Preparation method of gallium oxide junction barrier Schottky diode based on p-type Cr2O3
By introducing multiple parallel p-type chromium oxide doped layer structures and optimizing the metal layer combination into the gallium oxide Schottky diode, the problem of uneven electric field distribution in the gallium oxide Schottky diode under high reverse bias is solved. Improved breakdown voltage and reliability, reduced leakage current.
Patent Information
- Application Number
- CN202410863742.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-29
- Publication Date
- 2024-10-29
AI Technical Summary
When the gallium oxide Schottky diode is highly reverse biased, due to uneven electric field distribution, the peak electric field appears at the edge of the anode, causing premature breakdown of the device and failing to fully take advantage of the high breakdown electric field.
Using multiple parallel p-type chromium oxide doped layer structures, embedded or placed in the gallium oxide epitaxial layer, by adjusting the spacing, thickness and width of the doped layers, a stronger electric field control capability is formed, and combined with titanium, aluminum, The combination of platinum and other metal layers optimizes the contact between the anode metal layer and the epitaxial layer and reduces leakage current.
It improves the breakdown voltage of the device, reduces the turn-on voltage and leakage current, enhances the reliability of the gallium oxide material, and ensures the stability of the device under high-voltage and high-power conditions.
Smart Images

Figure CN118866985A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of microelectronic technology, and in particular relates to a gallium oxide junction barrier Schottky diode, which can be used for high-voltage, high-power, and power switch equipment. Background Art
[0002] As an ultra-wide bandgap semiconductor material, gallium oxide has a higher bandgap width, critical breakdown field strength and Baliga quality factor compared to wide bandgap materials such as silicon carbide and gallium nitride, and thus has high power conversion efficiency and current handling capacity. High-quality single crystal substrates can be obtained by melt growth or confined edge growth, and high-quality gallium oxide thin films can be obtained by halide vapor phase epitaxy or molecular beam epitaxy. It has attracted much attention for its controllability of donor-type doping using silicon, tin, etc. during bulk material growth or epitaxial growth. At present, the limitation of gallium oxide Schottky diodes in applications is that when a higher reverse bias is applied to it, a peak electric field is likely to appear at the edge of the anode due to the uneven distribution of the electric field, resulting in premature breakdown of the device. Therefore, the advantage of the high breakdown electric field of gallium oxide materials cannot be fully utilized. Therefore, it is necessary to improve the device structure to optimize the electric field at the edge of the anode.
[0003] The patent document with publication number CN115312605A discloses a gallium oxide Schottky diode and a preparation method for improving the peak electric field at the terminal edge. Its structure includes from bottom to top: a cathode ohmic metal layer, a heavily doped gallium oxide substrate layer, an n-type lightly doped gallium oxide epitaxial layer, an anode Schottky metal layer, and a p-type nickel oxide layer, wherein the p-type nickel oxide layer is located at both ends of the anode Schottky metal layer. The device mainly solves the problem of uneven electric field distribution at the terminal edge of the gallium oxide device and the device is easily broken down. However, since the nickel oxide material is mostly prepared by magnetron sputtering at room temperature, its reliability is low, and the anode metal layer of the device is in Schottky contact with the n-type lightly doped gallium oxide epitaxial layer, when the device is in high reverse bias, the leakage current is large. Summary of the invention
[0004] The purpose of the present invention is to address the deficiencies of the above-mentioned prior art and propose a p-type Cr2O3-based gallium oxide junction barrier Schottky diode and a preparation method thereof, so as to improve device reliability, reduce device turn-on voltage, reduce device leakage current, and increase device breakdown voltage.
[0005] In order to achieve the above object, the technical solution of the present invention includes the following:
[0006] Technical Solution 1: A p-type Cr2O3-based gallium oxide junction barrier Schottky diode, comprising from bottom to top: a cathode metal layer, a substrate layer, an epitaxial layer, a p-type doped layer, and an anode metal layer, characterized in that: the p-type doped layer adopts a plurality of parallel p-type chromium oxide doped layer structures, the spacing of which is 0.5 to 100 μm, the thickness of each p-type chromium oxide doped layer is 10 to 500 nm, the width is 0.5 to 100 μm, and the doping concentration is 10 15 cm -3 ~10 20 cm -3 .
[0007] Furthermore, the planar shape of the plurality of parallel p-type doped layers is a concentric circular, square or polygonal structure.
[0008] Furthermore, the cathode metal layer is made of any one or more combinations of titanium, aluminum, platinum, tungsten, chromium, molybdenum, tantalum, nickel, and gold; the anode metal layer is made of any one or more combinations of titanium, aluminum, platinum, tungsten, chromium, molybdenum, tantalum, nickel, and gold.
[0009] Furthermore, the substrate layer is doped with a concentration of 10 17 ~10 20 cm -3 , an n+ gallium oxide doped substrate with a thickness of 200 to 1000 microns; the epitaxial layer is doped with a concentration of 10 15 ~10 17 cm -3 , an n-gallium oxide doped epitaxial layer with a thickness of 1 to 50 microns.
