Electromagnetic coupling field repairing method for service damage of low-pressure turbine blade of aero-engine

Through the electromagnetic coupling field repair method, pulsed electric fields and magnetic fields are used to treat aeroengine blades, which solves the problems of long repair time, high energy consumption and environmental pollution in the existing technology, achieves efficient and environmentally friendly blade performance recovery, and extends service life and reduced maintenance costs.

CN118854045APending Publication Date: 2024-10-29SICHUAN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410907544.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing repair methods for service damage of low-pressure turbine blades in aeroengines have problems such as long time, high energy consumption, low efficiency and environmental pollution, and have not been widely used.

Method used

The electromagnetic coupling field repair method is used to perform pre-treatment, primary treatment and secondary treatment on the blades through pulsed electric fields and pulsed magnetic fields to regulate the residual stress and microstructure of the material surface, reduce residual stress, homogenize the stress distribution, and improve the mechanical properties of the material. .

Benefits of technology

It effectively reduces the residual stress amplitude, improves the mechanical properties of the material, extends the service life of the blade, reduces maintenance costs, and the process is simple, efficient, environmentally friendly, and avoids environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854045A_ABST
    Figure CN118854045A_ABST
Patent Text Reader

Abstract

The invention discloses an electromagnetic coupling field repairing method for service damage of a low-pressure turbine blade of an aero-engine. The electromagnetic coupling field repairing method comprises the steps that an electromagnetic coupling processing clamp fixed with the blade is placed in electromagnetic coupling processing equipment; setting parameters of a pulsed electric field and a pulsed magnetic field, and performing electromagnetic coupling pretreatment on the blade; parameters of the pulsed electric field and the pulsed magnetic field are set again, and electromagnetic coupling primary treatment and electromagnetic coupling secondary treatment are sequentially conducted on the blade according to the parameters; and after electromagnetic coupling secondary treatment is completed, cutting off power and taking out the blade. According to the method, the electromagnetic coupling energy field is adopted for repairing the service damaged blade, the residual stress amplitude is reduced, the residual stress distribution is more uniform, the partially deformed microstructure is recovered, the creep durability is greatly improved, the repaired turbine blade can continue to serve, the service life of the blade is prolonged, and the service life of the blade is prolonged. And the maintenance cost of the engine is effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-temperature alloy repair, and in particular relates to an electromagnetic coupling field repair method for service damage of a low-pressure turbine blade of an aero-engine. Background Art

[0002] High-temperature alloy refers to a type of metal with iron, cobalt and nickel as the matrix, which can work for a long time at high temperatures above 600℃ and under certain stress. It has high high-temperature strength, good corrosion resistance, oxidation resistance, good fracture toughness, creep resistance and fatigue performance, etc., and is widely used in aerospace, petrochemical and other fields. Nickel-based high-temperature alloy is an alloy prepared with nickel as the matrix element and rare metal elements such as chromium, aluminum, titanium, tungsten, cobalt and rhenium. Nickel-based high-temperature alloy has good high-temperature strength, creep performance, fracture toughness, fatigue performance, corrosion and oxidation resistance and organizational stability, and is widely used in key components such as aircraft engine turbine blades, guide vanes, casings, combustion chambers, gas turbine blades, nuclear reactor heat transfer tubes, etc.

[0003] As the heart of an aircraft, the performance of an aircraft engine is related to the flight performance and flight safety of the aircraft. As one of the core components of the engine, the low-pressure turbine blades of an aircraft engine are widely made of nickel-based high-temperature alloys. During the operation of the aircraft engine, the blades are in an extreme service environment of high temperature, high pressure, high speed, thermal shock, and thermal corrosion. Therefore, the performance of the blades is related to the service life and performance of the engine. After the aircraft engine blades have been in service for a period of time, the blade tissue material degenerates and creep damage occurs to varying degrees, resulting in performance degradation, which will greatly affect the flight safety of the aircraft. Since the materials of aircraft engine blades are expensive and the preparation process is complicated and cumbersome, directly replacing new blades will result in excessive costs. Therefore, for blades that have been damaged in service, a restoration treatment is used to restore the original performance of the blades with tissue damage so that they can continue to serve, which can effectively save the maintenance cost of the engine.

