are as follows:
[0118]
[0119] The blast furnace gas mud has a total Fe content of 42.2%, an Al2O3 content of 6.9%, and a Zn content of 3.6%.
[0120] The desulfurization ash is semi-dry desulfurization ash. The hydrogen peroxide is industrial grade. The water is distilled water.
[0121] (1) The CaSO4 oxygen carrier precursor is mixed and ground with blast furnace gas mud, and a 250-mesh mixed micropowder is obtained after drying for 22 hours; the mixed micropowder is mixed with water, and the pH of the mixed micropowder solution is adjusted to 1 using sulfuric acid with a concentration of 4 mol / L to obtain an acidic mixed micropowder solution.
[0122] (2) The acidic mixed micropowder solution and hydrogen peroxide were stirred for 1 hour using a magnetic stirrer at a temperature of 130°C and a rotation speed of 400 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier precursor.
[0123] (3) The Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier precursor was calcined in a tubular furnace at a temperature of 600°C for 3 hours to obtain a Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier.
[0124] Example 10
[0125] Based on Example 7, the components and their mass ratios used in this example for preparing 100 g of the product of the present invention are as follows:
[0126]
[0127] The blast furnace gas mud has a total Fe content of 42.2%, an Al2O3 content of 6.9%, and a Zn content of 3.6%.
[0128] (1) The CaSO4 oxygen carrier precursor is mixed and ground with blast furnace gas mud, and a 250-mesh mixed micropowder is obtained after drying for 20 hours; the mixed micropowder is mixed with water, and the pH of the mixed micropowder solution is adjusted to 1 using sulfuric acid with a concentration of 5 mol / L to obtain an acidic mixed micropowder solution.
[0129] (2) The acidic mixed micropowder solution and hydrogen peroxide were stirred for 2 h using a magnetic stirrer at a temperature of 100° C. and a rotation speed of 500 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier precursor.
[0130] (3) The Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier precursor was calcined in a tubular furnace at a temperature of 400°C for 2.5 hours to obtain a Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier.
[0131] Embodiment 11
[0132] Based on Example 7, the components and their mass ratios used to prepare 100 g of the product of the present invention are as follows:
[0133]
[0134] The blast furnace gas mud has a total Fe content of 42.2%, an Al2O3 content of 6.9%, and a Zn content of 3.6%.
[0135] (1) The CaSO4 oxygen carrier precursor is mixed and ground with blast furnace gas mud, and 350 mesh mixed micropowder is obtained after drying for 22 hours; after the mixed micropowder is mixed with water, the pH of the mixed micropowder solution is adjusted to 1 with sulfuric acid having a concentration of 3 mol / L to obtain an acidic mixed micropowder solution.
[0136] (2) The acidic mixed micropowder solution and hydrogen peroxide were stirred for 1 hour using a magnetic stirrer at a temperature of 120°C and a rotation speed of 300 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier precursor.
[0137] (3) The Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier precursor was calcined in a tubular furnace at a temperature of 600°C for 3.5 hours to obtain a Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier.
[0138] Example 12
[0139] Based on Example 7, the components and their mass ratios used in this example for preparing 100 g of the product of the present invention are as follows:
[0140]
[0141] The blast furnace gas mud has a total Fe content of 42.2%, an Al2O3 content of 6.9%, and a Zn content of 3.6%.
[0142] The desulfurization ash is semi-dry desulfurization ash.
[0143] The hydrogen peroxide is of industrial grade.
[0144] The water is distilled water.
[0145] (1) The CaSO4 oxygen carrier precursor is mixed and ground with blast furnace gas mud, and after drying for 20 hours, a 300-mesh mixed micropowder is obtained; after the mixed micropowder is mixed with water, the pH of the mixed micropowder solution is adjusted to 1 using sulfuric acid with a concentration of 4 mol / L to obtain an acidic mixed micropowder solution.
[0146] (2) The acidic mixed micropowder solution and hydrogen peroxide were stirred for 1.5 h using a magnetic stirrer at a temperature of 140° C. and a rotation speed of 400 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnOO-based oxygen carrier precursor.
