Nonaqueous electrolyte secondary battery
By forming a layer structure containing Me and W on the surface of the lithium transition metal composite oxide of the non-aqueous electrolyte secondary battery and using a cellulose derivative, the instability of the layered structure of the lithium transition metal composite oxide and the reduction of the battery capacity are solved problem, achieving high capacity and excellent charge-discharge cycle characteristics and load characteristics.
Patent Information
- Application Number
- CN202380026593.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-18
- Filing Date
- 2023-03-03
- Publication Date
- 2024-10-29
AI Technical Summary
Existing non-aqueous electrolyte secondary batteries have deficiencies in charge-discharge cycle characteristics and load characteristics, especially the instability of the layered structure of lithium transition metal composite oxides and reduced battery capacity, and they fail to effectively balance high capacity. and charge-discharge cycle characteristics.
A lithium transition metal composite oxide containing more than 80 mol% Ni is used as the positive electrode active material, and a layer structure containing Me and W is formed on its surface. Secondary particles are formed by agglomeration of primary particles, and cellulose derivatives are used to improve load characteristics and Charge and discharge cycle characteristics.
Significantly improve the battery capacity, charge and discharge cycle characteristics and load characteristics, ensuring the high capacity and stability of the battery.
Smart Images

Figure CN118872090A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a non-aqueous electrolyte secondary battery. Background Art
[0002] In the past, as a high-output, high-capacity secondary battery, a non-aqueous electrolyte secondary battery having a positive electrode, a negative electrode, and a non-aqueous electrolyte, and charging and discharging by moving Li ions between the positive electrode and the negative electrode, was widely used. As a positive electrode active material of a non-aqueous electrolyte secondary battery, a lithium transition metal composite oxide containing transition metals such as nickel, cobalt, and manganese is generally used. In Patent Document 1, in order to suppress the reaction between the lithium transition metal composite oxide and the non-aqueous electrolyte, a technology of covering a predetermined metal oxide on the surface of the lithium transition metal composite oxide is disclosed.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2003-173775 Summary of the invention
[0006] In recent years, the use of non-aqueous electrolyte secondary batteries has been expanded to power supplies for electric vehicles, etc. In these uses, in order to shorten the charging time, the improvement of load characteristics is required. In addition, in order to obtain high discharge capacity, it is possible to consider increasing the design of the content of Ni in the lithium transition metal composite oxide as a positive electrode active material. However, when the ratio of Ni is more than 80 mol% relative to the total molar number of the metal elements other than Li, the layered structure of the lithium transition metal composite oxide becomes unstable, and there is a situation where the battery capacity is reduced along with the charge and discharge cycle. The technology recorded in patent document 1 does not consider the balance between the charge and discharge cycle characteristics and the load characteristics of the high-capacity battery, and there is still room for improvement.
[0007] An object of the present invention is to provide a nonaqueous electrolyte secondary battery having a high capacity and excellent charge-discharge cycle characteristics and load characteristics.
[0008] A nonaqueous electrolyte secondary battery as one embodiment of the present invention is characterized in that it comprises a positive electrode, a negative electrode and a nonaqueous electrolyte, the positive electrode comprising a positive electrode collector and a positive electrode mixture layer formed on the surface of the positive electrode collector, the positive electrode mixture layer comprising a positive electrode active material and a cellulose derivative, the positive electrode active material comprising a lithium transition metal composite oxide containing 80 mol % or more of Ni relative to the total molar number of metal elements excluding Li, the lithium transition metal composite oxide comprising secondary particles formed by agglomeration of primary particles, a Me-containing layer containing a metal element Me (Me is at least one element selected from Nb, Sr, Mo and Ca) and a W-containing layer containing W are formed on the surface of the primary particles, the content of Me in the Me-containing layer is 0.005 mol % to 1 mol % relative to the total molar number of metal elements excluding Li in the lithium transition metal composite oxide, and the W-containing layer covers at least a portion of the Me-containing layer.