[0010] Technical Solution 2: A p-type Cr2O3-based gallium oxide junction barrier Schottky diode, comprising: a cathode metal layer, a substrate layer, an epitaxial layer, a p-type doped layer, and an anode metal layer, characterized in that: the p-type doped layer adopts a plurality of parallel p-type chromium oxide doped layer structures, embedded in the epitaxial layer, with a spacing of 0.5 to 100 μm, a depth of 10 to 500 nm, a width of each p-type chromium oxide doped layer of 0.5 to 100 μm, and a doping concentration of 10 15 cm -3 ~10 20 cm -3 .
[0011] Technical Solution 3: A method for preparing a Schottky diode according to Technical Solution 1, characterized in that it comprises the following steps:
[0012] 1) Cleaning and heat treating the surface of the substrate layer, ultrasonically cleaning in acetone, isopropanol, anhydrous ethanol and deionized water for 5 to 15 minutes, heating in a solution of H2SO4:H3PO3=3:1 for 5 to 10 minutes, and then cleaning in deionized water to eliminate surface dangling bonds, removing surface oxides with a 5% HF solution, and then drying with a nitrogen gun;
[0013] 2) The substrate layer after cleaning and heat treatment is loaded into the reaction chamber, and a hydride vapor phase epitaxial process is used to deposit a layer with a thickness of 1 to 50 μm and a doping concentration of 10 15 cm -3 ~10 17 cm -3 epitaxial layer;
[0014] 3) depositing a cathode metal layer on the back of the substrate layer by electron beam evaporation or magnetron sputtering, and performing rapid annealing to form an ohmic contact with the epitaxial layer;
[0015] 4) using photolithography to make a mask on the epitaxial layer, and using a pulsed laser method or a magnetron sputtering process to deposit a p-type doped layer of chromium oxide;
[0016] 5) The sample after chromium oxide deposition is placed in acetone and heated for 5 to 30 minutes, and then ultrasonically cleaned in isopropanol and deionized water for 5 to 10 minutes to remove excess photoresist;
[0017] 6) The heat-treated and cleaned samples are placed in a magnetron sputtering or electron beam evaporation chamber to deposit an anode metal layer so that it forms a Schottky contact with the epitaxial layer, thereby completing device preparation.
[0018] Technical Solution 4: A method for preparing a Schottky diode according to Technical Solution 2, characterized in that it comprises the following steps:
[0019] The first step is to clean and heat-treat the surface of the substrate layer, ultrasonically clean it in acetone, isopropanol, anhydrous ethanol, and deionized water for 5 to 15 minutes, heat it in a solution of H2SO4:H3PO3=3:1 for 5 to 10 minutes, and then wash it in deionized water to eliminate surface dangling bonds, remove surface oxides with a 5% HF solution, and then blow dry it with a nitrogen gun;
[0020] In the second step, the substrate layer after cleaning and heat treatment is loaded into the reaction chamber, and a hydride vapor phase epitaxial process is used to deposit a layer with a thickness of 1 to 50 μm and a doping concentration of 10 15 cm -3 ~10 17 cm -3 epitaxial layer;
[0021] The third step is to deposit a cathode metal layer on the back of the substrate layer by electron beam evaporation or magnetron sputtering, and perform rapid annealing to form an ohmic contact with the epitaxial layer;
[0022] In the fourth step, a mask is made on the epitaxial layer by using photolithography, and the epitaxial layer is etched by using RIE or ICP etching technology to form a chromium oxide deposition area.
[0023] The fifth step is to deposit a p-type doped layer of chromium oxide on the etched sample using a pulsed laser method or a magnetron sputtering process;
[0024] Step 6: Place the sample after chromium oxide deposition in acetone and heat it for 5 to 30 minutes, then place it in isopropanol and deionized water for ultrasonic cleaning for 5 to 10 minutes to remove excess photoresist;
[0025] In the seventh step, the heat-treated and cleaned samples are placed in a magnetron sputtering or electron beam evaporation chamber to deposit the anode metal layer so that it forms a Schottky contact with the epitaxial layer, thereby completing the device preparation.
[0026] The present invention adopts a chromium oxide material with a larger dielectric constant and adopts a structure in which a plurality of parallel p-type chromium oxide doped layers are arranged on the upper surface of the embedded epitaxial layer or a plurality of parallel p-type chromium oxide doped layers are embedded in the epitaxial layer. Compared with the prior art, the present invention has the following advantages:
[0027] First, when the device is in reverse bias, the structure can produce stronger electric field regulation capabilities, and the electric field distribution under the anode metal layer is flatter, the device's leakage current is smaller, and the breakdown voltage is larger.
[0028] Secondly, the heterogeneous Schottky structure formed by chromium oxide and gallium oxide has a smaller turn-on voltage.