[0147] (3) The Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier precursor was calcined in a tubular furnace at a temperature of 500°C for 3 hours to obtain a Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier.
[0148] Comparative Example 1
[0149] Taking the preparation of 100g of the product of the present invention as an example, the components and their mass ratios are as follows:
[0150]
[0151] The desulfurization ash is semi-dry desulfurization ash. The hydrogen peroxide is industrial grade. The water is distilled water.
[0152] (1) Grind the desulfurized ash and dry it for 20 hours to obtain 300 mesh desulfurized ash powder; mix the desulfurized ash powder with water, and adjust the pH of the desulfurized ash powder solution to 1 using 4 mol / L sulfuric acid to obtain an acidic desulfurized ash powder solution.
[0153] (2) The acidic desulfurization ash powder solution and hydrogen peroxide were stirred for 1.5 h using a magnetic stirrer at a temperature of 140°C and a rotation speed of 400 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier precursor.
[0154] (3) The Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier precursor was calcined in a tubular furnace at a temperature of 500°C for 3 hours to obtain a Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier.
[0155] Comparative Example 2
[0156] Taking the preparation of 100g of the product of the present invention as an example, the components and their mass ratios are as follows:
[0157]
[0158] The blast furnace gas mud has a total Fe content of 42.2%, an Al2O3 content of 6.9%, and a Zn content of 3.6%.
[0159] The desulfurization ash is semi-dry desulfurization ash. The water is distilled water.
[0160] (1) Desulfurized ash and blast furnace gas mud are mixed and ground, and after drying for 20 hours, 300-mesh mixed micropowder is obtained; after mixing the mixed micropowder with water, the pH of the mixed micropowder solution is adjusted to 1 using sulfuric acid with a concentration of 4 mol / L to obtain an acidic mixed micropowder solution.
[0161] (2) The acidic mixed micropowder solution was stirred for 1.5 h using a magnetic stirrer at a temperature of 140° C. and a rotation speed of 400 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier precursor.
[0162] (3) The Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier precursor was calcined in a tubular furnace at a temperature of 500°C for 3 hours to obtain a Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier.
[0163] Comparative Example 3
[0164] Taking the preparation of 100g of the product of the present invention as an example, the components and their mass ratios are as follows:
[0165]
[0166] The desulfurization ash is semi-dry desulfurization ash. The water is distilled water.
[0167] (1) Grind the desulfurized ash and dry it for 20 hours to obtain 300 mesh desulfurized ash powder; mix the desulfurized ash powder with water, and adjust the pH of the desulfurized ash powder solution to 1 using 4 mol / L sulfuric acid to obtain an acidic desulfurized ash powder solution.
[0168] (2) The acidic desulfurization ash powder solution was stirred for 1.5 h using a magnetic stirrer at a temperature of 140°C and a rotation speed of 400 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier precursor.
[0169] (3) The Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier precursor was calcined in a tubular furnace at a temperature of 500°C for 3 hours to obtain a Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carrier.
[0170] The Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carriers prepared in Examples 7 to 12 and Comparative Examples 1 to 3 were subjected to H2 combustion to obtain the following oxygen carrier conversion rates:
[0171] Table 1. Conversion rate of Fe2O3-Al2O3-CaSO4-ZnO based oxygen carrier
[0172] Sample Conversion rate (%) Example 7 92 Example 8 89 Example 9 87 Example 10 90 Embodiment 11 92 Example 12 90 Comparative Example 1 81 Comparative Example 2 77 Comparative Example 3 73
[0173] The combination of the above-mentioned Example 8 and Example 10 shows that as the concentration of the CaSO4 oxygen carrier precursor increases, the conversion rate of the Fe2O3-Al2O3-CaSO4-ZnO based oxygen carrier is improved. The comparison between Example 12 and Comparative Example 1 shows that the CaSO4 oxygen carrier precursor or desulfurization ash also contains Fe2O3, Al2O3 and ZnO.