[0009] According to the nonaqueous electrolyte secondary battery which is one embodiment of the present invention, the battery capacity, the charge and discharge cycle characteristics, and the load characteristics can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 This is an axial cross-sectional view of a cylindrical secondary battery as an example of an embodiment. DETAILED DESCRIPTION
[0011] Hereinafter, an example of an embodiment of a cylindrical secondary battery of the present invention will be described in detail with reference to the accompanying drawings. In the following description, specific shapes, materials, numerical values, directions, etc. are examples for facilitating the understanding of the present invention and can be appropriately changed to match the specifications of the secondary battery. In addition, the following example illustrates a cylindrical secondary battery in which a wound electrode body is housed in a cylindrical outer packaging body, but the electrode body is not limited to a wound type, and may also be a stacked type in which a plurality of positive electrodes and a plurality of negative electrodes are alternately stacked one by one with a separator. The outer packaging body is not limited to a cylindrical shape, and may be, for example, a square shape, a button shape, etc. In addition, the outer packaging body may also be a bag-type composed of a laminated sheet comprising a metal layer and a resin layer. In addition, in this specification, a record such as "value (A) to value (B)" means above value (A) and below value (B).
[0012] Figure 1 1 is an axial cross-sectional view of a cylindrical secondary battery 10 as an example of an embodiment. Figure 1 The secondary battery 10 shown contains an electrode body 14 and a non-aqueous electrolyte (not shown) in an outer package 15. The electrode body 14 has a wound structure in which a positive electrode 11 and a negative electrode 12 are wound with a separator 13 interposed therebetween. It should be noted that, in the following, for the convenience of description, the sealing body 16 side is set as "upper" and the bottom side of the outer package 15 is set as "lower".
[0013] The open end of the upper part of the outer packaging body 15 is sealed by the sealing body 16, thereby sealing the interior of the secondary battery 10. Insulating plates 17 and 18 are provided above and below the electrode body 14, respectively. The positive lead 19 extends upward after passing through the through hole of the insulating plate 17, and is welded to the lower surface of the filter 22 serving as the bottom plate of the sealing body 16. In the secondary battery 10, the cap 26 serving as the top plate of the sealing body 16 electrically connected to the filter 22 becomes the positive terminal. On the other hand, the negative lead 20 passes through the outside of the insulating plate 18 and extends to the bottom side of the outer packaging body 15, and is welded to the bottom inner surface of the outer packaging body 15. In the secondary battery 10, the outer packaging body 15 becomes the negative terminal.
[0014] The outer package 15 is, for example, a metal outer package can in a cylindrical shape with a bottom. A gasket 27 is provided between the outer package 15 and the sealing body 16 to ensure the airtightness of the interior of the secondary battery 10. The outer package 15 has, for example, a groove 21 formed by punching a side surface from the outside. The groove 21 is preferably formed in an annular shape along the circumferential direction of the outer package 15, and the sealing body 16 is supported by the upper surface thereof with the gasket 27 interposed therebetween.
[0015] The sealing body 16 has a filter 22, a lower valve body 23, an insulating member 24, an upper valve body 25 and a cap 26 stacked in sequence from the electrode body 14 side. The components constituting the sealing body 16 have, for example, a disc shape or a ring shape, and the components except the insulating member 24 are electrically connected to each other. The lower valve body 23 and the upper valve body 25 are connected to each other at their respective central portions, and an insulating member 24 is sandwiched between their respective peripheral portions. When the internal pressure of the battery increases due to abnormal heat, for example, the lower valve body 23 breaks, whereby the upper valve body 25 bulges toward the cap 26 side and detaches from the lower valve body 23, thereby blocking the electrical connection between the two. When the internal pressure increases further, the upper valve body 25 breaks, and gas is discharged from the opening of the cap 26.
[0016] Hereinafter, the positive electrode 11 , the negative electrode 12 , the separator 13 , and the nonaqueous electrolyte constituting the secondary battery 10 , particularly the positive electrode 11 , will be described in detail.
[0017] [positive electrode]
[0018] The positive electrode 11 has a positive electrode current collector and a positive electrode mixture layer formed on the surface of the positive electrode current collector. The positive electrode mixture layer is preferably formed on both sides of the positive electrode current collector. The positive electrode current collector can be made of a foil of a metal such as aluminum or an aluminum alloy that is stable in the potential range of the positive electrode 11, or a film having the metal disposed on the surface.
