Mineral-based expandable foams
The UV resistance and yellowing issues of polyurethane foam are solved by mineral-expanded foam using protective colloid-stabilized polymers and pore formers, enabling a recyclable and fire-resistant alternative suitable for filling cavities.
Patent Information
- Application Number
- CN202280094470.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-04
- Publication Date
- 2024-10-29
AI Technical Summary
Existing polyurethane foam is not UV-resistant when filling cavities, is prone to yellowing, and cannot be recycled, resulting in environmental pollution and high-cost disposal, and is difficult to replace.
A mineral-expanded foam containing a protective colloid-stabilized polymer, a foam stabilizer and a specific pore former is applied through a cartridge to form a one-component mixture (1K system) to replace polyurethane foam.
A UV-resistant, yellowing-resistant, recyclable mineral-expanded foam is achieved, which reduces environmental pollution and disposal costs, and provides fire resistance and good mechanical properties, making it suitable for filling cavities.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to mineral expanded foams, to a method for producing mineral expanded foams and to their use for filling cavities, for example when installing windows or doors. Background Art
[0002] At present, polyurethane foam is usually used to fill the cavity when installing windows or doors. However, polyurethane is associated with a whole series of disadvantages. By way of example, polyurethane is not UV-resistant, has a tendency to yellow and is in particular not fire-resistant. When filling the cavity, an excess of polyurethane foam is usually applied, which then adheres, for example, to the masonry or the window or door and can usually no longer be removed without leaving residues. Residues left as a result of applying polyurethane foam or construction waste contaminated with polyurethane foam must be treated as hazardous waste. Polyurethane foam is usually applied with the aid of cartridges, which cannot be cleaned after their use and are therefore non-recyclable and must be disposed of at great cost and inconvenience. In addition, a more cost-effective polyurethane alternative is needed.
[0003] Against this background, the object is to provide a material for filling cavities which makes it possible to solve one or more of the above-mentioned problems. In particular, the material should be able to be applied through a cartridge.
[0004] Surprisingly, this object was achieved with a mineral expanded foam comprising a polymer stabilized by a protective colloid, a foam stabilizer and a specific pore former as well as a further potential pore former and cement. It was particularly surprising that the mineral expanded foam could also be applied as a one-component mixture (1K system) in a cartridge for filling cavities.
[0005] Cement foam mortars with pore formers and foam stabilizers are known, for example, from WO 2021 / 180309 or WO 2019038105. In WO / EP2021 / 062371 (application number) and DE102014101519, the corresponding foam mortars are used as tile adhesives and as filling compounds, respectively. CN108484211 and CN108529940 recommend foam mortars as insulating materials. DE4209897 and DE3090083 describe gypsum-based foam mortars. GB20047636 relates to silicate foams. DE2056255 discloses foaming agents for gypsum and cement compositions. DE4009967 teaches mortars with pore formers, which are provided with a deactivating coating. US 2012-286190 describes thermal insulation materials based on fast-setting cement and small amounts of Portland cement, as well as fillers and optionally additives as foam formers. Summary of the invention
[0006] The present invention provides mineral expanded foams based on one or more foam stabilizers,
[0007] one or more pore formers selected from the group consisting of ammonium or alkali metal salts of bicarbonates or carbonates,
[0008] optionally one or more fillers, and
[0009] Optionally one or more additives, characterised in that the mineral expanded foam is additionally based on
[0010] A polymer of ethylenically unsaturated monomers stabilized by one or more protective colloids in the form of an aqueous dispersion or a water-redispersible powder,
[0011] one or more potential pore formers selected from the group consisting of aluminum and silicon and their alloys and calcium carbide, and
[0012] 30 to 95% by weight of cement, based on the dry weight of the mineral expanded foam,
[0013] Provided that the proportion of the latent pore former is ≥ 10% by weight based on the total weight of the pore former and the latent pore former.
[0014] The invention further provides a method for producing a mineral expanded foam,
[0015] Wherein a dry mixture is produced by mixing:
[0016] one or more foam stabilizers,
[0017] one or more pore formers selected from the group comprising ammonium or alkali metal salts of bicarbonates or carbonates,
[0018] optionally one or more fillers, and
[0019] Optionally, one or more additives, and
[0020] The dry mixture thus obtained is mixed with water, characterized in that
[0021] a polymer of one or more ethylenically unsaturated monomers stabilized by a protective colloid in the form of a water-redispersible powder,
[0022] one or more potential pore formers selected from the group consisting of aluminum and silicon and their alloys and calcium carbide, and
[0023] 30 to 95% by weight of cement, based on the dry weight of the mineral expanded foam, is additionally introduced into the dry mixture,
[0024] Provided that the dry mixture is based on the latent pore former to an extent of ≥ 10% by weight, based on the total weight of the pore former and the latent pore former.
[0025] The invention further provides for the use of the mineral expanded foam according to the invention for filling cavities, for example when installing windows or doors.
[0026] The invention further provides a method for filling cavities, for example when installing windows or doors, characterised in that these cavities are filled with a mineral expanded foam according to the invention.
[0027] Mineral expanded foams are usually mortars which implicitly contain an increased degree of porosity. The porosity of the mineral expanded foam can be introduced, for example, by pore formers and optionally by the introduction of air.
[0028] The figures given below in % by weight based on the dry weight of the mineral expanded foam are generally based on the dry weight of the components used to produce the mineral expanded foam.
[0029] Examples of air pore formers are one or more ammonium or alkali metal salts of bicarbonates or carbonates, in particular ammonium or sodium or potassium salts thereof. Bicarbonates are particularly preferred. Sodium bicarbonate is most preferred. These air pore formers preferably do not include any alkaline earth metal carbonates.
[0030] The particle size of the pore-forming agent is preferably 10 µm to 1 mm, particularly preferably 100 µm to 800 µm, and most preferably 200 µm to 700 µm.
[0031] The pore formers are usually different from latent air pore formers; that is, pore formers are used as further or additional pore formers in addition to latent air pore formers; or, in other words, the mineral expanded foam usually comprises one or more pore formers i) and one or more latent air pore formers ii). The pore formers i) usually do not comprise any latent air pore formers ii).
[0032] The mineral expanded foam is based on pore formers, preferably to an extent of 0.01 to 10% by weight, more preferably 0.05 to 5% by weight, still more preferably 0.08 to 3% by weight, particularly preferably 0.1 to 1% by weight and most preferably 0.2 to 0.8% by weight, based on the dry weight of the mineral expanded foam.