[0004] At present, there are two main methods for repairing damaged blades in service, one is hot isostatic pressing treatment, and the other is recovery heat treatment. Hot isostatic pressing technology is to add high-pressure inert gas to a closed container under high temperature and high pressure conditions, so that the workpiece being processed is subjected to balanced pressure in all directions, thereby achieving the purpose of repairing the organization and restoring performance. However, hot isostatic pressing equipment is expensive and the processing process is complicated, so it is costly to use this technology to repair damaged blades. Recovery heat treatment mostly uses solid solution plus aging treatment to repair damaged blades. Although it can achieve a certain performance recovery effect, the processing process is complicated, time-consuming, inefficient, and there are problems such as environmental pollution. The journal article The recovery of microstructure and mechanical properties of directionally solidified Ni-based superalloy DZ411 after long-term thermal exposure at different temperatures (Materials Science & Engineering A, 2023, 888: 145831) performs recovery heat treatment on the DZ411 alloy after thermal exposure, repairs the degraded microstructure, and effectively prolongs the creep life. The journal article Effect of microstructures restoration on high temperature fatigue behavior of DZ125superalloy (Progress in Natural Science: Materials International, 2021, 31: 633-640) treated the creep-damaged DZ125 alloy by combining hot isostatic pressing technology with recovery heat treatment, repaired the degraded microstructure, and effectively improved the fatigue resistance. Although there is a certain repair effect on blades damaged in service, these methods have problems such as long time, high energy consumption, low efficiency, and environmental pollution, and have not been widely used in actual industrial production. Summary of the invention

[0005] The purpose of the present invention is to address the above-mentioned deficiencies in the prior art and to provide an electromagnetic coupling field repair method for service damage of low-pressure turbine blades of aircraft engines, so as to solve the problems of the existing repair methods such as long time, high energy consumption, low efficiency, environmental pollution, etc., and the problem that they have not been widely used in actual industrial production.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] An electromagnetic coupling field repair method for service damage of low-pressure turbine blades of an aero-engine comprises the following steps:

[0008] S1. Fix the blade to be processed in the electromagnetic coupling processing fixture, and place the blade axis parallel to the direction of the pulse current;

[0009] S2, placing the electromagnetic coupling processing fixture with the blade fixed thereon into the electromagnetic coupling processing device;

[0010] S3, setting the pulse electric field and pulse magnetic field parameters of the electromagnetic coupling processing equipment;

[0011] S4, starting the electromagnetic coupling processing equipment to perform electromagnetic coupling preprocessing on the blade according to the pulse electric field and pulse magnetic field parameters set in S3;

[0012] S5, resetting the pulse electric field and pulse magnetic field parameters of the electromagnetic coupling processing device;

[0013] S6, starting the electromagnetic coupling processing device to perform electromagnetic coupling primary processing on the blade according to the pulse electric field and pulse magnetic field parameters set in S5;

[0014] S7, after completing the first level of electromagnetic coupling processing, wait for the blade to be discharged, take out the blade and cool it in the air;

[0015] S8, turning the blade around, placing it into the electromagnetic coupling processing fixture again, and placing the electromagnetic coupling processing fixture with the blade fixed thereon into the electromagnetic coupling processing device again;

[0016] S9, starting the electromagnetic coupling processing device to perform electromagnetic coupling secondary processing on the blade according to the pulse electric field and pulse magnetic field parameters set in S5;

[0017] S10, after completing the electromagnetic coupling secondary processing, turn off the power and take out the blade.

[0018] The present invention utilizes the energy generated by electromagnetic coupling to regulate the residual stress on the surface of the material. On the one hand, it can reduce the residual stress amplitude, and on the other hand, it can evenly distribute the residual stress and improve the creep stress concentration phenomenon caused by the service of the blade. In addition, the high energy field generated by electromagnetic coupling can also regulate the microstructure inside the material and repair the degraded microstructure. Under the action of the pulsed electric field, the Joule heating effect, electroplastic effect, skin effect, etc. provide driving force for the movement of dislocations and vacancy atoms; under the action of the pulsed magnetic field, the binding force between electron pairs is weakened by the magnetoplastics effect, magnetostriction effect and magnetic field force, which promotes the movement of dislocations and vacancies inside the material, making the dislocation distribution more uniform, thereby evenly distributing the residual stress and improving the mechanical properties of the material.