[0019] The positive electrode mixture layer contains a positive electrode active material and a cellulose derivative. The content of the positive electrode active material in the positive electrode mixture layer is, for example, 80% to 99% by mass relative to the total mass of the positive electrode mixture layer. The active material density in the positive electrode mixture layer is, for example, 3.30 g / cm 3~3.64g / cm 3 For example, the positive electrode 11 can be produced by applying a positive electrode mixture slurry containing a positive electrode active material, a cellulose derivative, etc., on the surface of a positive electrode current collector, drying the coating, and then rolling the coating using a roller or the like.
[0020] By making the positive electrode mixture layer contain a cellulose derivative, the load characteristics are improved. It is speculated that this is because the conductivity of Li ions in the positive electrode mixture layer is improved by intercalating a cellulose derivative. As cellulose derivatives contained in the positive electrode mixture layer, for example, carboxymethyl cellulose and its salts, methyl cellulose and its salts can be cited. As a cellulose derivative, from the aspect of suppressing the increase in the viscosity of the positive electrode mixture slurry, it is preferred to contain methyl cellulose, and it is particularly preferred to contain methyl cellulose with a weight average molecular weight of 10,000 to 150,000.
[0021] The content of the cellulose derivative in the positive electrode mixture layer is preferably 0.005% to 0.5% by mass, more preferably 0.01% to 0.1% by mass, relative to the total mass of the positive electrode active material. If the content of the cellulose derivative is within this range, the charge-discharge cycle characteristics and load characteristics can be improved while suppressing the reduction of the battery capacity.
[0022] The positive electrode active material contained in the positive electrode mixture layer contains a lithium transition metal composite oxide, which contains more than 80 mol% of Ni relative to the total molar number of metal elements other than Li. Thus, the high capacity of the battery can be achieved. The lithium transition metal composite oxide can have, for example, a layered structure belonging to the space group R-3m, a layered structure belonging to the space group C2 / m, etc. Among them, from the perspectives of high capacity, stability of the crystal structure, etc., a layered structure belonging to the space group R-3m is preferred. The layered structure of the lithium transition metal composite oxide may include a transition metal layer, a Li layer, and an oxygen layer.
[0023] Lithium transition metal composite oxides such as Li a Ni b Co 1-b-c X c O d (wherein, 0.9≤a≤1.25, 0.80≤b≤0.96, 0≤c≤0.20, 1.9≤d≤2.1, and X is at least one element selected from Mn and Al). The molar fraction of the metal element contained in the lithium transition metal composite oxide can be measured by inductively coupled plasma (ICP) emission spectrometry.
[0024] The lithium transition metal composite oxide has secondary particles formed by the aggregation of primary particles. The secondary particles are particles whose volume-based median particle size (D50) is preferably 3μm to 30μm, more preferably 5μm to 25μm, and particularly preferably 7μm to 15μm. D50 means the particle size at which the cumulative frequency reaches 50% from the smaller particle size in the volume-based particle size distribution, also known as the median diameter. The particle size distribution of the secondary particles of the lithium transition metal composite oxide can be measured using a laser diffraction particle size distribution measuring device (e.g., MT3000II manufactured by MicrotracBEL Co., Ltd.) using water as a dispersion medium. The particle size of the primary particles constituting the secondary particles is, for example, 0.05μm to 1μm. The particle size of the primary particles is measured as the diameter of the circumscribed circle in the particle image observed using a scanning electron microscope (SEM).
[0025] On the surface of the primary particle, a Me-containing layer containing Me (Me is at least one element selected from Nb, Sr, Mo and Ca) and a W-containing layer containing W are formed, and the W-containing layer covers at least a portion of the Me-containing layer. By covering the Me-containing layer with the W-containing layer, the charge-discharge cycle characteristics and the load characteristics are improved. It can be inferred that the W-containing layer protects the Me-containing layer from the influence of the non-aqueous electrolyte, thereby improving the charge-discharge cycle characteristics and the load characteristics. The so-called Me-containing layer and the W-containing layer are formed on the surface of the primary particle, which means that the Me-containing layer and the W-containing layer are respectively present on the surface of the secondary particle, or at the interface between the primary particles. The Me-containing layer may exist in a dotted manner in a manner covering at least a portion of the surface of the primary particle, or may exist in a manner covering the entirety of the primary particle. The W-containing layer covers a portion or all of the Me-containing layer, or a portion of the W-containing layer may cover the surface of the primary particle. The Me-containing layer, for example, contains an oxide of Me. The W-containing layer, for example, contains WO3.