[0174] The Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carriers prepared in Examples 7 to 12 and Comparative Examples 1 to 3, after H2 combustion, obtain the reactivity of the oxygen carriers for the first combustion as follows:
[0175] Table 2. Reactivity of Fe2O3-Al2O3-CaSO4-ZnO-based oxygen carriers for first combustion
[0176]
[0177]
[0178] From the data of reduction rate and oxidation rate in the above embodiments, it can be seen that, in combination with Embodiment 12 and Comparative Example 1, the reduction of blast furnace gas mud simultaneously reduces the reduction rate and oxidation rate; in combination with Embodiment 12 and Comparative Example 2, the reduction of hydrogen peroxide simultaneously reduces the reduction rate and oxidation rate, and the reduction is greater than the combined data of Embodiment 12 and Comparative Example 1.
[0179] Embodiment 13
[0180] First, grind the desulfurization ash through a 100-500 mesh sieve, place it in an oven to dry for 6 hours to remove deionized water, weigh 10g of dry desulfurization ash and dissolve it in a beaker, add water to 100mL, prepare 2mol / L sulfuric acid, add sulfuric acid to adjust the pH to 1, place it on a magnetic stirrer, adjust the speed to 200r / min, heat the solution to 50℃ and react for 0.5h. Filter the resulting solution and wash it with deionized water until it is neutral, and dry it for 6 hours to obtain a CaSO4 oxygen carrier precursor; the desulfurization ash is semi-dry desulfurization ash, the potassium permanganate is industrial grade, and the water is distilled water.
[0181] Taking the preparation of 100g of the product of the present invention as an example, the components and their mass ratios are as follows:
[0182]
[0183] The blast furnace gas mud has a total Fe content of 38.2%, an Al2O3 content of 5.2%, and a Zn content of 2.6%.
[0184] The desulfurization ash is semi-dry desulfurization ash, the potassium permanganate is industrial grade, and the water is distilled water.
[0185] (1) The CaSO4 oxygen carrier precursor is mixed and ground with blast furnace gas mud, and 350 mesh mixed micropowder is obtained after drying for 20 hours; after the mixed micropowder is mixed with water, the pH of the mixed micropowder solution is adjusted to 1 with sulfuric acid having a concentration of 3 mol / L to obtain an acidic mixed micropowder solution.
[0186] (2) The acidic mixed micropowder solution and potassium permanganate were stirred for 2 h using a magnetic stirrer at a temperature of 100° C. and a rotation speed of 400 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier precursor.
[0187] (3) The Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier precursor was calcined in a tubular furnace at a temperature of 600°C for 2.5h to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier.
[0188] Embodiment 14
[0189] Based on Example 13, the components and their mass ratios used in preparing 100 g of the product of the present invention in this example are as follows:
[0190]
[0191] The blast furnace gas mud has a total Fe content of 36.5%, an Al2O3 content of 6.3%, and a Zn content of 2.2%.
[0192] The desulfurization ash is semi-dry desulfurization ash; the potassium permanganate is industrial grade; and the water is distilled water.
[0193] (1) The CaSO4 oxygen carrier precursor is mixed and ground with blast furnace gas mud, and a 300-mesh mixed micropowder is obtained after drying for 18 hours; the mixed micropowder is mixed with water, and the pH of the mixed micropowder solution is adjusted to 1 using sulfuric acid with a concentration of 4 mol / L to obtain an acidic mixed micropowder solution.
[0194] (2) The acidic mixed micropowder solution and potassium permanganate were stirred for 1.5 h using a magnetic stirrer at a temperature of 150° C. and a rotation speed of 300 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier precursor.
[0195] (3) The Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier precursor was calcined in a tubular furnace at a temperature of 400°C for 3h to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier.
[0196] Embodiment 15
[0197] Based on Example 13, the components and their mass ratios used in preparing 100 g of the product of the present invention in this example are as follows:
[0198]
[0199] The blast furnace gas mud has a total Fe content of 37.2%, an Al2O3 content of 5.4%, and a Zn content of 3.1%.