[0019] Furthermore, the electromagnetic coupling processing fixture in S1 includes two conductive clamps connected to the pulse electrodes and an insulating guide rail bottom plate; the conductive clamps fix the blades on the insulating guide rail bottom plate.

[0020] Furthermore, in S2, the electromagnetic coupling processing fixture with blades is fixed at both ends of the electrodes of the pulse electric field generating device, and then placed in the excitation coil of the pulse magnetic field.

[0021] Furthermore, the pulse electric field and pulse magnetic field parameters of the electromagnetic coupling processing device are set in S3, including:

[0022] Each group of electric pulses is set to contain multiple positive and negative pulses, the frequency of each positive and negative pulse is 50Hz, each group of positive and negative electric pulses has 10, and the pulse group interval is 500ms;

[0023] Set the excitation coil frequency of the magnetic field generating device to 50 Hz and the magnetic pulse interval to 10 s;

[0024] The pulse electric field current density was set to 100 A / mm 2 , the pulse magnetic field strength is 1.5T.

[0025] Furthermore, electromagnetic coupling preprocessing is performed in S4, including:

[0026] A pulse electric field is generated by a pulse electrode, and electricity is converted into a pulse magnetic field by an excitation coil. The pulse electric field and pulse magnetic field are applied to the blades at the same time. The total application time of the pulse electromagnetic field is 20s.

[0027] Furthermore, in S5, the pulse electric field and pulse magnetic field parameters of the electromagnetic coupling processing device are set again, including:

[0028] Set each group of positive and negative electric pulses to 5 to 10, the pulse group interval is 500ms, the number of pulse groups is 200 to 300, and the discharge time is 140 to 270s;

[0029] Set the interval between each magnetic pulse to 10s, the number of pulses to 10 to 20 times, and the magnetic release time to 100 to 200s;

[0030] Set the pulse electric field current density to 25~60A / mm 2 , the pulse magnetic field strength is 0.5~1.5T.

[0031] Furthermore, in S6, the blade is subjected to a first-level electromagnetic coupling process, including:

[0032] The electromagnetic coupling processing device is started, and a pulse electric field and a pulse magnetic field are simultaneously applied to the blade according to the pulse electric field and pulse magnetic field parameters set in S5, wherein the total application time of the pulse electromagnetic field is 100 to 270 seconds.

[0033] Furthermore, in S9, the blades are subjected to electromagnetic coupling secondary processing, including:

[0034] The electromagnetic coupling processing device is started, and a pulse electric field and a pulse magnetic field are simultaneously applied to the blade according to the pulse electric field and pulse magnetic field parameters set in S5, wherein the total application time of the pulse electromagnetic field is 100 to 270 seconds.

[0035] The electromagnetic coupling field repair method for service damage of low-pressure turbine blades of an aero-engine provided by the present invention has the following beneficial effects:

[0036] 1. The present invention adopts electromagnetic coupling energy field to repair damaged blades in service, and the residual stress amplitude is reduced, the residual stress distribution is more uniform, the partially deformed microstructure is restored, and the creep endurance performance is greatly improved. The repaired turbine blades can continue to serve, which extends the service life of the blades and effectively reduces the engine maintenance cost.

[0037] 2. The electromagnetic coupling equipment required by the present invention has simple working conditions. It only requires a device that can provide a stable pulsed electric field and a pulsed magnetic field. No additional high temperature, high pressure or vacuum conditions are required. The entire electromagnetic coupling treatment method has a simple process, high efficiency, low energy consumption and low cost. It has great advantages over traditional recovery heat treatment and hot isostatic pressing treatment with higher requirements.

[0038] 3. The energy used in the present invention is electric energy, which is a clean energy. The treatment process will not produce waste gas, waste water, or waste residue, and will not cause pollution to the environment. It is a green, clean and efficient treatment method.

[0039] 4. The electromagnetic coupling energy field method proposed in the present invention has an extremely short processing time and will not produce obvious thermal effects on metal materials. The material will not generate heat, thus avoiding negative effects such as deformation of the material.

[0040] 5. Before the electromagnetic coupling primary treatment and the electromagnetic coupling secondary treatment, the present invention first performs electromagnetic coupling pretreatment on the blades. The purpose is to use a strong pulsed electromagnetic field to input energy into the interior of the blades to be treated, so that the temperature of the blades rises slightly, making the particles inside the metal more active, and activating internal defects such as dislocations and vacancies, so as to better control them in the subsequent treatment process.