[0029] Third, chromium oxide materials have better reliability.
[0030] Figure Description
[0031] Figure 1 The schematic diagram of the structure of the p-type Cr2O3-based gallium oxide junction barrier Schottky diode of the present invention is shown in FIG.
[0032] Figure 1 (a) is a Schottky diode structure with multiple exposed parallel p-type chromium oxide doped layers;
[0033] Figure 1 (b) is a Schottky diode structure with multiple parallel p-type chromium oxide doped layers embedded;
[0034] Figure 2 Prepared for the present invention Figure 1 (a) Schematic diagram of the implementation process of the Schottky diode structure;
[0035] Figure 3 Prepared for the present invention Figure 1 (b) Schematic diagram of the implementation process of the Schottky diode structure. DETAILED DESCRIPTION
[0036] The following is a detailed description of the embodiments of the present invention in conjunction with the accompanying drawings:
[0037] Reference Figure 1 (a) The gallium oxide junction barrier Schottky diode based on p-type Cr2O3 of the present invention comprises: a cathode metal layer 1, a substrate layer 2, an epitaxial layer 3, a p-type doped layer 4, and an anode metal layer 5, wherein:
[0038] The substrate layer 2 is made of n+ gallium oxide material.
[0039] The epitaxial layer 3 is located on the substrate layer 2 and is made of n-gallium oxide material.
[0040] The p-type doped layer 4 is located on the epitaxial layer 3, and adopts a structure of N parallel p-type chromium oxide doped layers. The spacing between the p-type chromium oxide doped layers is set to be equidistant or unequal in the range of 0.5 to 100 μm. The thickness of each p-type chromium oxide doped layer is 10 to 500 nm, the width is 0.5 to 100 μm, and the doping concentration is 10 15 cm -3 ~10 20 cm -3 , N≥2.
[0041] The anode metal layer 5 is located on the epitaxial layer 3 and the p-type doped layer 4 and is made of any one or more combinations of titanium, aluminum, platinum, tungsten, chromium, molybdenum, tantalum, nickel and gold.
[0042] The cathode metal layer 1 is made of any one or more combinations of titanium, aluminum, platinum, tungsten, chromium, molybdenum, tantalum, nickel, and gold.
[0043] Reference Figure 1 (b) The gallium oxide junction barrier Schottky diode based on p-type Cr2O3 of the present invention comprises: a cathode metal layer 1, a substrate layer 2, an epitaxial layer 3, a p-type doped layer 4, and an anode metal layer 5, wherein:
[0044] The substrate layer 2 is made of n+ gallium oxide material.
[0045] The epitaxial layer 3 is located on the substrate layer 2 and is made of n-gallium oxide material.
[0046] The p-type doped layer 4 is embedded in the epitaxial layer 3, and adopts a structure of N parallel p-type chromium oxide doped layers. The spacing between the p-type chromium oxide doped layers is set to be equidistant or unequal in the range of 0.5 to 100 μm. The thickness of each p-type chromium oxide doped layer is 10 to 500 nm, the width is 0.5 to 100 μm, and the doping concentration is 10 15 cm -3 ~10 20 cm -3 , N≥2.
[0047] The anode metal layer 5 is located on the epitaxial layer 3 and the p-type doped layer 4 and is made of any one or more combinations of titanium, aluminum, platinum, tungsten, chromium, molybdenum, tantalum, nickel and gold.
[0048] The cathode metal layer 1 is made of any one or more combinations of titanium, aluminum, platinum, tungsten, chromium, molybdenum, tantalum, nickel, and gold.
[0049] Reference Figure 2 The present invention provides a preparation Figure 1 (a) The following three embodiments of the Schottky diode structure:
[0050] Example 1
[0051] Prepare n+ gallium oxide substrate layer with a doping concentration of 10 20 cm -3 , with a thickness of 1000 μm and a doping concentration of 1×10 17 cm -3 , thickness is 1 micron, the number of chromium oxide p-type doping layers is 6, the spacing is 0.5μm, the thickness is 500nm, the width is 0.5μm, and the doping concentration is 1×10 20 cm -3 Gallium oxide Schottky diode.
[0052] Step 1: pre-treat the surface of the epitaxial wafer.
[0053] The gallium oxide epitaxial wafer was ultrasonically cleaned in acetone, isopropanol, anhydrous ethanol, and deionized water for 5 minutes in sequence, heated in a solution of H2SO4:H3PO3=3:1 for 5 minutes, and then washed in deionized water to eliminate surface dangling bonds, and the surface oxide was removed with a 5% HF solution, and then dried with a nitrogen gun;
[0054] Step 2, making a cathode metal layer, such as Figure 2 (a) shown.
[0055] The pre-treated gallium oxide epitaxial wafer is placed with its reverse side facing upward into an electron beam evaporation chamber, the temperature of the reaction chamber is set to room temperature, and metal Ti / Au is deposited in sequence as a cathode.
[0056] Step 3: Ohmization of the cathode metal.