[0033] The mineral expanded foam is based on pore formers, preferably in an amount of 0.01 to 15% by weight, particularly preferably 0.1 to 5% by weight and most preferably 0.2 to 1% by weight, based on the dry weight of cement present in the mineral expanded foam.
[0034] Introducing air to produce mineral expansion foam can optionally be achieved by mechanically mixing the water-based mortar with air in addition. For this purpose, the water-based mortar can, for example, be beaten, wherein air is mixed therein. Mechanical mixing is preferably carried out by stirring blades, mixing coils, paddle stirrers, propeller stirrers or perforated plate stirrers. Particularly preferred are mixing coils and perforated plates. Foam generators can also be used. Foam generators are commercially available machines for producing foam. It is also possible to blow air into the water-based mortar. The air preferably has a temperature of 5°C to 35°C, particularly ambient temperature.
[0035] Examples of potential pore formers are aluminum and silicon and their alloys or calcium carbide. Aluminum, silicon and their alloys are usually present in metallic form here. Suitable alloys are, for example, alloys of aluminum or silicon with metals such as iron. Preferred aluminum. Potential pore formers can optionally be coated, for example, with fats, oils, resins or waxes (such as lanolin, in particular wool wax) or dry oils (such as linseed oil, silicone oil or silicone resin). For such coatings, the release of air pores in the mineral expansion foam can be delayed in a temporarily controlled manner, for example by the type or thickness of the coating. Potential pore formers are preferably in the form of powders or particles. Corresponding potential pore formers are commercially available, for example from Benda-Lutz under the trade name Expandal 9-6355.
[0036] The mineral expanded foam is based on latent pore formers in an amount of 0.01 to 10% by weight, particularly preferably 0.1 to 5% by weight, still more preferably 0.5 to 4% by weight and most preferably 1 to 3% by weight, based on the dry weight of the mineral expanded foam.
[0037] The mineral expanded foam is based on latent pore formers, preferably in an amount of 0.01 to 15% by weight, particularly preferably 0.5 to 10% by weight and most preferably 1 to 5% by weight, based on the dry weight of cement present in the mineral expanded foam.
[0038] The mineral expanded foam is based on latent pore formers to an extent generally greater than or equal to 10% by weight, preferably 10 to 95% by weight, particularly preferably 50 to 90% by weight and most preferably 75 to 85% by weight, based on the total weight of latent pore formers and further pore formers.
[0039] The mineral expanded foam is based on a latent pore former and an additional pore former, preferably in an amount of 0.01% to 15% by weight, particularly preferably 0.5% to 10% by weight and most preferably 1% to 5% by weight, based on the dry weight of the cement present in the mineral expanded foam. The mineral expanded foam is based on a latent pore former and an additional pore former, preferably in an amount of 0.02% to 15% by weight, particularly preferably 0.5% to 10% by weight and most preferably 1% to 5% by weight, based on the dry weight of the mineral expanded foam. The additional pore formers here are generally the above-mentioned pore formers which are different from the latent pore formers.
[0040] Foam stabilizers based on, for example, surfactants, polymers, proteins or enzymes may be used.
[0041] Examples of surfactants as foam stabilizers are olefinsulfonic acids; fatty acids or salts thereof, preferably having 16 to 18 carbon atoms; fatty alcohols, preferably having 10 to 18 carbon atoms; alkylphenols or hydroxyalkylphenols, preferably having an alkyl chain of 10 to 18 carbon atoms; alkyl and alkylaryl ether sulfates having preferably 8 to 18 carbon atoms and preferably 1 to 50 ethylene oxide units in the hydrophobic group; sulfonates, in particular alkylsulfonates having preferably 8 to 18 carbon atoms, alkylarylsulfonates, preferably having an alkyl group of 8 to 18 carbon atoms, esters or monoesters of sulfosuccinic acid with preferably monohydric alcohols or alkylphenols having preferably 4 to 15 carbon atoms in the alkyl group, wherein these alcohols or alkylphenols may also be ethoxylated with 1 to 40 ethylene oxide units; metaphosphates, in particular alkyl or alkaryl phosphates having 8 to 20 carbon atoms in the organic group, alkyl esters having 8 to 20 carbon atoms and 1 to 50 EO units in the alkyl or alkaryl group; Ether phosphates and alkyl aryl ether phosphates; preferably alkyl polyglycol ethers having 8 to 40 EO units and alkyl groups having 8 to 20 carbon atoms; alkyl aryl polyglycol ethers, preferably having 8 to 40 EO units and 8 to 20 carbon atoms in the alkyl and aryl groups; preferably ethylene oxide / propylene oxide (EO / PO) block copolymers having 8 to 40 EO or PO units; preferably N-methyl taurates of higher fatty acids having 10 to 18 carbon atoms; fatty acid alkyl Alcoholamides, such as monoethanolamides or diethanolamides of fatty acids; amine oxides or phosphine oxides, such as cocodimethylamine oxide or cocodimethylphosphine oxide of the general formula RN(CH3)2=0 or RP(CH3)2=0; ampholytes, such as sodium cocoyldimethylaminoacetate or sulfobetaine; phosphoric acid esters, in particular phosphoric acid esters of long-chain alcohols having preferably 10 to 18 carbon atoms, or alcohols which have been ethoxylated with 1 to 4 mol of ethylene oxide and have 8 to 10 carbon atoms in the molecule.
[0042] Preferred surfactants herein are olefin sulfonic acids, fatty acids, fatty alcohols, alkyl and alkyl aryl ether sulfates and sulfonates.
[0043] The EO units are ethylene oxide units and the PO units are propylene oxide units. The above acids can also be in the form of their salts, in particular ammonium salts or alkali (alkaline earth) metal salts. The olefin sulfonic acids preferably contain 10 to 20 carbon atoms. The olefin sulfonic acids preferably carry one or two sulfonic acid or hydroxyalkylsulfonic acid groups. Preference is given here to alpha-olefin sulfonic acids.
[0044] Examples of polymers as foam stabilizers are polyvinyl alcohol; polyvinyl acetal; polyvinyl pyrrolidone; water-soluble forms of polysaccharides such as starch (amylose and amylopectin), cellulose and its derivatives such as carboxymethyl, methyl, hydroxyethyl, hydroxypropyl derivatives, dextrins and cyclodextrins; lignin sulfonates; poly(meth)acrylic acid; copolymers of (meth)acrylates with carboxyl-functionalized comonomer units; poly(meth)acrylamide; polyvinylsulfonic acid and its water-soluble copolymers; melamine-formaldehyde sulfonates; naphthalene-formaldehyde sulfonates; styrene-maleic acid copolymers and vinyl ether-maleic acid copolymers.