[0041] 6. The present invention uses electromagnetic coupling for primary and secondary treatments, wherein after the primary treatment, dislocations and vacancies move under the drive of electroplasticity, magnetostriction, Joule heating effect, etc., and residual stress is relaxed. At the same time, particles in an excited state after the primary treatment are more likely to further diffuse, move, and rearrange during the secondary treatment, promoting the repair of microscopic defects inside the material. Compared with the one-time treatment, the secondary treatment uses an opposite electromagnetic field, which can offset the residual magnetic field of the primary treatment and reduce the impact of residual magnetism on the subsequent service of the blade. The two-stage treatment method can release the residual stress more thoroughly and the repair effect of microscopic defects in the material is better. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is a schematic diagram of the electromagnetic coupling process of the present invention.

[0043] Figure 2 The high temperature creep endurance life comparison of the blade body and tenon of a damaged blade in service before and after the electromagnetic coupling treatment of the present invention.

[0044] Figure 3 Figure 2 shows the microscopic morphology of a damaged blade in service before and after the electromagnetic coupling treatment of the present invention; Figure (a) shows before the treatment; Figure (b) shows after the treatment.

[0045] Figure 4 The microscopic morphology of the tenon of a damaged blade in service before and after the electromagnetic coupling treatment of the present invention; Figure (a) is before the treatment; Figure (b) is after the treatment. DETAILED DESCRIPTION

[0046] The specific implementation modes of the present invention are described below so that those skilled in the art can understand the present invention. However, it should be clear that the present invention is not limited to the scope of the specific implementation modes. For those of ordinary skill in the art, as long as various changes are within the spirit and scope of the present invention as defined and determined by the attached claims, these changes are obvious, and all inventions and creations utilizing the concept of the present invention are protected.

[0047] Example 1

[0048] The present embodiment provides an electromagnetic coupling field repair method for service damage of low-pressure turbine blades of aircraft engines. Under the action of a pulsed electric field, the method provides driving force for the movement of dislocations and vacancy atoms through Joule heating effect, electroplastic effect, skin effect, etc. Under the action of a pulsed magnetic field, the binding force between electron pairs is weakened by magnetoplastic effect, magnetostrictive effect and magnetic field force, thereby promoting the movement of dislocations and vacancies inside the blade, making the dislocation distribution more uniform, thereby homogenizing the residual stress, and further improving the mechanical properties of the blade. The method specifically includes the following steps:

[0049] Step S1, fixing the service damaged nickel-based high-temperature alloy low-pressure turbine blade to be treated (hereinafter referred to as the blade) in an electromagnetic coupling treatment fixture, and placing the blade axially parallel to the direction of the pulse current;

[0050] The electromagnetic coupling processing fixture is mainly composed of two conductive chucks connected to the pulse electrode and an insulating guide rail base plate. The conductive chucks are fastened to the pulse electrode and the insulating guide rail base plate respectively with bolts. The conductive chucks fix the blades and conduct the pulse current, and the insulating guide rail base plate supports the blades and stabilizes the conductive chucks.

[0051] Step S2, placing the electromagnetic coupling processing fixture with the blade fixed thereon into the electromagnetic coupling processing equipment;

[0052] Specifically, refer to Figure 1 The electromagnetic coupling processing fixture with blades is fixed on both ends of the electrodes of the pulse electric field generating device, and then placed in the excitation coil of the pulse magnetic field.

[0053] The electromagnetic coupling processing equipment is mainly composed of two electrodes that generate a pulse electric field and an excitation coil that generates a pulse magnetic field.

[0054] Step S3, setting the pulse electric field and pulse magnetic field parameters of the electromagnetic coupling processing device, the parameter settings are as follows:

[0055] Each group of electric pulses is set to contain multiple positive and negative pulses, the frequency of each positive and negative pulse is 50Hz, each group of positive and negative electric pulses has 10, and the pulse group interval is 500ms;

[0056] Set the excitation coil frequency of the magnetic field generating device to 50 Hz and the magnetic pulse interval to 10 s;

[0057] The pulse electric field current density was set to 100 A / mm 2 , the pulse magnetic field strength is 1.5T.

