Preparation method and application of sulfur-doped Pt-based bimetallic alloy nanocluster ammoxidation catalyst
By incorporating sulfur elements to regulate the electronic structure of the Pt(110) surface, an efficient sulfur-doped Pt-based bimetallic alloy nanocluster catalyst was prepared, which solved the problem of slow ammonia oxidation reaction kinetics in ammonia fuel cells and achieved high current Density and low-cost ammonia oxidation performance have promoted the development of ammonia fuel cell technology.
Patent Information
- Application Number
- CN202410894652.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The kinetics of the anode ammonia oxidation reaction in existing ammonia fuel cells is slow, which hinders the further development of ammonia fuel cells, especially the commercial application of low-temperature direct ammonia fuel cells. Moreover, the Pt catalyst is easy to deactivate and the cost is high.
The sulfur-doped Pt-based bimetallic alloy nanocluster catalyst is used to regulate the electronic structure of the Pt(110) surface through the introduction of sulfur element to improve the ammonia oxidation reaction activity. The catalyst is prepared using a simple hydrothermal reaction and calcination steps and has excellent ammonia Oxidation properties.
In a mixed electrolyte of 1M KOH and 0.1M NH3, an ammonia oxidation current density of 269.1A g-1 was achieved, far exceeding the performance of commercial precious metal Pt/C catalysts, with low cost and promising industrial production prospects.
Smart Images

Figure CN118867289A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalyst technology, and in particular to a preparation method and application of a sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst. Background Art
[0002] As a new energy source, hydrogen can be used in hydrogen power generation and fuel cell systems. These systems only produce water vapor and heat during the reaction process, thus avoiding the production of harmful gases such as carbon dioxide, providing potential for zero-carbon energy conversion. However, H2 has a very low safety factor, strict storage and transportation requirements, and traditional natural gas hydrogen production may emit harmful gases (CO, CO2, etc.). Compared with H2, NH3 has a higher energy density per unit volume. Moreover, the current production, storage and application technology of NH3 is relatively mature, and it is a high-quality hydrogen storage carrier. NH3 can be directly used as reforming gas and decomposed into hydrogen for the construction of indirect ammonia fuel cells (IAFC). In addition, it can be directly used as fuel for direct ammonia fuel cell power generation (DAFC). It is worth noting that low-temperature direct ammonia fuel cells (DAFCs) have the advantage of using ammonia directly at the anode, and have a faster start-up time compared with high-temperature DAFCs (such as ammonia fuel solid oxide fuel cells). Therefore, they have greater prospects in practical applications. However, due to the slow kinetics of the anode ammonia oxidation reaction, the further development of ammonia fuel cells on the current market is hindered, and the development of a feasible and efficient ammonia oxidation catalyst is imminent. It is imperative to prioritize the design and implementation of innovative catalysts that can effectively address this limitation, thereby advancing the development of efficient and commercially viable ammonia fuel cell technology.
[0003] Of course, in many studies, platinum (Pt) is recognized as the most effective metal catalyst for ammonia oxidation due to its good catalytic activity. The Pt surface has a high adsorption affinity for NH3, which is conducive to the moderate binding of N and the dehydrogenation process of NH3. However, the use of Pt is hindered by its status as a noble metal, and it is easily deactivated due to the poisoning effect of *N or *NOx during the reaction. Therefore, how to improve the unit activity, selectivity and stability of the active sites of the catalyst under high voltage is the research focus of ammonia oxidation catalysts. At present, the addition of low-cost non-noble metals (such as M=Fe or Zn, etc.) to Pt to alloy it is an effective strategy to improve the AOR electrocatalytic performance and reduce the cost of the catalyst. Modification of Pt by alloying or structural control can optimize the electronic structure and geometric structure of Pt, which will help regulate the activation behavior of NH3 on the catalyst surface, thereby enhancing the AOR activity, which is the key to the realization of commercial DAFC technology. On this basis, the appropriate introduction of non-metallic element sulfur can regulate the electronic structure of the catalyst through a synergistic effect, thereby improving the AOR activity of Pt-based catalysts. In addition, no related research on this type of sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst has been reported.