[0045] Examples of proteins as foam stabilizers are casein, caseinates, soy protein or gelatin. Proteins can be obtained, for example, by protein hydrolysis, in particular animal proteins, for example from horns, blood, bones and similar waste products of cattle, pigs and other animal carcasses. Enzymes as foam stabilizers can, for example, be of biotechnological origin.
[0046] Preferred foam stabilizers are surfactants; polyvinyl alcohol; polyvinyl pyrrolidone; cellulose and its derivatives, such as carboxymethyl, methyl, hydroxyethyl, hydroxypropyl derivatives; proteins such as casein or caseinates, soy protein and gelatin.
[0047] Particularly preferred foam stabilizers are surfactants, especially olefin sulfonic acids.
[0048] Particularly preferred is the combined use of a surfactant foam stabilizer and a polymer foam stabilizer.
[0049] These foam stabilizers preferably have a molecular weight of ≤4000 g / mol, more preferably ≤3000 g / mol, even more preferably ≤2500 g / mol, particularly preferably ≤1500 g / mol and most preferably ≤1000 g / mol.
[0050] Foam stabilizers and protective colloid-stabilized polymers are usually present simultaneously with one another. Foam stabilizers are usually not a component of the protective colloid-stabilized polymer.
[0051] The mineral expanded foam is based on the foam stabilizer to a degree of preferably 0.01% to 35% by weight, particularly preferably 0.05% to 20% by weight and most preferably 0.1% to 10% by weight. The surfactant or polymer as foam stabilizer is present in a degree of preferably 0.01% to 10% by weight, particularly preferably 0.05% to 5% by weight and most preferably 0.1% to 3% by weight. The protein or enzyme as foam stabilizer is present in a degree of preferably 10% to 35% by weight, particularly preferably 15% to 30% by weight and most preferably 20% to 25% by weight. The figures of % by weight are based on the dry weight of the mineral expanded foam.
[0052] The mineral expanded foams are based on polymers of ethylenically unsaturated monomers stabilized by protective colloids, the extent of which is preferably 0.5 to 40% by weight, particularly preferably 2 to 25% by weight and most preferably 5 to 15% by weight, based on the dry weight of the mineral expanded foam.
[0053] The polymers of ethylenically unsaturated monomers are based, for example, on one or more monomers selected from the group consisting of vinyl esters, (meth)acrylates, vinyl aromatic compounds, olefins, 1,3-dienes and vinyl halides.
[0054] Suitable vinyl esters are, for example, vinyl esters of carboxylic acids having 1 to 15 carbon atoms. Preference is given to vinyl acetate, vinyl propionate, vinyl butyrate, vinyl 2-ethylhexanoate, vinyl laurate, 1-methylvinyl acetate, vinyl pivalate and vinyl esters of α-branched monocarboxylic acids having 9 to 11 carbon atoms, such as VeoVa 9R or VeoVa 10R (trade names of Resolution). Particular preference is given to vinyl acetate.
[0055] Suitable monomers from the group of acrylates or methacrylates are, for example, esters of unbranched or branched alcohols having 1 to 15 carbon atoms. Preferred methacrylates or acrylates are methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, n-butyl acrylate, n-butyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, 2-ethylhexyl acrylate. Particularly preferred are methyl acrylate, methyl methacrylate, n-butyl acrylate, tert-butyl acrylate and 2-ethylhexyl acrylate.
[0056] Preferred vinyl aromatic compounds are styrene, methylstyrene and vinyltoluene. Preferred vinyl halides are vinyl chloride. Preferred olefins are ethylene and propylene, and preferred dienes are 1,3-butadiene and isoprene.
[0057] Optionally, it is also possible to copolymerize 0 to 10% by weight, preferably 0.1 to 5% by weight, of auxiliary monomers, based on the total weight of the monomers. Examples of auxiliary monomers are ethylenically unsaturated mono- and dicarboxylic acids, preferably acrylic acid, methacrylic acid, fumaric acid and maleic acid; ethylenically unsaturated carboxamides and nitriles, preferably acrylamide and acrylonitrile; mono- and diesters of fumaric acid and maleic acid, such as diethyl and diisopropyl esters, and maleic anhydride; ethylenically unsaturated sulfonic acids or their salts, preferably vinylsulfonic acid and 2-acrylamido-2-methylpropanesulfonic acid. Further examples are pre-crosslinking comonomers, such as polyethylenically unsaturated comonomers, for example diallyl phthalate, divinyl adipate, diallyl maleate, allyl methacrylate or triallyl cyanurate, or post-crosslinking comonomers, such as acrylamidoglycolic acid (AGA), methyl methacrylamidoglycolate (MAGME), N-methylolacrylamide (NMA), N-methylolmethacrylamide, N-methylolallylcarbamate, alkyl ethers, such as isobutoxy ether or esters of N-methylolacrylamide, N-methylolmethacrylamide and N-methylolallylcarbamate. Also suitable are epoxy-functional comonomers, such as glycidyl methacrylate and glycidyl acrylate. Further examples are silicon-functional comonomers such as acryloxypropyltri(alkoxy)- and methacryloxypropyltri(alkoxy)silanes, vinyltrialkoxysilanes and vinylmethyldialkoxysilanes, in which the alkoxy groups present may be, for example, ethoxy and ethoxypropylene glycol ether groups. Mention should also be made of monomers having hydroxyl or CO groups, such as hydroxyalkyl methacrylates and acrylic esters such as hydroxyethyl, hydroxypropyl or hydroxybutyl acrylic or methacrylic acid, and compounds such as diacetoneacrylamide and acetoacetoxyethyl acrylic or methacrylic acid.
[0058] Preference is given to copolymers of vinyl acetate with 1 to 50% by weight of ethylene; copolymers of vinyl acetate with 1 to 50% by weight of ethylene and 1 to 50% by weight of one or more further comonomers from the group of vinyl esters having 1 to 12 carbon atoms in the carboxyl group, such as vinyl propionate, vinyl laurate, vinyl esters of α-branched carboxylic acids having 9 to 13 carbon atoms, such as VeoVa 9, VeoVa 10, VeoVa 11; copolymers of vinyl acetate, 1 to 50% by weight of ethylene and preferably 1 to 60% by weight of (meth)acrylic esters of unbranched or branched alcohols having 1 to 15 carbon atoms, in particular n-butyl acrylate or 2-ethylhexyl acrylate. and copolymers with 30 to 75% by weight of vinyl acetate, 1 to 30% by weight of vinyl laurate or of vinyl esters of α-branched carboxylic acids having 9 to 11 carbon atoms and 1 to 30% by weight of (meth)acrylic esters of unbranched or branched alcohols having 1 to 15 carbon atoms, in particular n-butyl acrylate or 2-ethylhexyl acrylate, the copolymers also containing 1 to 40% by weight of ethylene; copolymers with vinyl acetate, 1 to 50% by weight of ethylene and 1 to 60% by weight of vinyl chloride; wherein the polymers may also contain the auxiliary monomers mentioned in the amounts mentioned, and the figures in % by weight in each case add up to 100% by weight.