[0200] The desulfurization ash is semi-dry desulfurization ash; the potassium permanganate is industrial grade; and the water is distilled water.
[0201] (1) The CaSO4 oxygen carrier precursor is mixed and ground with blast furnace gas mud, and a 250-mesh mixed micropowder is obtained after drying for 24 hours; the mixed micropowder is mixed with water, and the pH of the mixed micropowder solution is adjusted to 1 using sulfuric acid with a concentration of 5 mol / L to obtain an acidic mixed micropowder solution.
[0202] (2) The acidic mixed micropowder solution and potassium permanganate were stirred for 1 hour using a magnetic stirrer at a temperature of 120° C. and a rotation speed of 500 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO-based oxygen carrier precursor.
[0203] (3) The Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier precursor was calcined in a tubular furnace at a temperature of 500°C for 3.5h to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier.
[0204] Example 16
[0205] Based on Example 13, the components and their mass ratios used in preparing 100 g of the product of the present invention in this example are as follows:
[0206]
[0207] The blast furnace gas mud has a total Fe content of 36.1%, an Al2O3 content of 7.4%, and a Zn content of 3.6%.
[0208] The desulfurization ash is semi-dry desulfurization ash; the potassium permanganate is industrial grade; and the water is distilled water.
[0209] (1) The CaSO4 oxygen carrier precursor is mixed and ground with blast furnace gas mud, and a 250-mesh mixed micropowder is obtained after drying for 22 hours; the mixed micropowder is mixed with water, and the pH of the mixed micropowder solution is adjusted to 1 using sulfuric acid with a concentration of 3 mol / L to obtain an acidic mixed micropowder solution.
[0210] (2) The acidic mixed micropowder solution and potassium permanganate were stirred for 2 h using a magnetic stirrer at a temperature of 140° C. and a rotation speed of 300 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier precursor.
[0211] (3) The Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier precursor was calcined in a tubular furnace at a temperature of 400°C for 3.5h to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier.
[0212] Embodiment 17
[0213] Based on Example 13, the components and their mass ratios used in preparing 100 g of the product of the present invention in this example are as follows:
[0214]
[0215] The blast furnace gas mud has a total Fe content of 35.9%, an Al2O3 content of 6.3%, and a Zn content of 2.9%.
[0216] The desulfurization ash is semi-dry desulfurization ash; the potassium permanganate is industrial grade; and the water is distilled water.
[0217] (1) The CaSO4 oxygen carrier precursor is mixed and ground with blast furnace gas mud, and 350 mesh mixed micropowder is obtained after drying for 24 hours; after the mixed micropowder is mixed with water, the pH of the mixed micropowder solution is adjusted to 1 with sulfuric acid with a concentration of 5 mol / L to obtain an acidic mixed micropowder solution.
[0218] (2) The acidic mixed micropowder solution and potassium permanganate were stirred for 1 hour using a magnetic stirrer at a temperature of 110° C. and a rotation speed of 500 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier precursor.
[0219] (3) The Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier precursor 2.5 is calcined in a tubular furnace at a temperature of 600°C to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier.
[0220] Embodiment 18
[0221] Based on Example 13, the components and their mass ratios used in preparing 100 g of the product of the present invention in this example are as follows:
[0222]
[0223] The blast furnace gas mud has a total Fe content of 36.8%, an Al2O3 content of 6.5%, and a Zn content of 3.4%.
[0224] The desulfurization ash is semi-dry desulfurization ash; the potassium permanganate is industrial grade; and the water is distilled water.
[0225] (1) The CaSO4 oxygen carrier precursor is mixed and ground with blast furnace gas mud, and after drying for 20 hours, a 300-mesh mixed micropowder is obtained; after the mixed micropowder is mixed with water, the pH of the mixed micropowder solution is adjusted to 1 using sulfuric acid with a concentration of 4 mol / L to obtain an acidic mixed micropowder solution.
[0226] (2) The acidic mixed micropowder solution and potassium permanganate were stirred for 1.5 h using a magnetic stirrer at a temperature of 130° C. and a rotation speed of 400 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier precursor.