[0004] According to literature reports, AOR is a structure-sensitive reaction. Compared with Pt(1 1 1) and Pt(1 1 0) crystal planes, Pt(10 0) crystal planes show lower starting potential and higher reaction rate. In view of the various barriers that exist in the practical application of Pt-based catalysts, the present invention aims to adjust the electronic structure of Pt(1 10) surface by doping appropriate non-metallic sulfur elements, so as to achieve efficient AOR activity of the catalyst. Summary of the invention
[0005] The purpose of the present invention is to solve the shortcomings of the prior art and propose a preparation method and application of a sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst. The preparation method is simple and controllable, economical and environmentally friendly, and the prepared sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst has excellent ammonia oxidation performance. In a mixed electrolyte of 1M KOH and 0.1M NH3, it can reach 269.1A g -1 The ammonia oxidation current density is close to 2.5 times that of commercial precious metal Pt / C under the same conditions (110A g -1 ), achieving ammonia oxidation performance far exceeding that of commercial precious metal catalysts.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing a sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst, the specific steps are as follows:
[0008] Step 1, preparation of S-containing carbon black: weigh a certain amount of carbon black and sodium thiosulfate and place them at both ends of a corundum boat respectively, calcine under an inert gas environment, and collect the carbon black containing a certain amount of S element after cooling;
[0009] Step 2, weighing a certain amount of platinum source, zinc source, ascorbic acid and S-containing carbon black, uniformly dispersing them in ethylene glycol, ultrasonically stirring to obtain a mixed solution, transferring the mixed solution to a polytetrafluoroethylene reactor liner for high-temperature hydrothermal reaction, taking out the sample after natural cooling, washing it by centrifugation with deionized water, and vacuum drying to obtain a sulfur-doped Pt-based bimetallic alloy nanocluster catalyst;
[0010] Step 3, preparation method of sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst slurry: take the catalyst synthesized in step 2, mix it thoroughly with isopropanol and Nafion solution, and ultrasonicate for 30-60 minutes until it is evenly dispersed.
[0011] Preferably, in step 1, the carbon black is any one of acetylene black, Ketjen black, and Super P; the amount of carbon black is 10 to 50 mg, the amount of sodium thiosulfate is 30 to 300 mg, and the calcination temperature is 200° C. to 600° C.
[0012] Preferably, in step 2, the amount of platinum source is 10 mg to 50 mg, the amount of zinc source is 10 mg to 50 mg, the amount of ascorbic acid is 50 mg to 200 mg, the volume of ethylene glycol used to disperse the platinum source, zinc source, ascorbic acid and carbon black is 30 ml, the temperature is room temperature, and ultrasound is performed for 30-60 minutes until the dispersion is uniform.
[0013] Preferably, in step 2, the platinum source is any one of chloroplatinic acid, platinum acetate and platinum acetylacetonate; and the zinc source is any one of zinc acetate, zinc sulfate and zinc acetylacetonate.
[0014] Preferably, in step 2, the hydrothermal temperature of the reactor is 100° C. to 200° C., and the thermal reaction time is 6 to 12 hours.
[0015] Preferably, in step 2, the cleaning condition is to rinse with deionized water for 3 to 5 times.
[0016] Preferably, in step 2, the vacuum drying temperature is 50° C. to 80° C., and the drying time is 12 to 24 hours.
[0017] Preferably, in step 1, the inert gas is a 5wt% hydrogen-argon mixed gas or high-purity nitrogen, and the calcination temperature is 200°C to 600°C.
[0018] The present invention also provides an application of the sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst obtained by the above-mentioned preparation method in a direct ammonia fuel cell.
[0019] By adopting the above technical scheme: the sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst prepared by the present invention synthesizes high-quality PtZn bimetallic alloy particles through a simple hydrothermal reaction, and further calcined to incorporate an appropriate amount of sulfur, with adjustable composition and exposed (1 0 0) surface. In the ammonia oxidation reaction (AOR), the mass specific activity of PtZnS-400 (269.1A g -1 ) and area specific activity (16 mA cm -2 ) is significantly higher than other PtZnS-200, PtZnS-300, PtZnS-200 and commercial Pt-based catalysts. Therefore, the present invention improves the inherent activity of the catalytic active sites of the material itself through simple and efficient sulfur doping, so that the electrocatalytic material has excellent electrochemical activity.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The electrochemical test of the present invention shows that the catalyst prepared by the present invention has excellent catalytic activity in alkaline medium, can reach a large current density at a very small overpotential, and has performance far exceeding that of commercial precious metal catalysts. It can reach 269.1A g in 1M KOH and 0.1M NH3 electrolyte. -1 The ammonia oxidation current density is about 150% higher than that of the precursor (110A g -1 ), and is also superior to common commercial precious metal catalysts (Pt-C).
[0022] 2. The sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst prepared by the present invention is low-cost, economical and environmentally friendly, simple to prepare, greatly simplifies the electrode manufacturing process, and has prospects for industrial production.