[0059] Also preferred are (meth)acrylate polymers, such as copolymers of n-butyl acrylate or 2-ethylhexyl acrylate or copolymers of methyl methacrylate with n-butyl acrylate and / or 2-ethylhexyl acrylate; styrene-acrylate copolymers with one or more monomers from the group of methyl acrylate, ethyl acrylate, propyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate; vinyl acetate-acrylate copolymers with one or more monomers from the group of methyl acrylate, ethyl acrylate, propyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate and optionally ethylene; styrene-1,3-butadiene copolymers; wherein the polymers may also comprise the auxiliary monomers mentioned in the amounts mentioned, and the figures in % by weight in each case add up to 100% by weight.
[0060] Most preferred are copolymers with vinyl acetate and 5 to 50% by weight of ethylene; or copolymers with vinyl acetate, 1 to 50% by weight of ethylene and 1 to 50% by weight of vinyl esters of α-branched monocarboxylic acids having 9 to 11 carbon atoms; or copolymers with 30 to 75% by weight of vinyl acetate, 1 to 30% by weight of vinyl laurate or vinyl esters of α-branched carboxylic acids having 9 to 11 carbon atoms, and 1 to 30% by weight of (meth)acrylic esters of unbranched or branched alcohols having 1 to 15 carbon atoms, the copolymers also containing 1 to 40% by weight of ethylene; or copolymers with vinyl acetate, 5 to 50% by weight of ethylene and 1 to 60% by weight of vinyl chloride.
[0061] The weight ratio of these monomers and these comonomers is selected so as to produce a glass transition temperature Tg of -25°C to +35°C, preferably -10°C to +25°C, particularly preferably -10°C to +20°C. The glass transition temperature Tg of the polymer can be determined in a known manner by differential scanning calorimetry (DSC). The approximate Tg can also be precalculated by the Fox equation. According to Fox TG, Bull. Am. Physics Soc. 1, 3, page 123 (1956): 1 / Tg = x1 / Tg1 +x2 / Tg2 + ...+ xn / Tgn, wherein xn is the mass fraction (by weight % / 100) of monomer n, and Tgn is the glass transition temperature of the homopolymer of monomer n in Kelvin. The Tg values of homopolymers are listed in Polymer Handbook 2nd Edition, J. Wiley & Sons, New York (1975).
[0062] The polymers are usually prepared in aqueous medium and preferably by emulsion or suspension polymerization processes - as described, for example, in DE-A 102008043988. In the polymerization, standard protective colloids and / or emulsifiers can be used, as described in DE-A 102008043988. The polymers in the form of aqueous dispersions can be converted into the corresponding water-redispersible powders, as described in DE-A 102008043988. In general, a drying aid is used here, preferably the above-mentioned polyvinyl alcohol.
[0063] These polymers can be, for example, in the form of aqueous dispersions, in particular protective colloid-stabilized aqueous dispersions. Preferred protective colloids are polyvinyl alcohols, such as partially hydrolyzed or fully hydrolyzed polyvinyl alcohols, in particular with a degree of hydrolysis of 80 mol % to 100 mol %. Particularly preferred are partially hydrolyzed polyvinyl alcohols with a degree of hydrolysis of 80 mol % to 94 mol % and, in particular, a Höppler viscosity of 1 mPas to 30 mPas in a 4% aqueous solution (Höppler method at 20° C., DIN 53015). The mentioned protective colloids can be obtained by methods known to those skilled in the art. The protective colloids are generally present in a total amount of 1% to 20% by weight, based on the total weight of the polymer.
[0064] The polymer is preferably in the form of a protective colloid-stabilized, water-redispersible powder. Dispersing the protective colloid-stabilized, water-redispersible polymer powder results in the protective colloid-stabilized polymer in water-redispersible form. The powder preferably comprises 3 to 30% by weight, particularly preferably 5 to 20% by weight, of polyvinyl alcohol, in particular the abovementioned polyvinyl alcohols, based on the total weight of the powder.
[0065] The protective colloid-stabilized polymer is usually present separately from the pore former, latent pore former and / or foam stabilizer. The pore former, latent pore former and / or foam stabilizer are usually not coated with the protective colloid-stabilized polymer. The protective colloid-stabilized polymer or protective colloid or protective colloid-stabilized polymer is usually different from the foam stabilizer and any thickener.
[0066] The cement may be, for example, Portland cement (CEM I), Portland slag cement (CEM II), blast furnace slag cement (CEM III), pozzolanic cement (CEM IV), composite cement (CEM V), Portland silicate dust cement, Portland shale cement, Portland limestone cement, volcanic rock cement, magnesium oxide cement, phosphate cement, blended cement or filler cement or quick-setting cement. Examples of quick-setting cements are aluminate cement, calcium sulphoaluminate cement and high alumina cement.
[0067] Preference is given to Portland cement CEM I, Portland slag cement CEM II / AS, CEM II / BS, Portland limestone cement CEM II / A-LL, Portland fly ash cement CEM II / AV, Portland fly ash slag cement CEM II / B-SV or blast furnace slag cement CEM III / A, CEM III / B, CEM III / B and also aluminate cement.
[0068] The mineral expanded foam is cement-based, preferably to an extent of 40 to 95% by weight, more preferably 50 to 92% by weight, particularly preferably 60 to 91% by weight and most preferably 70 to 90% by weight, based on the dry weight of the mineral expanded foam.
[0069] In a preferred example, the mineral expanded foam comprises a fast-setting cement, such as a high-alumina cement, in particular aluminate cement or calcium sulfoaluminate cement, and one or more cements other than fast-setting cement, in particular Portland cement. Rapidly setting cements are particularly advantageous for achieving the objects according to the invention.