[0058] Step S4: according to the pulse electric field and pulse magnetic field parameters set in S3, start the electromagnetic coupling processing equipment to perform electromagnetic coupling preprocessing on the blade:

[0059] Start the electromagnetic coupling processing equipment, generate a pulse electric field through the pulse electrode, convert electricity into a pulse magnetic field through the excitation coil, and apply the pulse electric field and pulse magnetic field to the sample simultaneously for 20 seconds for electromagnetic coupling pretreatment.

[0060] Step S5: After the electromagnetic coupling preprocessing is completed, the pulse electric field and pulse magnetic field parameters of the electromagnetic coupling processing equipment are set again. After the electromagnetic coupling preprocessing, the parameter settings are as follows:

[0061] Set each group of positive and negative electric pulses to 5 to 10, the pulse group interval to 500ms, the number of pulse groups to 200 to 300 groups, and the discharge time to 140 to 270s.

[0062] Set the interval between each magnetic pulse to 10s, the number of pulses to 10 to 20 times, and the demagnetization time to 100 to 200s.

[0063] Set the pulse electric field current density to 25~60A / mm 2 , the pulse magnetic field strength is 0.5~1.5T.

[0064] Step S6: according to the pulse electric field and pulse magnetic field parameters set in S5, start the electromagnetic coupling processing equipment to perform electromagnetic coupling primary processing on the blade:

[0065] That is, the electromagnetic coupling treatment equipment is started, and a pulse electric field and a pulse magnetic field are simultaneously applied to the blades for electromagnetic coupling primary treatment. The total application time of the pulse electromagnetic field is 100 to 270 seconds.

[0066] Step S7: After the first level of electromagnetic coupling treatment is completed, the blade is taken out and cooled in the air, and then placed in the air for 2 minutes.

[0067] Step S8, turn the blade around, install it into the electromagnetic coupling processing fixture again, and place the electromagnetic coupling processing fixture with the blade fixed thereon into the electromagnetic coupling processing device again.

[0068] Step S9, starting the electromagnetic coupling processing device to perform electromagnetic coupling secondary processing on the blade according to the pulse electric field and pulse magnetic field parameters set in S5;

[0069] The parameters of the electromagnetic coupling secondary treatment in this embodiment are exactly the same as those of the electromagnetic coupling primary treatment, and the total application time of the pulsed electromagnetic field is also 100 to 270 seconds.

[0070] Step S10: After completing the electromagnetic coupling secondary treatment, wait for the discharge to be completed, turn off the power and take out the sample, and the repair treatment of the damaged blade in service can be completed.

[0071] Example 2

[0072] This embodiment is based on the repair method of embodiment 1, and repairs the blade body of a low-pressure turbine blade damaged by a nickel-based high-temperature alloy in service, which specifically includes the following steps:

[0073] Step S1, sampling the blade part, fixing the sample in an electromagnetic coupling processing fixture, and placing the sample axis parallel to the direction of the pulse current;

[0074] Step S2, placing the electromagnetic coupling processing fixture with the sample fixed thereon into the electromagnetic coupling processing device;

[0075] Specifically, refer to Figure 1 The electromagnetic coupling processing fixture with the sample is fixed on both ends of the electrodes of the pulse electric field generating device, and then placed in the excitation coil of the pulse magnetic field.

[0076] The electromagnetic coupling processing equipment is mainly composed of two electrodes that generate a pulse electric field and an excitation coil that generates a pulse magnetic field.

[0077] Step S3, setting the pulse electric field and pulse magnetic field parameters of the electromagnetic coupling processing device, the parameter settings are as follows:

[0078] Each group of electric pulses contains multiple positive and negative pulses. The frequency of each positive and negative pulse is set to 50 Hz. There are 10 positive and negative electric pulses in each group, and the pulse group interval is 500 ms.

[0079] Set the excitation coil frequency of the magnetic field generating device to 50 Hz and the magnetic pulse interval to 10 s.

[0080] Set the pulse electric field current density to 100A / mm 2 , the pulse magnetic field strength is 1.5T.

[0081] Step S4, starting the electromagnetic coupling processing device to perform electromagnetic coupling pretreatment on the sample according to the pulse electric field and pulse magnetic field parameters set in step S3;

[0082] That is, a pulse electric field and a pulse magnetic field are applied to the sample simultaneously, with a duration of 20 seconds.