[0023] 3. The effective doping of non-metallic sulfur elements in this invention will provide a promising paradigm for the design of advanced catalysts for AOR direct ammonia fuel cells and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a field emission transmission electron microscopy image of the sulfur-doped Pt-based bimetallic alloy nanocluster (PtZnS-400) prepared in Example 4 of the present invention at a scale of 20 nm;
[0025] Figure 2 XRD patterns of PtZn prepared in Example 1 of the present invention, PtZnS-200 prepared in Example 2, PtZnS-300 prepared in Example 3, PtZnS-400 prepared in Example 4, PtZnS-500 prepared in Example 4 and Pt-C prepared in Comparative Example 1;
[0026] Figure 3 AOR cycle curves of PtZn prepared in Example 1, PtZnS-200 prepared in Example 2, PtZnS-300 prepared in Example 3, PtZnS-400 prepared in Example 4, and PtZnS-500 prepared in Example 5 of the present invention;
[0027] Figure 4 AOR cycle curves of sulfur-doped Pt-based bimetallic alloy nanoclusters (PtZnS-400) prepared in Example 4 of the present invention at different temperatures;
[0028] Figure 5 This is a power density curve of the sulfur-doped Pt-based bimetallic alloy nanoclusters (PtZnS-400) prepared in Example 4 of the present invention as a direct ammonia fuel cell anode at room temperature (25°C). DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings, so that those skilled in the art can better understand the advantages and features of the present invention, thereby making a clearer definition of the protection scope of the present invention. The embodiments described in the present invention are only a part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.
[0030] All the materials used to prepare the precursors in the present invention are common commercially available products.
[0031] Embodiment 1:
[0032] (1) Add 29.4 mg of zinc acetate, 100 mg of ascorbic acid and 30 mg of Ketjen black to 30 mL of oleylamine, then add 10.5 mL of chloroplatinic acid solution (2 g / L), disperse evenly by ultrasonication, and transfer the solution to a 50 mL polytetrafluoroethylene liner;
[0033] (2) The polytetrafluoroethylene liner described in step (1) was transferred to an oven and reacted at 150° C. for 6 h. After natural cooling, the sample was taken out and filtered and washed with deionized water for 5 times, and vacuum dried at 50° C. for 12 h to obtain a Pt-based bimetallic alloy nanocluster (PtZn) sample.
[0034] Embodiment 2:
[0035] Preparation of Pt-based bimetallic alloy nanoclusters (PtZnS-200):
[0036] (1) Weigh 30 mg of carbon black and 150 mg of sodium thiosulfate and place them at the two ends of a corundum boat respectively. Calcine them at 200 °C in an inert gas environment for 2 h. After cooling, collect and obtain carbon black (S-200) containing a certain amount of S element.
[0037] (2) 29.4 mg of zinc acetate, 100 mg of ascorbic acid and 30 mg of S-200 containing Ketjen Black were added to 30 mL of oleylamine, and then 10.5 mL of chloroplatinic acid solution (2 g / L) was added, ultrasonically dispersed evenly, and the solution was transferred to a 50 mL polytetrafluoroethylene liner;
[0038] (3) The polytetrafluoroethylene liner described in step (1) was transferred to an oven and reacted at 150° C. for 6 h. After natural cooling, the sample was taken out and filtered and washed with deionized water for 5 times, and then vacuum dried at 50° C. for 12 h to obtain a sulfur-doped Pt-based bimetallic alloy nanocluster (PtZnS-200) sample.
[0039] (4) 5 mg of the above PtZnS-200 sample was thoroughly mixed with 900 μL of isopropanol and 100 μL of Nafion solution, and ultrasonicated for 30 to 60 min until the mixture was uniformly dispersed. 20 μL of the slurry was drop-coated on a rotating disk electrode for testing.
[0040] Embodiment 3:
[0041] Preparation of Pt-based bimetallic alloy nanoclusters (PtZnS-300):
[0042] (1) Weigh 30 mg of carbon black and 150 mg of sodium thiosulfate and place them at the two ends of a corundum boat respectively. Calcine them at 300 °C in an inert gas environment for 2 h. After cooling, collect and obtain carbon black (S-300) containing a certain amount of S element.
[0043] (2) Add 29.4 mg of zinc acetate, 100 mg of ascorbic acid and 30 mg of S-300 containing Ketjen Black to 30 mL of oleylamine, then add 10.5 mL of chloroplatinic acid solution (2 g / L), disperse evenly by ultrasonication, and transfer the solution to a 50 mL polytetrafluoroethylene liner.
[0044] (3) The polytetrafluoroethylene liner described in step (1) was transferred to an oven and reacted at 150° C. for 6 h. After natural cooling, the sample was taken out and filtered and washed with deionized water for 5 times, and vacuum dried at 50° C. for 12 h to obtain a sulfur-doped Pt-based bimetallic alloy nanocluster (PtZnS-300) sample.