[0026] The content of Me in the Me-containing layer is 0.005 mol% to 1 mol% relative to the total molar number of metal elements other than Li in the lithium transition metal composite oxide. If the content of Me is out of this range, both the charge-discharge cycle characteristics and the load characteristics cannot be achieved. The content of Me is more preferably 0.01 mol% to 0.5 mol%.
[0027] The content of W in the W-containing layer is preferably 0.2 mol% or less relative to the total molar number of metal elements other than Li in the lithium transition metal composite oxide. If the content of W is greater than 0.2 mol%, the battery capacity may be reduced. The lower limit of the content of W is, for example, 0.01 mol%, or may be 0.06 mol%.
[0028] The presence of the Me-containing layer on the surface of the lithium transition metal composite oxide can be confirmed by energy dispersive X-ray spectroscopy (TEM-EDX). In addition, the contents of Sr, Ca and W in the surface modification layer can be measured by inductively coupled plasma (ICP) emission spectrometry.
[0029] Next, an example of a method for producing a positive electrode active material according to the present embodiment will be described. The method for producing a positive electrode active material includes, for example, a synthesis step, a washing step, and an addition step.
[0030] In the synthesis step, for example, a metal oxide containing Ni, a Li compound, and a Me compound are mixed and calcined to obtain a lithium transition metal composite oxide having a Me-containing layer formed thereon.
[0031] The metal oxide can be obtained, for example, by stirring a solution of a metal salt containing Ni and any metal element (Co, Al, Mn, etc.), dropping an alkaline solution such as sodium hydroxide, adjusting the pH to the alkaline side (e.g., 8.5 to 12.5), thereby precipitating (coprecipitating) a composite hydroxide containing Ni and any metal element, and heat-treating the composite hydroxide. The heat treatment temperature is not particularly limited, for example, in the range of 300°C to 600°C.
[0032] Examples of Li compounds include Li2CO3, LiOH, Li2O2, Li2O, LiNO3, LiNO2, Li2SO4, LiOH·H2O, LiH, and LiF. Examples of Me compounds include hydroxides, oxides, carbonates, sulfates, nitrates, and chlorides containing Me.
[0033] Regarding the mixing ratio of the metal oxide, the Li compound and the Me compound, from the aspect of facilitating the adjustment of the above parameters to the above-mentioned prescribed ranges, for example, it is preferably set to a ratio in the range of 1: (0.9 to 1.2): (0.00005 to 0.005) of the molar ratio of the metal element other than Li: Li: Me. It should be noted that when mixing the metal oxide, the Li compound, etc., other metal raw materials may be added as needed. Here, the so-called other metal raw materials are oxides of metal elements other than Me and metal elements constituting the metal oxide.
[0034] The mixture of the metal oxide and the Li compound is calcined, for example, in an oxygen atmosphere. Regarding the calcination conditions, for example, the heating rate at 450°C to 650°C is in the range of 1.0°C / min to 5.5°C / min, and the heating rate from 650°C to the maximum reached temperature is, for example, 0.1°C / min to 3.5°C / min. The maximum reached temperature can be in the range of 700°C to 800°C. In addition, the holding time of the maximum reached temperature can be more than 1 hour and less than 10 hours. A Me-containing layer is formed on the surface of the primary particles of the lithium transition metal composite oxide after the synthesis step.
[0035] In the washing step, first, the lithium transition metal composite oxide obtained in the synthesis step is washed with water and dehydrated to obtain a cake-like composition. The washing and dehydration can be performed using known methods and conditions. Thereafter, the cake-like composition is dried to obtain a powdery composition. The drying conditions are, for example, drying in a vacuum atmosphere at 150° C. to 400° C. for 0.5 to 15 hours.