[0083] Step S5: After the pre-processing is completed, the pulse electric field and pulse magnetic field parameters of the electromagnetic coupling processing device are set again. The parameter settings are as follows:

[0084] The frequency of each positive and negative pulse is set to 50 Hz, 5 positive and negative electric pulses are set in each group, the pulse group interval is 500 ms, the number of pulse groups is 200 groups, and the discharge time is 140 s.

[0085] Set the magnetic pulse interval to 10s, the number of pulses to 15 times, and the magnetic release time to 150s.

[0086] The current density of the pulse electric field was set to 50 A / mm 2 , the pulse magnetic field strength is 1.0T.

[0087] Step S6: according to the pulse electric field and pulse magnetic field parameters set in step S5, start the electromagnetic coupling processing equipment to perform electromagnetic coupling primary processing on the sample, and the total application time of the pulse electromagnetic field is 150s.

[0088] Step S7: After the first level of electromagnetic coupling treatment is completed, the sample is taken out and placed in the air for 2 minutes after the discharge is completed.

[0089] Step S8, turn the sample around, put it into the electromagnetic coupling processing fixture again, and place the electromagnetic coupling processing fixture with the sample fixed in the electromagnetic coupling processing device again.

[0090] Step S9, starting the electromagnetic coupling processing device to perform electromagnetic coupling secondary processing on the sample according to the pulse electric field and pulse magnetic field parameters set in step S5;

[0091] The parameters of the electromagnetic coupling secondary treatment in this embodiment are exactly the same as those of the electromagnetic coupling primary treatment, that is, the electromagnetic coupling treatment equipment is started, and a pulsed electric field and a pulsed magnetic field are simultaneously applied to the sample for electromagnetic coupling secondary treatment, and the total application time of the pulsed electromagnetic field is 150s.

[0092] Step S10: After completing the electromagnetic coupling secondary treatment, wait for the discharge to be completed, turn off the power and take out the sample, and the repair treatment of the service damaged sample can be completed.

[0093] refer to Figure 2 After completing the repair of step S1 to step S10, this embodiment performs a high temperature creep endurance test at 980°C and 216MPa. The high temperature creep endurance rupture time of the blade body of the untreated nickel-based high temperature alloy damaged blade in service is 0.1h, 2.3h, and 5.4h. The high temperature creep endurance rupture time of the blade body after electromagnetic coupling treatment is 9.07h, which is an average improvement of 348.8%.

[0094] The residual stress test was carried out on the samples, and the results are shown in Table 1. The residual stress test results show that the residual stress amplitude of the blade specimen after electromagnetic coupling treatment is reduced, and the residual stress distribution of the treated specimen is more uniform.

[0095] Comparison of the microscopic morphology of the blade specimens before and after electromagnetic coupling treatment Figure 3 The results show that the main strengthening phase γ' phase of the blade was severely deformed before treatment, changing from a cube to an irregular ellipsoid, and the partially deformed γ' strengthening phase restored the cubic morphology after treatment.

[0096] Table 1 Comparison of residual stress of blade specimens before and after electromagnetic coupling treatment

[0097]

[0098] Example 3

[0099] This embodiment is based on the repair method of Example 1, and samples and repairs the tenon part of the low-pressure turbine blade damaged in service by a nickel-based high-temperature alloy, which specifically includes the following steps:

[0100] Step S1, sampling the tenon part of the nickel-based high-temperature alloy low-pressure turbine blade that is damaged in service, fixing the taken sample in an electromagnetic coupling processing fixture, and placing the sample axis parallel to the direction of the pulse current.

[0101] Step S2, placing the electromagnetic coupling processing fixture with the sample fixed thereon into the electromagnetic coupling processing device;

[0102] Specifically, refer to Figure 1 The electromagnetic coupling processing fixture with the sample is fixed on both ends of the electrodes of the pulse electric field generating device, and then placed in the excitation coil of the pulse magnetic field.

[0103] The electromagnetic coupling processing equipment is mainly composed of two electrodes that generate a pulse electric field and an excitation coil that generates a pulse magnetic field.

[0104] Step S3, setting the pulse electric field and pulse magnetic field parameters of the electromagnetic coupling processing device, wherein the parameter settings are as follows:

[0105] Each group of electric pulses contains multiple positive and negative pulses. The frequency of each positive and negative pulse is set to 50 Hz. There are 10 positive and negative electric pulses in each group, and the pulse group interval is 500 ms.