[0045] (4) 5 mg of the above PtZnS-300 sample was thoroughly mixed with 900 μL of isopropanol and 100 μL of Nafion solution, and ultrasonicated for 30 to 60 min until the mixture was uniformly dispersed. 20 μL of the slurry was drop-coated on the rotating disk electrode for testing.
[0046] Example 4
[0047] Preparation of Pt-based bimetallic alloy nanoclusters (PtZnS-400):
[0048] (1) Weigh 30 mg of carbon black and 150 mg of sodium thiosulfate and place them at the two ends of a corundum boat respectively. Calcine them at 400 °C in an inert gas environment for 2 h. After cooling, collect and obtain carbon black (S-400) containing a certain amount of S element.
[0049] (2) 29.4 mg of zinc acetate, 100 mg of ascorbic acid and 30 mg of S-containing Ketjen Black S-400 were added to 30 mL of oleylamine, and then 10.5 mL of chloroplatinic acid solution (2 g / L) was added, and ultrasonic dispersion was performed uniformly. The solution was then transferred to a 50 mL polytetrafluoroethylene liner.
[0050] (3) The polytetrafluoroethylene liner described in step (1) was transferred to an oven and reacted at 150° C. for 6 h. After natural cooling, the sample was taken out and filtered and washed with deionized water for 5 times, and vacuum dried at 50° C. for 12 h to obtain a sulfur-doped Pt-based bimetallic alloy nanocluster (PtZnS-400) sample.
[0051] Example 5
[0052] Preparation of Pt-based bimetallic alloy nanoclusters (PtZnS-500):
[0053] (1) Weigh 30 mg of carbon black and 150 mg of sodium thiosulfate and place them at the two ends of a corundum boat respectively. Calcine them at 500 °C in an inert gas environment for 2 h. After cooling, collect and obtain carbon black (S-500) containing a certain amount of S element.
[0054] (2) Add 29.4 mg of zinc acetate, 100 mg of ascorbic acid and 30 mg of S-500 containing Ketjen Black to 30 mL of oleylamine, then add 10.5 mL of chloroplatinic acid solution (2 g / L), disperse evenly by ultrasonication, and transfer the solution to a 50 mL polytetrafluoroethylene liner.
[0055] (3) The polytetrafluoroethylene liner described in step (1) was transferred to an oven and reacted at 150° C. for 6 h. After natural cooling, the sample was taken out and filtered and washed with deionized water for 5 times, and vacuum dried at 50° C. for 12 h to obtain a sulfur-doped Pt-based bimetallic alloy nanocluster (PtZnS-500) sample.
[0056] The surface morphology of each sample was observed using a field emission scanning electron microscope (ZEISS Gemini SEM 300, produced by Carl Zeiss AG) and a transmission electron microscope (FEI Talos F200X, produced by FEI Company, USA). Figure 1), it can be clearly found that the sample has sintered after calcination and the lattice has expanded significantly.
[0057] The material structure of each sample was analyzed using an X-ray diffractometer (model Brucker D8-advance, Brucker, Germany). Figure 2 ), with the change of the content of doped elements, the crystal structure of the sample also changed significantly.
[0058] Comparative Example 1
[0059] Using a commercial catalyst instead of the PtZn catalyst in Example 1, Pt-C was prepared:
[0060] (1) 5 mg of commercial Pt / C catalyst was thoroughly mixed with 900 μL of isopropanol and 100 μL of Nafion solution and ultrasonicated for 30 to 60 min until the mixture was uniformly dispersed.
[0061] (2) Take 20 μl of the slurry and drop it onto the rotating disk electrode for testing.
[0062] Electrochemical testing:
[0063] 1.0 mol / L KOH solution and 1.0 mol / L KOH and 0.1 mol / L NH3 solution were used as electrolytes, a three-electrode system was adopted, and the PtZn electrode prepared in Example 1, the PtZnS-200 electrode prepared in Example 2, the PtZnS-300 electrode prepared in Example 3, the PtZnS-400 electrode prepared in Example 4, and the Pt-C electrode prepared in Comparative Example 1 were used as working electrodes, respectively, a mercuric oxide electrode was used as a reference electrode, and a graphite electrode was used as a counter electrode. The linear sweep voltammetry curves and cyclic voltammetry curves of PtZn, PtZnS-200, PtZnS-300, PtZnS-400, PtZnS-500 and Pt-C were tested. (As shown in Figure 3 (shown)
[0064] The electrochemical properties of PtZn, PtZnS-200, PtZnS-300, PtZnS-400, PtZnS-500 and Pt-C in Example 1, Example 2, Example 3, Example 4, Example 5 and Comparative Example 1 were tested by an electrochemical workstation. The electrochemical workstation used was Chenhua electrochemical workstation, model CHI660E.