[0070] The mineral expansive foam is based on fast-setting cement to an extent of preferably 0.5 to 30% by weight, particularly preferably 1 to 20% by weight and most preferably 2 to 10% by weight, based on the dry weight of the mineral expansive foam. The mineral expansive foam is based on fast-setting cement to an extent of preferably 0.5 to 40% by weight, particularly preferably 1 to 25% by weight and most preferably 2 to 15% by weight, based on the total weight of all cements used.
[0071] The mineral expansion foam may also contain one or more thickeners, for example polysaccharides such as cellulose ethers and modified cellulose ethers, cellulose esters, starch ethers, guar gum, xanthan gum, polycarboxylic acids such as polyacrylic acid and partial esters thereof, casein and associative thickeners. Preferred cellulose ethers are methyl cellulose ethers. The thickener is usually different from the foam stabilizer. These thickeners have a molecular weight of preferably >4000 g / mol, particularly preferably ≥10000 g / mol and most preferably ≥20000 g / mol. The mineral expansion foam is based on a thickener, the extent of which is preferably ≤5% by weight, particularly preferably 0.1% to 3% by weight and most preferably 0.5% to 1.5% by weight, based on the dry weight of the mineral expansion foam.
[0072] In addition, the mineral expanded foam may also contain a setting accelerator, such as an aluminum compound, a silicate, an alkaline earth metal hydroxide, a nitrate, a nitrite, a sulfate, a borate or a carboxylic acid. Preferred setting accelerators are aluminum salts, aluminates, alkali metal silicates, such as water glass, alkali metal formates, potassium hydroxide or calcium hydroxide (Ca(OH)2). Calcium hydroxide is also called slaked lime or refined slaked lime. The setting accelerator is usually not in the form of a metal, an alloy or a carbide. The setting accelerator is usually different from the potential pore former.
[0073] The mineral expanded foam is based on a setting accelerator, preferably to an extent of 0.1 to 15% by weight, more preferably 0.2 to 10% by weight, particularly preferably 0.3 to 7% by weight and most preferably 0.5 to 3% by weight, based on the dry weight of the mineral expanded foam.
[0074] The mineral expanded foam may additionally contain fibers, for example natural, modified natural or synthetic fiber materials based on organic and / or inorganic materials. Examples of natural organic fibers are cotton, hemp, jute, flax, wood fibers, cellulose, viscose, leather fibers or sisal. Examples of synthetic organic fibers are viscose fibers, polyamide fibers, polyester fibers, polyacrylonitrile fibers, Dralon fibers, polyethylene fibers, polypropylene fibers, polyvinyl alcohol fibers or aramid fibers. Inorganic fibers may be glass fibers, carbon fibers, mineral wool fibers or metal fibers, for example. Cotton fibers, polyacrylonitrile fibers and cellulose fibers are preferred. The fibers preferably have a length of 1 to 10 mm, 2 to 6 mm and most preferably 3 mm to 4 mm. The fibers may be used in the form of loose fibers, fibers bonded to bundles, fibrillated fibers, multifilament fibers or fibers in a dosage controlled package. Based on the dry weight of the components used to produce the mineral expanded foam, the mineral expanded foam is based on fibers preferably at a level of 0.01% to 3% by weight, particularly preferably 0.05% to 1% by weight, and most preferably 0.1% to 0.5% by weight. The fibers may increase the mechanical stability of the mineral expanded foam and reduce the tendency of the mineral expanded foam towards cracking.
[0075] The mineral expanded foam may also contain one or more pozzolans, such as kaolin, microsilica, diatomaceous earth, fly ash, ground coarse sandstone, ground blast furnace slag, ground glass, precipitated silica and fumed silica. Preferred pozzolans are kaolin, microsilica, fly ash, ground blast furnace slag, in particular metakaolin. The mineral expanded foam is based on pozzolans, for example to an extent of 0% to 10% by weight, preferably 0.5% to 5% by weight, based on the dry weight of the mineral expanded foam. Most preferably, the mineral expanded foam does not contain any pozzolans.
[0076] Preferably, the mineral expanded foam is based on gypsum, in an amount of 0.1 to 20% by weight, more preferably 0.5 to 15% by weight and particularly preferably 1 to 10% by weight, based on the dry weight of the components used to produce the mineral expanded foam. Exemplary embodiments of gypsum are alpha- or beta-hemihydrate (CaSO4 1 / 2 H2O), dihydrate, anhydrite or calcium sulfate (FGD gypsum) obtained in flue gas desulfurization. In particular, the addition of gypsum makes it possible, for example, to compensate for any shrinkage during the setting of the mineral expanded foam.
[0077] Alternatively, the gypsum can be omitted. This can, for example, improve the water resistance of the set mineral expanded foam.
[0078] The mineral expanded foam may also contain one or more fillers. Examples of fillers are quartz sand, ground quartz, sand, ground limestone, dolomite, clay, chalk, ground slag sand, white slaked lime, talc or mica, rubber particles or hard fillers such as aluminum silicate, corundum, basalt, carbides such as silicon carbide or titanium carbide. Preferred fillers are quartz sand, crushed quartz, crushed limestone, calcium carbonate, calcium magnesium carbonate (dolomite), chalk or white slaked lime. The filler is usually not in the form of a metal, alloy or carbide. The filler is usually different from the potential pore former. The filler has a particle size of preferably ≤2 mm, particularly preferably ≤1 mm.
[0079] The mineral expanded foam is based on fillers, preferably to an extent of ≤10% by weight, particularly preferably ≤5% by weight, based on the dry weight of the mineral expanded foam.
[0080] Most preferably, the mineral expanded foam does not contain any filler.
[0081] Mineral expansion foam can also include lightweight fillers. "Lightweight filler" generally refers to fillers with low bulk weight, usually less than 500 g / l. Lightweight fillers are preferably different from the above-mentioned fillers. Particularly preferably, in addition to lightweight fillers, mineral expansion foam does not contain any additional fillers. On a synthetic or natural basis, typical lightweight fillers are hollow microspheres of materials such as glass, polymers such as polystyrene beads, aluminosilicates, silicon oxides, aluminum oxides, hydrated calcium silicates, silicon dioxide, aluminum silicates, magnesium silicates, hydrated aluminum silicates, aluminum silicates, hydrated calcium silicates, aluminum iron magnesium silicates, calcium metasilicates and / or volcanic slag. Preferred lightweight fillers are perlite, Celite, Cabosil, Circosil, Eurocell, Filite, Promaxon, Vermex and / or wollastonite, and polystyrene. Lightweight fillers are not usually in the form of metals, alloys or carbides. Fillers are usually different from potential pore formers.