[0057] The gallium oxide epitaxial wafer was placed in a rapid annealing furnace and subjected to rapid thermal annealing in a nitrogen atmosphere with a flow rate of 2 sccm, an annealing temperature of 430° C., and an annealing time of 40 s.
[0058] Step 4: fabricate 6 parallel p-type chromium oxide doped layers.
[0059] The front side of the gallium oxide epitaxial wafer is photolithographically developed to determine five chromium oxide deposition areas arranged in parallel and at equal intervals, such as Figure 2 (b)
[0060] The epitaxial wafer after photolithography was placed in the magnetron sputtering chamber, and the argon flow rate of the magnetron sputtering chamber was set to 20 sccm, the oxygen flow rate was 10 sccm, the chamber pressure was 0.5 mTorr, and the temperature was room temperature. The doping concentration was 1×10 20 cm -3 , a chromium oxide doped layer with a thickness of 500nm, such as Figure 2 (c)
[0061] The sample that has completed the magnetron sputtering process is immersed in an acetone solution for 30 minutes to allow the acetone to fully react with the photoresist to be removed. The sample after immersion is ultrasonically cleaned, and then cleaned in isopropanol and deionized water for 5 minutes each, to form 6 parallel chromium oxide doped layers, such as Figure 2 (d) as shown.
[0062] Step 5: Make the anode.
[0063] The sample after the above process is subjected to photolithography to form an anode metal deposition area, and then the photolithographic sample is placed in an electron beam evaporation chamber to deposit 50 / 120nm thick metal Ni / Au as an anode on the surface of the chromium oxide and epitaxial layer. Figure 2 As shown in (e), the deposited sample is then placed in an organic solution for cleaning to remove excess photoresist, thereby completing device preparation.
[0064] Example 2
[0065] Prepare n+ gallium oxide substrate layer with a doping concentration of 10 17 cm -3 , with a thickness of 200 microns and a doping concentration of 1×10 15 cm -3 , thickness is 50 microns, the number of chromium oxide p-type doping layers is 9, each with a thickness of 10 nm, a width of 100 μm, and a doping concentration of 1×10 15 cm -3, a gallium oxide Schottky diode with unequal spacing between the chromium oxide p-type doped layers.
[0066] Step 1: pre-treat the surface of the epitaxial wafer.
[0067] The gallium oxide epitaxial wafer was ultrasonically cleaned in acetone, isopropanol, anhydrous ethanol, and deionized water for 15 minutes, heated in a solution of H2SO4:H3PO3=3:1 for 10 minutes, and then washed in deionized water to eliminate surface dangling bonds, and the surface oxide was removed with a 5% HF solution, and then dried with a nitrogen gun;
[0068] Step 2: Prepare the cathode metal layer, such as Figure 2 (a) shown.
[0069] The pre-treated gallium oxide epitaxial wafer is placed with its reverse side facing upward into an electron beam evaporation chamber, the temperature of the reaction chamber is set to room temperature, and metal Ti / Au is deposited in sequence as a cathode.
[0070] Step 3: Ohmization of the cathode metal.
[0071] The gallium oxide epitaxial wafer was placed in a rapid annealing furnace and subjected to rapid thermal annealing in a nitrogen atmosphere with a flow rate of 8 sccm, an annealing temperature of 500° C., and an annealing time of 80 s.
[0072] Step 4: fabricate 9 parallel p-type chromium oxide doped layers.
[0073] 4.1) Perform photolithography on the front side of the gallium oxide epitaxial wafer to determine nine chromium oxide deposition areas arranged in parallel with unequal spacing, such as Figure 2 (b)
[0074] 4.2) Place the photolithographic epitaxial wafer into a magnetron sputtering chamber, set the argon flow rate of the magnetron sputtering chamber to 20 sccm, the oxygen flow rate to 1 sccm, the chamber pressure to 0.1 mTorr, and the temperature to room temperature to prepare a doping concentration of 1×10 15 cm -3 , a chromium oxide doped layer with a thickness of 10 nm, such as Figure 2 (c) as shown.
[0075] 4.3) The sample after the magnetron sputtering process was immersed in an acetone solution for 5 minutes to allow the acetone to fully react with the photoresist to be removed, and the sample after immersion was ultrasonically cleaned, and then washed in isopropanol and deionized water for 10 minutes each, to form 9 parallel chromium oxide doped layers, and the spacing between the first p-type doping layer and the second p-type doping layer was 50 μm, the spacing between the second p-type doping layer and the third p-type doping layer was 60 μm, and the spacing between the third p-type doping layer was 100 μm. The spacing between the first p-type doping layer and the fourth p-type doping layer is 80 μm, the spacing between the fourth p-type doping layer and the fifth p-type doping layer is 100 μm, the spacing between the fifth p-type doping layer and the sixth p-type doping layer is 100 μm, the spacing between the sixth p-type doping layer and the seventh p-type doping layer is 80 μm, the spacing between the seventh p-type doping layer and the eighth p-type doping layer is 60 μm, and the spacing between the eighth p-type doping layer and the ninth p-type doping layer is 60 μm. Figure 2 (d) as shown.