[0065] The AOR performance of PtZn, PtZnS-200, PtZnS-300, PtZnS-400, PtZnS-500 and Pt-C was tested by cyclic voltammetry. As shown in the AOR cycle curve (CV diagram), the Pt-based bimetallic alloy nanocluster catalyst (PtZnS-400) with appropriate sulfur doping showed better performance, reaching 269.1A g -1 The ammonia oxidation current density was increased by about 150% (110 A g -1 ), and is also superior to common commercial precious metal catalysts (Pt-C).
[0066] like Figure 4 As shown, the appropriately sulfur-doped Pt-based bimetallic alloy nanocluster catalyst (PtZnS-400) can undergo AOR reaction at higher ammonia concentrations and present a normal distribution.
[0067] In summary, the appropriately sulfur-doped Pt-based bimetallic alloy nanocluster catalyst (PtZnS-400) electrocatalytic material provided by the present invention has an AOR electrocatalytic performance far superior to that of the precious metal catalyst (Pt / C), which is conducive to its commercial application in direct ammonia fuel cells.
[0068] The description and practice disclosed in the present invention are easy to think and understand for ordinary technicians in the technical field, and several improvements and modifications can be made without departing from the principles of the present invention. Therefore, modifications or improvements made without departing from the spirit of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing a sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst, It is characterized in that The specific steps are as follows: Step 1, preparation of S-containing carbon black: weigh a certain amount of carbon black and sodium thiosulfate and place them at both ends of a corundum boat respectively, calcine under an inert gas environment, and collect the carbon black containing a certain amount of S element after cooling; Step 2, weighing a certain amount of platinum source, zinc source, ascorbic acid and S-containing carbon black, uniformly dispersing them in ethylene glycol, ultrasonically stirring to obtain a mixed solution, transferring the mixed solution to a polytetrafluoroethylene reactor liner for high-temperature hydrothermal reaction, taking out the sample after natural cooling, washing it by centrifugation with deionized water, and vacuum drying to obtain a sulfur-doped Pt-based bimetallic alloy nanocluster catalyst; Step 3, preparation method of sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst slurry: take the catalyst synthesized in step 2, mix it thoroughly with isopropanol and Nafion solution, and ultrasonicate for 30-60 minutes until it is evenly dispersed.
2. A method for preparing a sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst according to claim 1, It is characterized in that In step 1, the carbon black is any one of acetylene black, Ketjen black, and Super P; the amount of carbon black is 10 to 50 mg, the amount of sodium thiosulfate is 30 to 300 mg, and the calcination temperature is 200° C. to 600° C.
3. The method for preparing a sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst according to claim 1, It is characterized in that In step 2, the amount of platinum source is 10 mg to 50 mg, the amount of zinc source is 10 mg to 50 mg, the amount of ascorbic acid is 50 mg to 200 mg, the volume of ethylene glycol used to disperse the platinum source, zinc source, ascorbic acid and carbon black is 30 ml, the temperature is room temperature, and ultrasound is performed for 30-60 minutes until the dispersion is uniform.
4. The method for preparing a sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst according to claim 1, It is characterized in that In step 2, the platinum source is any one of chloroplatinic acid, platinum acetate and platinum acetylacetonate; the zinc source is any one of zinc acetate, zinc sulfate and zinc acetylacetonate.
5. The method for preparing a sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst according to claim 1, It is characterized in that In step 2, the hydrothermal temperature of the reactor is 100° C. to 200° C., and the thermal reaction time is 6 to 12 hours.
6. The method for preparing a sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst according to claim 1, It is characterized in that In step 2, the cleaning condition is to rinse with deionized water 3 to 5 times.
7. The method for preparing a sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst according to claim 1, It is characterized in that In step 2, the vacuum drying temperature is 50° C. to 80° C., and the drying time is 12 to 24 hours.
8. The method for preparing a sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst according to claim 1, It is characterized in that In step 1, the inert gas is a 5wt% hydrogen-argon mixed gas or high-purity nitrogen, and the calcination temperature is 200°C to 600°C.
9. Use of a sulfur-doped Pt-based bimetallic alloy nanocluster ammonia oxidation catalyst obtained by the preparation method according to any one of claims 1 to 8 in a direct ammonia fuel cell.
Citation Information
Cited By
Preparation method and application of surface hydroxylation platinum-nickel bimetallic seawater hydrogen production catalyst
CN119657232A