[0227] (3) The Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier precursor was calcined in a tubular furnace at a temperature of 500°C for 3h to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier.
[0228] Comparative Example 4
[0229] Taking the preparation of 100g of the product of the present invention as an example, the components and their mass ratios are as follows:
[0230]
[0231] The desulfurization ash is semi-dry desulfurization ash; the potassium permanganate is industrial grade; and the water is distilled water.
[0232] (1) Grind the desulfurized ash and dry it for 20 hours to obtain 300 mesh desulfurized ash powder; mix the desulfurized ash powder with water, and adjust the pH of the desulfurized ash powder solution to 1 using 4 mol / L sulfuric acid to obtain an acidic desulfurized ash powder solution.
[0233] (2) The acidic desulfurization ash powder solution and potassium permanganate were stirred for 1.5 h using a magnetic stirrer at a temperature of 130° C. and a rotation speed of 400 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier precursor.
[0234] (3) The Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier precursor was calcined in a tubular furnace at a temperature of 500°C for 3h to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier.
[0235] Comparative Example 5
[0236] Taking the preparation of 100g of the product of the present invention as an example, the components and their mass ratios are as follows:
[0237]
[0238] The blast furnace gas mud has a total Fe content of 36.8%, an Al2O3 content of 6.5%, and a Zn content of 3.4%.
[0239] The desulfurization ash is semi-dry desulfurization ash.
[0240] The water is distilled water.
[0241] (1) Desulfurized ash and blast furnace gas mud are mixed and ground, and after drying for 20 hours, 300-mesh mixed micropowder is obtained; after mixing the mixed micropowder with water, the pH of the mixed micropowder solution is adjusted to 1 using sulfuric acid with a concentration of 4 mol / L to obtain an acidic mixed micropowder solution.
[0242] (2) The acidic mixed micropowder solution was stirred for 1.5 h using a magnetic stirrer at a temperature of 130° C. and a rotation speed of 400 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier precursor.
[0243] (3) The Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier precursor was calcined in a tubular furnace at a temperature of 500°C for 3h to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier.
[0244] Comparative Example 6
[0245] Taking the preparation of 100g of the product of the present invention as an example, the components and their mass ratios are as follows:
[0246]
[0247] The desulfurization ash is semi-dry desulfurization ash.
[0248] The water is distilled water.
[0249] (1) Grind the desulfurized ash and dry it for 20 hours to obtain 300 mesh desulfurized ash powder; mix the desulfurized ash powder with water, and adjust the pH of the desulfurized ash powder solution to 1 using 4 mol / L sulfuric acid to obtain an acidic desulfurized ash powder solution.
[0250] (2) The acidic desulfurization ash powder solution was stirred for 1.5 h using a magnetic stirrer at a temperature of 130°C and a rotation speed of 400 r / min, and then dried to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier precursor.
[0251] (3) The Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier precursor was calcined in a tubular furnace at a temperature of 500°C for 3h to obtain a Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier.
[0252] The Fe2O3-Al2O3-CaSO4-ZnO-MnO-based oxygen carrier prepared in Examples 1 to 6 and Comparative Examples 1 to 3 was subjected to H2 combustion to obtain the following oxygen carrier conversion rates:
[0253] Table 3. Conversion rate of Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier
[0254]
[0255]
[0256] In the above embodiments, in combination with Example 15 and Example 17, the increase of CaSO4 oxygen carrier precursor or desulfurization ash and the decrease of potassium permanganate will reduce the conversion rate; in combination with Example 15 and Example 18, the reduction of blast furnace gas mud and the increase of CaSO4 oxygen carrier precursor or desulfurization ash will reduce the conversion rate; in combination with Example 18 and Comparative Example 4, it can be obtained that the reduction of blast furnace gas mud will reduce the conversion rate; in combination with Example 18 and Comparative Example 5, it can be obtained that the reduction of potassium permanganate will reduce the conversion rate, and the reduction range is greater than the reduction range of Example 18 and Comparative Example 4.