[0076] Step 5: Make the anode.
[0077] 5.1) Photolithography is performed on the sample after the above process to form an anode metal deposition area;
[0078] 5.2) Place the photolithographic sample into an electron beam evaporation chamber and deposit a 60 / 200 nm thick Pt / Au metal anode on the chromium oxide and epitaxial layer. Figure 2 (e)
[0079] 5.3) The deposited sample is placed in an organic solution for cleaning to remove excess photoresist and complete the device preparation.
[0080] Example 3
[0081] Prepare n+ gallium oxide substrate layer with a doping concentration of 10 18 cm -3 , with a thickness of 600 microns and a doping concentration of 1×10 16 cm -3 , thickness is 10 microns, the number of chromium oxide p-type doping layers is 9, the spacing is 1 μm, the thickness is 200 nm, the width is 10 μm, and the doping concentration is 1×10 18 cm -3 Gallium oxide Schottky diode.
[0082] Step A, pre-treating the surface of the epitaxial wafer.
[0083] The gallium oxide epitaxial wafer was ultrasonically cleaned in acetone, isopropanol, anhydrous ethanol, and deionized water for 8 minutes, heated in a solution of H2SO4:H3PO3=3:1 for 8 minutes, and then washed in deionized water to eliminate surface dangling bonds, and the surface oxide was removed with a 5% HF solution, and then dried with a nitrogen gun;
[0084] Step B, making a cathode metal layer, such as Figure 2 (a) shown.
[0085] The pre-treated gallium oxide epitaxial wafer is placed with its reverse side facing upward into an electron beam evaporation chamber, the temperature of the reaction chamber is set to room temperature, and metal Ti / Au is deposited in sequence as a cathode.
[0086] Step C, ohmization of the cathode metal.
[0087] The gallium oxide epitaxial wafer was placed in a rapid annealing furnace and subjected to rapid thermal annealing in a nitrogen atmosphere with a flow rate of 5 sccm, an annealing temperature of 450° C., and an annealing time of 50 s.
[0088] Step D: fabricating nine parallel p-type chromium oxide doped layers.
[0089] The front side of the gallium oxide epitaxial wafer is photolithographically developed to determine nine parallel and equally spaced chromium oxide deposition areas, such as Figure 2 (b)
[0090] The epitaxial wafer after photolithography was placed in the magnetron sputtering chamber, and a doping concentration of 1×10 18 cm -3 The magnetron sputtering process conditions of the chromium oxide doped layer with a thickness of 200 nm are as follows: the argon flow rate is 20 sccm, the oxygen flow rate is 5 sccm, the chamber pressure is 0.3 mTorr, and the temperature is room temperature. Figure 2 (c)
[0091] The sample that has completed the magnetron sputtering process was immersed in an acetone solution for 10 minutes to remove the photoresist on the surface of the epitaxial layer. The sample after immersion was ultrasonically cleaned and then washed in isopropanol and deionized water for 8 minutes each to form 9 parallel chromium oxide doped layers with equal spacing, such as Figure 2 (d) as shown.
[0092] Step E, making the anode.
[0093] The sample after the above process is subjected to photolithography to form an anode metal deposition area, and then the photolithographic sample is placed in an electron beam evaporation chamber to deposit 30 / 60nm thick Ni / Pt metal on the upper surface of the epitaxial layer as an anode. Figure 2As shown in (e), the deposited sample is then placed in an organic solution for cleaning to remove excess photoresist and complete the device preparation.
[0094] Reference Figure 2 The present invention provides a preparation Figure 1 (b) The following three embodiments of the Schottky diode of structure:
[0095] Example 4
[0096] Prepare n+ gallium oxide substrate layer with a doping concentration of 10 20 cm -3 , with a thickness of 1000 microns and a doping concentration of 1×10 17 cm -3 , thickness is 1 micron, the number of chromium oxide p-type doping layers is 6, the spacing is 0.5μm, the thickness is 500nm, the width is 0.5μm, and the doping concentration is 1×10 20 cm -3 Gallium oxide Schottky diode.
[0097] Step 1: Pre-treat the surface of the epitaxial wafer.
[0098] The specific implementation of this step is the same as step 1 of Example 1.
[0099] Step 2: Make the cathode metal layer, such as Figure 3 (a) shown.
[0100] The specific implementation of this step is the same as step 2 of Example 1.
[0101] Step 3: Ohmization of cathode metal.
[0102] The specific implementation of this step is the same as step 3 of Example 1.
[0103] Step 4: Etch the epitaxial layer.