[0106] Set the excitation coil frequency of the magnetic field generating device to 50 Hz and the magnetic pulse interval to 10 s.

[0107] Set the pulse electric field current density to 100A / mm 2 , the pulse magnetic field strength is 1.5T.

[0108] Step S4: according to the pulse electric field and pulse magnetic field parameters set in step S3, start the electromagnetic coupling processing equipment, apply the pulse electric field and pulse magnetic field to the sample simultaneously, and apply them for 20 seconds to perform electromagnetic coupling pretreatment.

[0109] Step S5, re-setting the pulse electric field and pulse magnetic field parameters of the electromagnetic coupling processing device, wherein the parameter settings are as follows:

[0110] After the electromagnetic coupling pretreatment, the frequency of each positive and negative pulse was set to 50 Hz, 10 positive and negative electric pulses were set in each group, the pulse group interval was 500 ms, the number of pulse groups was 200 groups, and the discharge time was 180 s.

[0111] Set the magnetic pulse interval to 10s, the number of pulses to 20 times, and the demagnetization time to 200s.

[0112] The current density of the pulse electric field was set to 60A / mm 2 , the pulse magnetic field strength is 1.5T.

[0113] Step S6, starting the electromagnetic coupling processing device according to the pulse electric field and pulse magnetic field parameters set in step S5;

[0114] That is, the electromagnetic coupling processing equipment is started to apply a pulse electric field and a pulse magnetic field to the sample at the same time, and the total application time of the pulse electromagnetic field is 200s.

[0115] Step S7: After the first level of electromagnetic coupling treatment is completed, the sample is taken out and placed in the air for 2 minutes after the discharge is completed.

[0116] Step S8, turn the sample around, put it into the electromagnetic coupling processing fixture again, and place the electromagnetic coupling processing fixture with the sample fixed in the electromagnetic coupling processing device again.

[0117] Step S9, starting the electromagnetic coupling processing device to perform electromagnetic coupling secondary processing on the sample according to the pulse electric field and pulse magnetic field parameters set in step S5;

[0118] That is, the electromagnetic coupling treatment equipment is started, and a pulse electric field and a pulse magnetic field are simultaneously applied to the sample for electromagnetic coupling secondary treatment. The total application time of the pulse electromagnetic field is 200 s.

[0119] Step S10: After completing the electromagnetic coupling secondary treatment, wait for the discharge to be completed, cut off the power and take out the sample to complete the repair treatment of the sample.

[0120] refer to Figure 2 After completing the repair of step S1 to step S10, this embodiment performs a high-temperature creep endurance test at 980°C and 216MPa. The high-temperature creep endurance rupture time of the tenon of the untreated nickel-based high-temperature alloy service damaged sample is 0.2h, 3.8h, and 5.8h. The high-temperature creep endurance rupture time of the tenon after electromagnetic coupling treatment is 8.93h, which is an average improvement of 273.4%.

[0121] The residual stress test of the samples is carried out, and the results are shown in Table 2. The residual stress test results show that the residual stress amplitude of the tenon sample after electromagnetic coupling treatment is reduced, and the residual stress distribution of the treated sample is more uniform.

[0122] Comparison of the microscopic morphology of the blade specimens before and after electromagnetic coupling treatment Figure 4 As shown; the results show that before treatment, the main strengthening phase γ' phase of the sample was severely deformed, and part of the γ' phase was rafted and connected together. After treatment, the partially deformed γ' strengthening phase restored the cubic morphology, and the rafted γ' phase remelted and precipitated the cubic γ' phase.

[0123] Table 2 Comparison of residual stress of tenon specimens before and after electromagnetic coupling treatment

[0124]