[0036] In the adding process, a W-containing compound or a W-containing solution is added to the lithium transition metal composite oxide after the cleaning process to obtain a positive electrode active material. The W compound is added to the lithium transition metal composite oxide wetted by adding water, for example. Li compounds remain in the lithium transition metal composite oxide after the cleaning process, and the residual Li compounds dissolve in water to form an alkaline aqueous solution. The W compound dissolves in the alkaline aqueous solution and spreads to the entire surface of the calcined product. As W compounds, tungsten oxide (WO3), lithium tungstate (Li2WO4, Li4WO5, Li6W2O9) and the like can be exemplified. The amount of W added can be 0.01 mol% to 0.2 mol% relative to the total molar number of metal elements other than Li in the lithium transition metal composite oxide. In addition, when a W-containing solution is added to the lithium transition metal composite oxide, the W concentration in the W-containing solution is, for example, 0.05 mol / L or more, preferably 0.1 mol / L to 1 mol / L. The W-containing solution is not particularly limited as long as it contains W, but is preferably a solution obtained by dissolving a W compound that is easily soluble in an alkaline solution, such as tungsten oxide, lithium tungstate, or ammonium tungstate, in an aqueous solution of lithium hydroxide.
[0037] By adding a W-containing compound or a W solution as described above and heat-treating the lithium transition metal composite oxide, a positive electrode active material is produced. The heat treatment conditions are not particularly limited, and for example, the heat treatment temperature can be set to 150° C. to 400° C. and the heat treatment time can be set to 0.5 hours to 15 hours in a vacuum atmosphere. Thus, a Me-containing layer can be formed on the primary particle surface of the lithium transition metal composite oxide, and a W-containing layer can be further formed on the Me-containing layer.
[0038] The molar fraction of the metal element contained in the positive electrode active material obtained by the above operation is measured by inductively coupled plasma emission spectrometry (ICP), and can be expressed as: a Ni b Co 1-b-c X c Me s W t O d (wherein, 0.9≤a≤1.25, 0.80≤b≤0.96, 0≤c≤0.20, 1.9≤d≤2.1, 0.00005≤s≤0.005, 0.0001≤t≤0.002, X is at least one element selected from Mn and Al, and Me is at least one element selected from Nb, Sr, Mo and Ca). It should be noted that a portion of Me and W can be dissolved in the lithium transition metal composite oxide.
[0039] The positive electrode active material may include other lithium transition metal composite oxides in addition to the lithium transition metal composite oxide of this embodiment. Examples of other lithium transition metal composite oxides include lithium transition metal composite oxides having a Ni content of 0 mol % or more and less than 80 mol %.
[0040] The positive electrode mixture layer may further include a conductive agent. As the conductive agent contained in the positive electrode mixture layer, for example, carbon black (CB), acetylene black (AB), Ketjen black, carbon nanotubes (CNT), graphene, graphite and other carbon particles can be cited. They can be used alone or in combination of two or more.
[0041] The positive electrode mixture layer may further include a binder. As the binder contained in the positive electrode mixture layer, for example, fluorine resins such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyimide resins, acrylic resins, polyolefin resins, polyacrylonitrile (PAN) etc. may be cited. They may be used alone or in combination of two or more.
[0042] [negative electrode]
[0043] The negative electrode 12 includes, for example, a negative electrode current collector and a negative electrode mixture layer formed on the surface of the negative electrode current collector. The negative electrode mixture layer is preferably formed on both sides of the negative electrode current collector. The negative electrode current collector can be made of a foil of a metal such as copper that is stable in the potential range of the negative electrode, or a film having the metal disposed on the surface.
[0044] The negative electrode mixture layer contains, for example, a negative electrode active material and a binder. The content of the negative electrode active material in the negative electrode mixture layer is, for example, 80% by mass to 99% by mass relative to the total mass of the negative electrode mixture layer. For example, a negative electrode mixture slurry containing a negative electrode active material, a binder, etc. is coated on the surface of the negative electrode current collector, and after the coating film is dried, the coating film is calendered using a roller or the like, whereby the negative electrode 12 can be manufactured.
[0045] As the negative electrode active material contained in the negative electrode mixture layer, there is no particular limitation as long as it is a material capable of reversibly occluding and releasing Li ions, and carbon materials such as graphite are usually used. The graphite can be any of natural graphite such as flake graphite, massive graphite, and earthy graphite, massive artificial graphite, graphitized mesophase carbon microspheres, etc. artificial graphite. In addition, metals alloyed with Li such as Si and Sn, metal compounds containing Si and Sn, lithium titanium composite oxides, etc. can also be used as the negative electrode active material. For example, silicon oxides represented by SiO x (x is 0.5 to 1.6), lithium silicate phases represented by Li 2y SiO (2+y) (0 < y < 2) containing silicon-containing materials in which fine particles of Si are dispersed, silicon-containing materials in which fine particles of Si are dispersed in a carbon phase, etc. can be used in combination with graphite.