[0104] Use photolithography to make a mask on the epitaxial layer, such as Figure 3 As shown in (b), the photolithographic epitaxial wafer is placed in an ICP etching chamber, and the epitaxial layer is etched under the conditions of a BCl3 flow rate of 30 sccm, an Ar2 flow rate of 3 sccm, and a pressure of 5 mTorr to form 6 parallel chromium oxide deposition areas with equal spacing, as shown in FIG. Figure 3 (c) as shown.
[0105] Step 5: Make 6 parallel p-type chromium oxide doped layers.
[0106] The etched epitaxial wafer was placed in a magnetron sputtering chamber, and a doping concentration of 1×10 20 cm -3 , a chromium oxide doped layer with a thickness of 500nm, such as Figure 3 (d)
[0107] The sample that has completed the magnetron sputtering process is immersed in an acetone solution for 30 minutes to allow the acetone to fully react with the photoresist to be removed. The sample after immersion is ultrasonically cleaned, and then cleaned in isopropanol and deionized water for 5 minutes each, to form 6 parallel chromium oxide doped layers, such as Figure 3 (e) as shown.
[0108] Step 6: Making the Anode.
[0109] The sample after the above process is subjected to photolithography to form an anode metal deposition area;
[0110] Then, the photolithographic sample is placed in an electron beam evaporation chamber, and a metal Ni / Au with a thickness of 50 / 120 nm is deposited on the upper surface of the epitaxial layer as an anode. Figure 3 (f)
[0111] The deposited sample is then placed in an organic solution for cleaning to remove excess photoresist and complete device preparation.
[0112] Example 5
[0113] Prepare n+ gallium oxide substrate layer with a doping concentration of 10 17 cm -3 , with a thickness of 200 microns and a doping concentration of 1×10 15 cm -3 , thickness is 50 microns, the number of chromium oxide p-type doping layers is 9, each with a thickness of 10 nm, a width of 100 μm, and a doping concentration of 1×10 15 cm -3 , a gallium oxide Schottky diode with unequal spacing between the chromium oxide p-type doped layers.
[0114] Step 1: Pre-treat the surface of the epitaxial wafer.
[0115] The specific implementation of this step is the same as step 1 in Example 2.
[0116] Step 2: Make the cathode metal layer, such as Figure 3 (a) shown.
[0117] The specific implementation of this step is the same as step 2 of Example 2.
[0118] Step 3: Ohmization of cathode metal.
[0119] The specific implementation of this step is the same as step 3 of Example 2.
[0120] Step 4: Etching the epitaxial layer.
[0121] Use photolithography to make a mask on the epitaxial layer, such as Figure 3 As shown in (b), the photolithographic epitaxial wafer is placed in the ICP etching chamber, and the process conditions are set to 40 sccm of BCl3 flow, 8 sccm of Ar2 flow, and 20 mTorr of pressure. The epitaxial layer is etched to form 9 parallel chromium oxide deposition areas with unequal spacing, as shown in FIG. Figure 3 (c) as shown.
[0122] Step 5: Make 9 parallel p-type chromium oxide doped layers.
[0123] 5.1) Place the photolithographic epitaxial wafer into a magnetron sputtering chamber, set the argon flow rate to 20 sccm, the oxygen flow rate to 1 sccm, the chamber pressure to 0.1 mTorr, and the temperature to room temperature, and prepare a doping concentration of 1×10 15 cm -3 , a chromium oxide doped layer with a thickness of 10 nm, such as Figure 3 (d)
[0124] 5.2) The sample after the magnetron sputtering process is immersed in an acetone solution for 5 minutes to allow the acetone to fully react with the photoresist to be removed. The sample after immersion is ultrasonically cleaned, and then cleaned in isopropanol and deionized water for 10 minutes each, to form 9 parallel chromium oxide doped layers with different spacings, such as Figure 3 (e), where:
[0125] The distance between the first p-type doping layer and the second p-type doping layer is 50 μm.
[0126] The distance between the second p-type doped layer and the third p-type doped layer is 60 μm.
[0127] The distance between the third p-type doped layer and the fourth p-type doped layer is 80 μm.
[0128] The distance between the fourth p-type doped layer and the fifth p-type doped layer is 100 μm.
[0129] The distance between the fifth p-type doped layer and the sixth p-type doped layer is 100 μm.
[0130] The distance between the sixth p-type doped layer and the seventh p-type doped layer is 80 μm.
[0131] The distance between the 7th p-type doped layer and the 8th p-type doped layer is 60 μm.
[0132] The interval between the eighth p-type doping layer and the ninth p-type doping layer is 60 μm.
[0133] Step 6: Make the anode.
[0134] The sample after the above process is subjected to photolithography to form an anode metal deposition area, and then the photolithographic sample is placed in an electron beam evaporation chamber to deposit a metal Pt / Au with a thickness of 60 / 200 nm on the upper surface of the epitaxial layer as an anode. Figure 3 As shown in (f), the deposited sample is then placed in an organic solution for cleaning to remove excess photoresist and complete the device preparation.