[0125] Although the specific implementation of the invention is described in detail in conjunction with the drawings, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. An electromagnetic coupling field repair method for service damage of low-pressure turbine blades of an aircraft engine, characterized in that: The following steps are involved: S1. Fix the blade to be processed in the electromagnetic coupling processing fixture, and place the blade axis parallel to the direction of the pulse current; S2, placing the electromagnetic coupling processing fixture with the blade fixed thereon into the electromagnetic coupling processing device; S3, setting the pulse electric field and pulse magnetic field parameters of the electromagnetic coupling processing equipment; S4, starting the electromagnetic coupling processing equipment to perform electromagnetic coupling preprocessing on the blade according to the pulse electric field and pulse magnetic field parameters set in S3; S5, resetting the pulse electric field and pulse magnetic field parameters of the electromagnetic coupling processing device; S6, starting the electromagnetic coupling processing device to perform electromagnetic coupling primary processing on the blade according to the pulse electric field and pulse magnetic field parameters set in S5; S7, after completing the first level of electromagnetic coupling processing, wait for the blade to be discharged, take out the blade and cool it in the air; S8, turning the blade around, placing it into the electromagnetic coupling processing fixture again, and placing the electromagnetic coupling processing fixture with the blade fixed thereon into the electromagnetic coupling processing device again; S9, starting the electromagnetic coupling processing device to perform electromagnetic coupling secondary processing on the blade according to the pulse electric field and pulse magnetic field parameters set in S5; S10, after completing the electromagnetic coupling secondary processing, turn off the power and take out the blade.

2. The electromagnetic coupling field repair method for service damage of low-pressure turbine blades of an aircraft engine according to claim 1, characterized in that: The electromagnetic coupling processing fixture in S1 includes two conductive clamps connected to the pulse electrodes and an insulating guide rail bottom plate; the conductive clamps fix the blades on the insulating guide rail bottom plate.

3. The electromagnetic coupling field repair method for service damage of low-pressure turbine blades of an aircraft engine according to claim 1, characterized in that: In the above S2, the electromagnetic coupling processing fixture with blades is fixed at both ends of electrodes of the pulse electric field generating device, and then placed in the excitation coil of the pulse magnetic field.

4. The electromagnetic coupling field repair method for service damage of low-pressure turbine blades of an aircraft engine according to claim 1, characterized in that: The pulse electric field and pulse magnetic field parameters of the electromagnetic coupling processing device are set in S3, including: Each group of electric pulses is set to contain multiple positive and negative pulses, the frequency of each positive and negative pulse is 50Hz, each group of positive and negative electric pulses has 10, and the pulse group interval is 500ms; Set the excitation coil frequency of the magnetic field generating device to 50 Hz and the magnetic pulse interval to 10 s; The pulse electric field current density was set to 100 A / mm 2 , the pulse magnetic field strength is 1.5T.

5. The electromagnetic coupling field repair method for service damage of low-pressure turbine blades of an aircraft engine according to claim 4, characterized in that: The electromagnetic coupling preprocessing is performed in S4, including: A pulse electric field is generated by a pulse electrode, and electricity is converted into a pulse magnetic field by an excitation coil. The pulse electric field and pulse magnetic field are applied to the blades at the same time. The total application time of the pulse electromagnetic field is 20s.

6. The electromagnetic coupling field repair method for service damage of low-pressure turbine blades of an aircraft engine according to claim 1, characterized in that: The pulse electric field and pulse magnetic field parameters of the electromagnetic coupling processing device are set again in S5, including: Set each group of positive and negative electric pulses to 5 to 10, the pulse group interval is 500ms, the number of pulse groups is 200 to 300, and the discharge time is 140 to 270s; Set the interval between each magnetic pulse to 10s, the number of pulses to 10 to 20 times, and the magnetic release time to 100 to 200s; Set the pulse electric field current density to 25~60A / mm 2 , the pulse magnetic field strength is 0.5~1.5T.

7. The electromagnetic coupling field repair method for service damage of low-pressure turbine blades of an aircraft engine according to claim 6, characterized in that: The step S6 performs electromagnetic coupling primary processing on the blade, including: The electromagnetic coupling processing device is started, and a pulse electric field and a pulse magnetic field are simultaneously applied to the blade according to the pulse electric field and pulse magnetic field parameters set in S5, wherein the total application time of the pulse electromagnetic field is 100 to 270 seconds.

8. The electromagnetic coupling field repair method for service damage of low-pressure turbine blades of an aircraft engine according to claim 6, characterized in that: The step S9 performs electromagnetic coupling secondary processing on the blade, including: The electromagnetic coupling processing device is started, and a pulse electric field and a pulse magnetic field are simultaneously applied to the blade according to the pulse electric field and pulse magnetic field parameters set in S5, wherein the total application time of the pulse electromagnetic field is 100 to 270 seconds.

Citation Information

Cited By

  • Electromagnetic coupling assisted aero-engine single crystal blade additive manufacturing repairing method

    CN119525909A