[0082] The mineral expanded foam is based on light fillers to an extent of preferably 0 to 10% by weight, more preferably 0.5 to 5% by weight and particularly preferably 1 to 3% by weight, based on the dry weight of the mineral expanded foam. Most preferably, the mineral expanded foam does not contain any light fillers.
[0083] Optionally, the mineral expanded foam may also contain additives, such as plasticizers, superplasticizers, flame retardants, film-forming aids, dispersants, hydrophobizing agents, pigments, preservatives, flame retardants (e.g. aluminum hydroxide), finely dispersed silicon dioxide. Preferred additives are superplasticizers, plasticizers and in particular hydrophobizing agents. The additives are preferably present in an amount of 0 to 20% by weight, particularly preferably 0.1 to 10% by weight and most preferably 0.5 to 7% by weight, based on the dry weight of the mineral expanded foam.
[0084] Examples of hydrophobizing agents are fatty acids or derivatives thereof, waxes and organosilicon compounds such as silanes or siloxanes.
[0085] Examples of organosilicon compounds are silanes of the formula (I) and / or mixtures thereof and / or hydrolysis products thereof, in particular oligomers or polymers of the hydrolysis products,
[0086] (RO) 4-n SiR' n (I)
[0087] Where n is from 1 to 3.
[0088] wherein each R′ is identical or different and is a branched or unbranched alkyl radical having 1 to 22 carbon atoms, a cycloalkyl radical having 3 to 10 carbon atoms, an alkylene radical having 2 to 4 carbon atoms, and an aryl, aralkyl, alkaryl radical having 6 to 18 carbon atoms, and R is identical or different, in each case an alkyl radical and an alkoxyalkylene radical having 1 to 20 carbon atoms, in particular 1 to 4 carbon atoms, or a trimethylsilyl radical or hydrogen, preferably methyl and ethyl.
[0089] Preferably, R' is an alkyl group having 1 to 12 carbon atoms, particularly preferably 1 or 8 carbon atoms. The alkyl group may be straight-chain or branched. Preferably, R is hydrogen, an alkyl group having 1 to 4 carbon atoms, such as a methyl, ethyl, propyl or butyl group, in particular an ethyl group.
[0090] The organosilicon compound can be introduced, for example, in pure, solid or preferably liquid form. The organosilicon compound can be added undiluted or diluted, for example with a solvent such as an alcohol, in particular ethanol, or in the form of an aqueous emulsion. In addition, the organosilicon compound can be used in the form of a powder. Liquid organosilicon compounds are preferably used in a supported form, for example absorbed on a carrier such as silicon dioxide, or as an encapsulated powder, for example encapsulated with polyvinyl alcohol or alginate.
[0091] Corresponding organosilicon compounds are commercially available.
[0092] Preferred fatty acids or fatty acid derivatives are selected from the group consisting of saturated and unsaturated fatty acids having 8 to 22 carbon atoms, their metal soaps, their amides and their esters with monohydric alcohols having 1 to 14 carbon atoms, with diols, with polyglycols, with polyalkylene glycols, with glycerol, with mono-, di- or triethanolamine, with monosaccharides and with polyhydroxy compounds.
[0093] Particularly preferred fatty acids are lauric acid (n-decanoic acid), myristic acid (n-tetradecanoic acid), palmitic acid (n-hexadecanoic acid), stearic acid (n-octadecanoic acid) and oleic acid (9-dodecenoic acid).
[0094] Particularly preferred metal soaps are preferably C8- to C 22 - those of fatty acids, with a metal of main group 1 to 3 or transition group 2 of PTE, and with an ammonium compound NX4 + , wherein X is the same or different and is H, C1- to C8-alkyl groups and C1- to C8-hydroxyalkyl groups. Most preferred are metal soaps with lithium, sodium, potassium, magnesium, calcium, aluminum, zinc, and ammonium compounds.
[0095] Particularly preferred fatty acid amides are those prepared from the above-mentioned mono- or diethanolamine and C8- to C 22 - Fatty acid amides obtainable from fatty acids.
[0096] Particularly preferred fatty acid esters are the C8- to C 22 - fatty acids C1- to C 14 -alkyl esters and -alkylaryl esters, preferably methyl, ethyl, propyl, butyl, ethylhexyl esters and benzyl esters. Particularly preferred fatty acid esters are also C8- to C 22 -mono-, di- and polyethylene glycol esters of fatty acids. Further particularly preferred fatty acid esters are monoesters and diesters of polyethylene glycols and / or polyalkylene glycols having up to 20 oxyalkylene units, such as polyethylene glycol and polypropylene glycol. Also particularly preferred are glycerol with the C8- to C6- 22 -mono-, di- and tri-fatty acid esters of fatty acids, and mono-, di- and triethanolamine with the C8- to C 22 - fatty acid esters of mono-, di- and tri-fatty acids. Particularly preferred are fatty acid esters of sorbitol and mannitol. Particularly preferred are C1- to C2-containing fatty acids of lauric acid and oleic acid. 14 - alkyl and alkylaryl esters, mono- and diethylene glycol esters of lauric acid and oleic acid, and mono-, di- and tri-fatty acid esters of glycerol with lauric acid and oleic acid.
[0097] The mineral expanded foam comprises a hydrophobizing agent preferably in an amount of 0.01 to 5% by weight, particularly preferably 0.05 to 2% by weight and most preferably 0.1 to 0.8% by weight, based on the dry weight of the mineral expanded foam.
[0098] The mineral expanded foam preferably does not contain any hexafluorosilicic acid, in particular any salts of hexafluorosilicic acid, such as calcium, magnesium, zinc or ammonium salts.
[0099] The mineral expanded foam is preferably a 1K system; that is to say, all components of the mineral expanded foam are preferably mixed in a mixing device. Particularly preferably, the mineral expanded foam is first produced in the form of a dry mixture and water is then added.
[0100] The individual components of the mineral expanded foam can be mixed in standard mixing devices, for example with a mortar mixing assembly, a mechanical drill stirrer, a dissolver or a mixing-coil stirrer, preferably at a stirring or mixing assembly speed of >100 rpm. This generally introduces air pores into the mineral expanded foam, for example via pore formers and optionally via the introduction of air, as already described further above.
[0101] When adding water, the mineral expanded foam is mixed and replenished for preferably 1 to 10 minutes, particularly preferably 2 to 5 minutes. The mixing is preferably carried out at 5°C to 35°C, particularly preferably 15°C to 25°C.