[0135] Example 6
[0136] Prepare n+ gallium oxide substrate layer with a doping concentration of 10 18 cm -3 , with a thickness of 600 microns and a doping concentration of 1×10 16 cm -3 , thickness is 10 microns, the number of chromium oxide p-type doping layers is 9, the spacing is 1 μm, the thickness is 200 nm, the width is 10 μm, and the doping concentration is 1×10 18 cm -3 Gallium oxide Schottky diode.
[0137] S1: Pre-treat the surface of the epitaxial wafer.
[0138] The specific implementation of this step is the same as step A in Example 3.
[0139] S2: Make cathode metal layer, such as Figure 3 (a) shown.
[0140] The specific implementation of this step is the same as step B in Example 3.
[0141] S3: Ohmization of cathode metal.
[0142] The specific implementation of this step is the same as step C in Example 3.
[0143] S4: Etching the epitaxial layer.
[0144] Use photolithography to make a mask on the epitaxial layer, such as Figure 3 As shown in (b), the epitaxial wafer after photolithography is placed in an ICP etching chamber to etch the epitaxial layer to form 9 parallel chromium oxide deposition areas with equal spacing. The etching process conditions are BCl3 flow rate 35sccm, Ar2 flow rate 5sccm, and pressure 10mTorr. Figure 3 (c)
[0145] S5: fabricating nine parallel p-type chromium oxide doped layers.
[0146] First, the epitaxial wafer after photolithography was placed in a magnetron sputtering chamber, and a magnetron sputtering process was used to prepare a doping concentration of 1×10 18 cm -3 , a chromium oxide doped layer with a thickness of 200 nm, wherein the process conditions of magnetron sputtering are: argon flow rate 20 sccm, oxygen flow rate 5 sccm, chamber pressure 0.3 mTorr, temperature is room temperature, such as Figure 3 (d)
[0147] Next, the sample that has completed the magnetron sputtering process is placed in an acetone solution and immersed for 10 minutes, so that the acetone and the photoresist to be removed can fully react to remove the photoresist;
[0148] Then, the sample after immersion was ultrasonically cleaned in isopropanol and deionized water for 8 min each, forming 9 parallel chromium oxide doped layers, such as Figure 3 (e) as shown.
[0149] S6: Making an anode.
[0150] The sample after the above process is subjected to photolithography to form an anode metal deposition area;
[0151] Then, the photolithographic sample is placed in an electron beam evaporation chamber, and a 30 / 60 nm thick metal Ni / Pt is deposited on the upper surface of the epitaxial layer as an anode. Figure 3 (f)
[0152] The deposited sample is then placed in an organic solution for cleaning to remove excess photoresist and complete device preparation.
[0153] The above are only six embodiments of the present invention and do not constitute any limitation to the present invention. Obviously, for professionals in this field, after understanding the content and principle of the present invention, it is possible to make various modifications and changes in form and details without departing from the principle and structure of the present invention. For example, in addition to Ni / Pt, Ni / Au, and Pt / Au, the anode metal can also be any one or more combinations of titanium, aluminum, platinum, tungsten, chromium, molybdenum, tantalum, nickel, and gold. However, these modifications and changes based on the concept of the present invention are still within the scope of protection of the claims of the present invention.
Claims
1. A p-type Cr2O3-based gallium oxide junction barrier Schottky diode, comprising from bottom to top: A cathode metal layer (1), a substrate layer (2), an epitaxial layer (3), a p-type doped layer (4), and an anode metal layer (5), wherein the p-type doped layer (4) is a plurality of parallel p-type chromium oxide doped layer structures, the spacing between which is 0.5 to 100 μm, the thickness of each p-type chromium oxide doped layer is 10 to 500 nm, the width is 0.5 to 100 μm, and the doping concentration is 10 15 cm -3 ~10 20 cm -3 .
2. The diode according to claim 1, characterized in that: The planar shape of the multiple parallel p-type doped layers (4) is a concentric circular, square or polygonal structure.
3. The diode according to claim 1, characterized in that: The cathode metal layer (1) is made of any one or more combinations of titanium, aluminum, platinum, tungsten, chromium, molybdenum, tantalum, nickel and gold; The anode metal layer (5) is made of any one or more combinations of titanium, aluminum, platinum, tungsten, chromium, molybdenum, tantalum, nickel and gold.
4. The diode according to claim 1, characterized in that: The substrate layer (2) has a doping concentration of 10 17 ~10 20 cm -3 , an n+ gallium oxide doped substrate having a thickness of 200 to 1000 microns; The epitaxial layer (3) has a doping concentration of 10 15 ~10 17 cm -3 , an n-gallium oxide doped epitaxial layer with a thickness of 1 to 50 microns.