[0257] The Fe2O3-Al2O3-CaSO4-ZnO-MnO-based oxygen carriers prepared in Examples 13 to 18 and Comparative Examples 4 to 6 were tested for 5 and 10 cycles, and the oxygen and reverse stability performances obtained were as follows:
[0258] Table 4. Multiple cycle stability of Fe2O3-Al2O3-CaSO4-ZnO-MnO based oxygen carrier
[0259] Sample After 5 cycles (%) After 10 cycles (%) Example 13 95 94 Embodiment 14 90 89 Embodiment 15 96 96 Example 16 94 92 Embodiment 17 90 90 Embodiment 18 90 88 Comparative Example 4 81 78 Comparative Example 5 75 72 Comparative Example 6 71 65
[0260] The Fe2O3-Al2O3-CaSO4-ZnO-MnO-based oxygen carrier maintained good reaction performance during the cycle as shown in Table 4. The addition of Mn element made the active components more dispersed and increased the stability of the carrier at high temperature, so that the Fe2O3-Al2O3-CaSO4-ZnO-MnO-based oxygen carrier maintained stable reaction performance during the reaction process.
[0261] Application: including application in the preparation of molecular oxygen transport materials, supplying oxygen to fuel during combustion, and absorbing oxygen in the environment after deoxidation. The multi-component composite oxygen carrier of the present invention can be used without introducing air, and the oxygen carrier reacts, releasing oxygen atoms at high temperature, and the composite oxygen carrier is reduced, thereby reducing the generation of nitrogen oxides, etc., and the generated gas contains relatively high purity water and carbon dioxide, which is also conducive to the capture and absorption of carbon dioxide.
[0262] After transporting oxygen molecules, the multi-component composite oxygen carrier can absorb oxygen in the environment again after deoxygenation, thereby achieving the absorption of oxygen in the environment.
[0263] For example, in chemical companies that burn methane, air is introduced into the combustion environment as a conventional method. However, nitrogen in the air easily generates nitrogen oxides at high temperatures, which pollute the atmospheric environment. Therefore, subsequent pollutant reduction treatment is required.
[0264] Figure 5This is a test curve of oxygen carrier stability. As can be seen from the figure, the rate of decline represents the reduction efficiency, and the greater the rate of decline, the better the effect; the rate of increase represents the oxidation efficiency, and the greater the rate of increase, the better the effect. After multiple weight loss (reduction reaction) and weight gain (oxidation reaction), the multi-element oxygen carrier still has good stability. The principle is that there are more active sites in the multi-element oxygen carrier, and the trace inert components (SiO2) in the oxygen carrier react with these active sites at high temperature to form stable crystals and glass, thereby increasing the stability of the oxygen carrier.
Claims
1. A method for preparing a multi-component composite oxygen carrier, It is characterized in that The raw materials for preparing the multi-component composite oxygen carrier are as follows by weight percentage: Among them, the Fe content in blast furnace gas mud is greater than 35%, Al 2 O 3 The content is greater than 5%, and the Zn content is greater than 2%; the desulfurization ash is semi-dry desulfurization ash; First, CaSO is enriched by acid hydrolysis at high temperature. 4 , washing to obtain a neutral active Ca-based oxygen carrier precursor; and then preparing a multi-system composite oxygen carrier by mixing.
2. The method for preparing a multi-component composite oxygen carrier according to claim 1, It is characterized in that The oxidant is of industrial grade, and the water is distilled water.
3. The method for preparing a multi-component composite oxygen carrier according to claim 1, It is characterized in that The oxidant is potassium permanganate or hydrogen peroxide.
4. The method for preparing a multi-component composite oxygen carrier according to claim 3, It is characterized in that The raw materials for preparing the multi-component composite oxygen carrier are as follows: Among them, the Fe content in blast furnace gas mud is greater than 35%, Al 2 O 3 The content is greater than 5% and the Zn content is greater than 2%.