[0102] To produce the aqueous mineral expanded foam, 4 to 30% by weight, particularly preferably 6 to 20% by weight and most preferably 8 to 15% by weight, of water, based on the dry weight of the mineral expanded foam, are used.
[0103] The aqueous mineral expanded foam can be applied, for example, immediately after formulation with water, preferably not more than 10 minutes after formulation with water, particularly preferably not more than 5 minutes.
[0104] The mineral expanded foam generally contains pores. The mineral expanded foam preferably has a creamy or creamy consistency. The mineral expanded foam has a density of preferably 100 to 1000 kg / m 3 , particularly preferably 200 to 900 kg / m 3 And most preferably 300 to 800 kg / m 3 The density can be determined in a conventional manner, for example by filling a container with a defined volume of foam and weighing it.
[0105] Preferably, the mineral expanded foam obtained in this way is applied immediately after having been produced, in particular without further processing steps.
[0106] Mineral expansion foams are preferably used to fill cavities, for example when installing windows or doors, in particular for filling the cavity between the window or door frame and the window or door glass. Furthermore, mineral expansion foams can also be used to fill cavities when installing roller shutter boxes or for filling slots when laying pipes or cables. Mineral expansion foams are also suitable for filling cavities in formwork construction or between prefabricated concrete parts or other spaces. Furthermore, cavities in shipbuilding processes can also be filled with mineral expansion foams.
[0107] The mineral expansion foam can advantageously be applied in a conventional manner, as is known, for example, from the filling of cavities with polyurethane foam (PU foam). For example, the aqueous mineral expansion foam can be applied to the substrate mechanically (for example using a sprayer) or preferably manually (for example using a spatula) or preferably via a cartridge filled with the aqueous mineral expansion foam. Any protruding residues of the mineral expansion foam can be removed, for example, by a spatula or washed off before or after it has solidified.
[0108] The mineral expanded foam can be applied here to standard substrates, for example to mineral substrates such as natural stone, bricks, tiles, concrete blocks, aerated concrete, concrete, screeds, plaster or floor filling compounds, or to natural organic substrates such as wood, or to artificial substrates such as polyvinyl chloride. The mineral expanded foam can also be applied to a variety of insulating materials, for example to glass fiber materials, polystyrene sheets, polyurethane sheets, mineral fiber sheets or mineral wool sheets.
[0109] The solidified mineral expanded foam has a relative humidity of preferably 10 to 1000 kg / m after 28 days under standard climatic conditions (23° C., 50% relative humidity). 3 , particularly preferably 100 to 800 kg / m 3 Dry bulk density (determination method: based on EN 1015-6).
[0110] The mineral expanded foam (solid mortar) has a thermal conductivity of preferably 50 to 200 mW / mK, particularly preferably 30 to 100 mW / mK after 28 days under standard climatic conditions (23° C., 50% relative humidity). The thermal conductivity is determined with an HFM 436 thermal conductivity measuring device from Netzsch in accordance with DIN EN 13163. The measurement is carried out with the "Lambda 10° C." setting; the lower plate is set to 2.5° C. and the upper plate to 17.5° C. The test substrate is sandwiched in between and the measurement is continued until the test substrate has reached a core temperature of 10° C.
[0111] Surprisingly, the mineral expanded foam according to the invention can be used like polyurethane foam, for example, to fill cavities when installing windows or doors. In this case, the mineral expanded foam is very user-friendly. For example, in contrast to polyurethane foam, by simple scraping (for example using a scraper) or by washing, protruding residues can be removed practically without leaving residues and without yellowing. Such residues of the mineral expanded foam can be disposed of with household waste and are not hazardous waste in contrast to polyurethane foam. The cartridge filled with the mineral expanded foam can be cleaned after its use and advantageously reused, which reduces the need for cartridges. Furthermore, the mineral expanded foam is UV-resistant, has no tendency to yellowing and is in particular fire-resistant.
[0112] Furthermore, the solidified mineral expanded foam exhibits advantageous mechanical properties, in particular a high compressive strength or flexural strength. The dry bulk density of the mineral expanded foam is also advantageously low.
[0113] It is particularly surprising here that the aqueous mineral expanded foam can also be applied as a one-component mixture (1K system) via cartridges and that this use makes it possible to obtain a foam with which conventional polyurethane foams can be replaced. DETAILED DESCRIPTION
[0114] The following examples serve to illustrate the present invention in more detail and should not be considered limiting in any way.
[0115] Production of mineral expanded foam:
[0116] Embodiment 1:
[0117] The amount of water specified in Table 1 was added to the dry mixture of the components listed in Table 1 and after 3 minutes of stirring using a Toni mixer (level 2; 130 rpm) a ready-to-use aqueous mineral expanded foam having a creamy consistency was obtained.
[0118] The aqueous mineral expanded foam thus obtained is placed in a cartridge and thus used to fill the cavity.
[0119] Components of mineral expanding foam:
[0120] - Polymer powder:
[0121] a water-redispersible polymer powder of a polyvinyl alcohol-stabilized vinyl acetate-ethylene copolymer having a glass transition temperature of 16°C;
[0122] - Tylose MH 60010 P4 (trade name of Shin Etsu):
[0123] Etherified methyl hydroxyethyl cellulose (thickener);
[0124] - Hostapur OSB (trade name of Shin Etsu):
[0125] Sodium salt of C14 / C16-alpha-olefin sulfonic acid;
[0126] - Milke CEM I 52, 5R: Portland cement;
[0127] - Fondu Lafarge (trade name Imerys):
[0128] Calcium aluminate cement (quick-setting cement);
[0129] - Walhalla Edelhydrate:
[0130] Calcium hydroxide (Ca(OH)2) (potentially hydraulic binder);
[0131] - Expandal 9-6355 (trade name Benda-Lutz):
[0132] Aluminum metal powder.
[0133] Table 1: Formulation of mineral expanded foam from Example 1:
[0134]
[0135] Tests on the mineral expanded foam from Example 1:
[0136] The wet and dry densities of the expanded foam are determined using a density measuring cup.
[0137] The determination of the flexural strength and the compressive strength and the production of the test specimens were carried out in accordance with DIN 18555-3 and according to the storage conditions specified in Table 2.
[0138] Thermal conductivity is determined as specified further above in the general description.
[0139] The test results are summarized in Table 2.
[0140] Table 2: Test results of mineral expanded foam of Example 1:
[0141]
[0142] a) 28dSCC: tested after 28 days of storage under standard climatic conditions.