5. A p-type Cr2O3-based gallium oxide junction barrier Schottky diode, comprising: A cathode metal layer (1), a substrate layer (2), an epitaxial layer (3), a p-type doped layer (4), and an anode metal layer (5), wherein the p-type doped layer (4) is a structure of multiple parallel p-type chromium oxide doped layers embedded in the epitaxial layer (3), with a spacing of 0.5 to 100 μm and a depth of 10 to 500 nm, and each p-type chromium oxide doped layer has a width of 0.5 to 100 μm and a doping concentration of 10 15 cm -3 ~10 20 cm -3 .
6. A method for preparing the Schottky diode according to claim 1, characterized in that: The steps include: 1) cleaning and heat treating the surface of the substrate layer (2), ultrasonically cleaning it in acetone, isopropanol, anhydrous ethanol and deionized water for 5 to 15 minutes, heating it in a solution of H2SO4:H3PO3=3:1 for 5 to 10 minutes, and then cleaning it in deionized water to eliminate surface dangling bonds, removing surface oxides with a 5% HF solution, and then drying it with a nitrogen gun; 2) The substrate layer (2) after cleaning and heat treatment is placed in a reaction chamber, and a hydride vapor phase epitaxial process is used to deposit a layer with a thickness of 1 to 50 μm and a doping concentration of 10 15 cm -3 ~10 17 cm -3 epitaxial layer (3); 3) depositing a cathode metal layer (1) on the back side of the substrate layer (2) by electron beam evaporation or magnetron sputtering, and performing rapid annealing to form an ohmic contact with the epitaxial layer (3); 4) using photolithography to make a mask on the epitaxial layer (3), and using a pulsed laser method or a magnetron sputtering process to deposit a p-type doped layer of chromium oxide (4); 5) The sample after chromium oxide deposition is placed in acetone and heated for 5 to 30 minutes, and then ultrasonically cleaned in isopropanol and deionized water for 5 to 10 minutes to remove excess photoresist; 6) The heat-treated and cleaned sample is placed in a magnetron sputtering or electron beam evaporation chamber to deposit an anode metal layer (5) so that it forms a Schottky contact with the epitaxial layer (3), thereby completing device preparation.
7. The method according to claim 6, characterized in that The process conditions of the rapid annealing in step 3) are as follows: Annealing temperature is 430℃~500℃; Annealing time is 40s~80s; The annealing atmosphere is N2 atmosphere with a flow rate of 2 to 8 sccm.
8. The method according to claim 6, characterized in that In step 4), chromium oxide is grown by magnetron sputtering, and the process parameters are as follows: The magnetron sputtering target material is chromium or chromium oxide target with a purity of 99.99%; The reaction chamber pressure is 0.1-0.5 mTorr; The temperature of the reaction chamber is room temperature; The reaction carrier gas is argon and oxygen, and the ratio of argon to oxygen is 20:1 to 2:
1.
9. A method for preparing the Schottky diode according to claim 5, characterized in that: The steps include: The first step is to clean and heat-treat the surface of the substrate layer (2), ultrasonically clean it in acetone, isopropanol, anhydrous ethanol, and deionized water for 5 to 15 minutes, heat it in a solution of H2SO4:H3PO3=3:1 for 5 to 10 minutes, and then wash it in deionized water to eliminate surface dangling bonds, remove surface oxides with a 5% HF solution, and then blow dry it with a nitrogen gun; In the second step, the substrate layer (2) after cleaning and heat treatment is placed in the reaction chamber, and a hydride vapor phase epitaxial process is used to deposit a layer with a thickness of 1 to 50 μm and a doping concentration of 10 15 cm -3 ~10 17 cm -3 epitaxial layer (3); The third step is to deposit a cathode metal layer (1) on the back side of the substrate layer (2) by electron beam evaporation or magnetron sputtering, and perform rapid annealing to form an ohmic contact with the epitaxial layer (3); In the fourth step, a mask is made on the epitaxial layer (3) by photolithography, and the epitaxial layer (3) is etched by RIE or ICP etching technology to form a chromium oxide deposition area. Step 5: Depositing a p-type doping layer (4) of chromium oxide on the etched sample by using a pulsed laser method or a magnetron sputtering process; Step 6: Place the sample after chromium oxide deposition in acetone and heat it for 5 to 30 minutes, then place it in isopropanol and deionized water for ultrasonic cleaning for 5 to 10 minutes to remove excess photoresist; In the seventh step, the heat-treated and cleaned sample is placed in a magnetron sputtering or electron beam evaporation chamber to deposit the anode metal layer (5) so that it forms a Schottky contact with the epitaxial layer (3), thereby completing the device preparation.
10. The method according to claim 9, characterized in that The process conditions of ICP etching in the fourth step are as follows: The BCl3 flow rate is 30-40 sccm; Ar2 flow rate is 3 to 8 sccm; The pressure is 5~20mTorr.
Citation Information
Cited By
SnO / beta-Ga2O3 power diode and preparation method thereof
CN119603981A
Gallium oxide junction barrier Schottky diode and preparation method thereof
CN120091572A
Gallium oxide Schottky diode with high breakdown voltage and preparation method and application thereof
CN120166721A