5. The method for preparing a multi-component composite oxygen carrier according to claim 3, It is characterized in that The raw materials for preparing the multi-component composite oxygen carrier are as follows: The Fe content of the blast furnace gas mud is 42.2%, Al 2 O 3 The content is 6.9%, and the Zn content is 3.6%.
6. A method for preparing a multi-component composite oxygen carrier according to any one of claims 1 to 5, It is characterized in that The following steps are involved: A. Preparation of CaSO 4 Oxygen carrier precursors; Step 1: Raw material preparation Grind the desulfurized ash and pass it through a 100-500 mesh sieve; then dry it in an oven for 6-36 hours, remove the deionized water, weigh 10g of the dried desulfurized ash and dissolve it in a beaker, and add water to 100mL; Prepare sulfuric acid with a concentration of 2 to 7 mol / L, add it dropwise into a beaker, and adjust the pH to 1 to 9; Step 2: Precursor preparation Place on a magnetic stirrer, adjust the speed to 200r / min-450r / min, heat the solution to 50-100°C, and react for 1-3h; The obtained solution was filtered and washed with deionized water until neutral, and then dried for 6 to 12 hours; Get CaSO 4 Oxygen carrier precursors; B. Preparation of multi-component composite oxygen carrier; Step 3: Preparation of composite solution CaSO 4 The oxygen carrier precursor is mixed and ground with blast furnace gas mud, and after drying for 18 to 24 hours, a mixed fine powder of 250 to 350 mesh is obtained; After mixing the mixed micropowder with water, the pH of the mixed micropowder solution is adjusted to 1 using sulfuric acid with a concentration of 3 to 5 mol / L to obtain an acidic mixed micropowder solution; Step 4, using a magnetic stirrer at a temperature of 100 to 150° C. and a rotation speed of 300 to 500 r / min to stir the acidic mixed micropowder solution and the oxidant for 1 to 2 hours, and then drying to obtain a multi-system composite oxygen carrier precursor; Step 5: calcining the multi-component composite oxygen carrier precursor in a tubular furnace at a temperature of 400 to 600° C. for 2.5 to 3.5 hours to obtain the multi-component composite oxygen carrier.
7. The method for preparing a multi-component composite oxygen carrier according to claim 6, It is characterized in that During the heating process of steps 1-5, a thermogravimetric mass spectrometer is used to perform oxygen carrier weight loss and gas release tests, thereby obtaining its lattice oxygen release characteristics; During the test, argon was used as the protective gas, nitrogen was used as the reaction atmosphere, the gas flow rate was 30 mL / min, the heating time was 2 h, and the temperature was raised from 42 °C to 850 °C; and it is suitable for measuring O 2 、N 2 , CO 2 , CO, SO 2 , H 2 O gas concentration changes.
8. A multi-component composite oxygen carrier, It is characterized by: Prepared by the preparation method of the multi-component composite oxygen carrier of claim 7; When the oxidant is potassium permanganate, the multi-component system composite oxygen carrier is Fe 2 O 3 -Al 2 O 3 -CaSO 4 -ZnO-MnO oxygen carrier; When the oxidant is hydrogen peroxide, the multi-component system composite oxygen carrier is Fe 2 O 3 -Al 2 O 3 -CaSO 4 -ZnO oxygen carrier.
9. Application of the multi-component composite oxygen carrier according to claim 8, It is characterized in that Application in the preparation of materials for transporting molecular oxygen.
10. Use of the multi-component composite oxygen carrier according to claim 8, It is characterized in that The multi-component composite oxygen carrier supplies oxygen to the fuel to assist combustion during combustion; the multi-component composite oxygen carrier absorbs oxygen in the environment after deoxygenation.
Citation Information
Patent Citations
Method for preparing Fe2O3 / Al2O3 oxygen carrier by taking ferrous metallurgy dust mud as main raw materials
CN104059714A
Perovskite type Fe-based composite oxygen carrier and preparation method thereof
CN112877110A
Semi-dry desulfurization ash and industrial waste sulfuric acid combined oxidation method
CN115448350A
Method and system for preparing solid oxygen carrier from sintering flue gas semi-dry desulfurization ash and application
CN115789681A