[0143] Comparative Example 2:
[0144] A dry mixture was produced by mixing with water as described in Example 1, the only difference being that 24 parts by weight of sodium bicarbonate were used and no Expandal 9-6355 was used.
[0145] The product thus obtained cannot be applied using a cartridge due to its consistency and is therefore not suitable for filling cavities.
Claims
1. A mineral expansion foam based on one or more foam stabilizers, one or more pore formers selected from the group consisting of ammonium or alkali metal salts of bicarbonates or carbonates, optionally one or more fillers and optionally one or more additives, characterized in that The mineral expanded foam is additionally based on A polymer of ethylenically unsaturated monomers stabilized by one or more protective colloids in the form of an aqueous dispersion or a water-redispersible powder, one or more potential pore formers selected from the group consisting of aluminum and silicon and their alloys and calcium carbide, and 30 to 95% by weight of cement, based on the dry weight of said mineral expanded foam, Provided that the proportion of the latent pore former is ≥ 10% by weight based on the total weight of the pore former and the latent pore former.
2. The mineral expanded foam according to claim 1, characterized in that The mineral expanded foam is based on latent pore formers in an amount of 0.01 to 10% by weight, based on the dry weight of the mineral expanded foam.
3. The mineral expanded foam according to claim 1 or 2, characterized in that The mineral expanded foam is based on latent pore formers to an extent of 0.01 to 15% by weight, based on the dry weight of cement present in the mineral expanded foam.
4. Mineral expanded foam according to claims 1 to 3, characterized in that The mineral expanded foam is based on latent pore formers to an extent of 10 to 95% by weight, based on the total weight of the latent pore formers and the pore formers.
5. Mineral expanded foam according to claims 1 to 4, characterized in that The mineral expanded foam is based on the latent pore former and the pore former to an extent of 10 to 95% by weight, based on the dry weight of cement present in the mineral expanded foam.
6. Mineral expanded foam according to claims 1 to 5, characterized in that The mineral expanded foam is based on the latent pore former and the pore former in an amount of 0.02 to 15% by weight, based on the dry weight of the mineral expanded foam.
7. Mineral expanded foam according to claims 1 to 6, characterized in that The mineral expanded foam is based on gypsum to an extent of 0.1 to 20% by weight, based on the dry weight of the mineral expanded foam.
8. Mineral expanded foam according to claims 1 to 7, characterized in that The mineral expanded foam is based on quick-setting cement to an extent of 0.5 to 40% by weight, based on the dry weight of all cement present, The fast-setting cement is selected from the group consisting of aluminate cement, calcium sulfoaluminate cement and high alumina cement.
9. Mineral expanded foam according to claims 1 to 8, characterized in that As foam stabilizer there is One or more surfactants selected from the group consisting of olefin sulfonic acid; fatty acid or its salt; fatty alcohol; alkylphenol or hydroxyalkylphenol; alkyl and alkyl aryl ether sulfates; alkyl sulfonates, alkyl aryl sulfonates; esters or monoesters of sulfosuccinic acid; metaphosphates; alkyl polyglycol ethers; alkylaryl polyglycol ethers; ethylene oxide / propylene oxide (EO / PO) block copolymers; N-methyl taurate; fatty acid alkylolamides; amine oxides; or phosphine oxides; sodium cocoyl dimethylaminoacetate; sulfobetaine and phosphate esters; or One or more polymers selected from the group comprising: polyvinyl alcohol; polyvinyl acetal; polyvinyl pyrrolidone; water-soluble forms of polysaccharides; lignin sulfonates; poly(meth)acrylic acid; copolymers of (meth)acrylates with carboxyl-functionalized comonomer units; poly(meth)acrylamide; polyvinyl sulfonic acid and water-soluble copolymers thereof; melamine-formaldehyde sulfonates; naphthalene-formaldehyde sulfonates; styrene-maleic acid copolymers; and vinyl ether-maleic acid copolymers; or One or more proteins selected from the group consisting of: casein, caseinate, soy protein; gelatin; and other proteins obtainable by proteolysis of animal protein; or Enzymes of biotechnological origin.
10. Mineral expanded foam according to claims 1 to 9, characterized in that The mineral expanded foam is based on polymers of ethylenically unsaturated monomers stabilized by protective colloids to an extent of 0.5 to 40% by weight, based on the dry weight of the mineral expanded foam.
11. Mineral expanded foam according to claims 1 to 10, characterized in that The polymer of ethylenically unsaturated monomers is based on one or more monomers selected from the group consisting of vinyl esters, (meth)acrylates, vinyl aromatic compounds, olefins, 1,3-dienes and vinyl halides.
12. Mineral expanded foam according to claims 1 to 11, characterized in that The mineral expanded foam does not contain any fillers.
13. Mineral expanded foam according to claims 1 to 12, characterized in that The mineral expanded foam comprises from 0.01% to 5% by weight, based on the dry weight of the mineral expanded foam, of one or more hydrophobizing agents selected from the group comprising fatty acids and derivatives thereof, waxes and organosilicon compounds.
14. A method for producing mineral expanded foam, Wherein a dry mixture is produced by mixing: one or more foam stabilizers, one or more pore formers selected from the group comprising ammonium or alkali metal salts of bicarbonates or carbonates, optionally one or more fillers and optionally one or more additives, and The dry mixture thus obtained is mixed with water and is characterized in that a polymer of one or more ethylenically unsaturated monomers stabilized by a protective colloid in the form of a water-redispersible powder, one or more potential pore formers selected from the group consisting of aluminum and silicon and their alloys and calcium carbide, and 30 to 95% by weight of cement, based on the dry weight of the mineral expanded foam, is additionally introduced into the dry mixture, Provided that the dry mixture is based on the latent pore former to an extent of ≥ 10% by weight, based on the total weight of the pore former and the latent pore former.
15. A method for filling a cavity, in particular when installing a window or a door, characterized in that The cavity is filled with a mineral expanded foam according to claims 1 to 13 .
Citation Information
Patent Citations
Preparation method of foamed concrete thermal insulation board
CN108484211A
Foamed concrete heat insulation board
CN108529940A
Fiber-containing mortar composition
DE102008043988A1
Pore-building in cement - using gas producing material coated with inactive layer to delay gas formation when components are initially mixed
DE4009967A1
Building material mixture for foam mortar as well as methods for the production of foam mortar and uses of the building material mixture
DE4209897C1
Cited By
Preparation method of bicarbonate dispersed silica fume cement-based material
CN120794689A
Stable foam control agent having rapid dispersion ability
WO2026143911A1