[0046] As the binder contained in the negative electrode mixture layer, for example, styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber (NBR), carboxymethyl cellulose (CMC) or its salts (CMC-Na, CMC-K, CMC-NH4, etc., and partial neutralization salts can also be used), polyacrylic acid (PAA) or its salts (PAA-Na, PAA-K, etc., and partial neutralization salts can also be used), polyvinyl alcohol (PVA), etc. can be cited. They can be used alone or in combination of two or more.
[0047] [Separator]
[0048] The separator 13 uses, for example, a porous sheet having ion permeability and insulation. Specific examples of the porous sheet include microporous films, woven fabrics, non-woven fabrics, etc. As the material of the separator, olefin-based resins such as polyethylene and polypropylene, cellulose, etc. are suitable. The separator 13 can be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin-based resin. In addition, it can also be a multi-layer separator containing a polyethylene layer and a polypropylene layer, and a separator having an aromatic polyamide-based resin, ceramics, etc. coated on the surface of the separator 13 can be used.
[0049] [Non-aqueous electrolyte]
[0050] A non-aqueous electrolyte is a liquid electrolyte (electrolyte solution) containing a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. As the non-aqueous solvent, for example, esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and a mixed solvent of two or more thereof can be used. The non-aqueous solvent may also contain a halogen-substituted product in which at least a part of the hydrogen of these solvents is substituted with a halogen atom such as fluorine.
[0051] Examples of the above esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, cyclic carboxylic acid esters such as γ-butyrolactone, γ-valerolactone, and chain carboxylic acid esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), ethyl propionate, etc.
[0052] Examples of the above ethers include cyclic ethers such as 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-epoxybutane, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, crown ether, and chain ethers such as 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, etc.
[0053] As the above halogen-substituted product, fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, fluorinated chain carboxylic acid esters such as fluoromethyl propionate (FMP), etc. are preferably used.
[0054] The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiBF4, LiClO4, LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiCF3SO3, LiCF3CO2, Li(P(C2O4)F4), LiPF 6-x (CnF 2n+1 ) x (1 < x < 6, n is 1 or 2), LiB 10 Cl 10, LiCl, LiBr, LiI, lithium chloroborane, lower aliphatic carboxylic acid lithium, Li2B4O7, Li(B(C2O4)F2) and other borates, LiN(SO2CF3)2, LiN(C1F 21+1 SO2)(C m F 2m+1 SO2) {l, m is an integer greater than 1} and other imide salts. The lithium salt may be used alone or in combination. Among them, LiPF6 is preferably used from the viewpoint of ion conductivity, electrochemical stability, etc. The concentration of the lithium salt is preferably set to 0.8 to 1.8 mol per 1 L of solvent.
[0055] Example
[0056] Hereinafter, the present invention will be further described using Examples and Comparative Examples; however, the present invention is not limited to the following Examples.
[0057] [Preparation of positive electrode active material]
[0058] <Example 1>
[0059] The [Ni 0.91 Co 0.04 Al 0.05 The composite hydroxide represented by ](OH)2 was calcined at 500°C for 8 hours to obtain a composite oxide (Ni 0.91 Co 0.04 Al 0.05 Then, LiOH, the composite oxide and Nb2O5 as a Me compound were mixed to obtain a mixture such that the molar ratio of Li, Ni, Co and Al to Nb was 1.03:1:0.0001. The mixture was heated under an oxygen flow with an oxygen concentration of 95% (per 10 cm 3 2mL / min in the mixture and 5L / min per 1kg of the mixture), calcined from room temperature to 650°C at a heating rate of 2.0°C / min, and then calcined from 650°C to 760°C at a heating rate of 0.5°C / min, washed with water, and dried to produce a lithium transition metal composite oxide having a Me-containing layer formed on the surface of the primary particles. After adding water to the lithium transition metal composite oxide to make it wet, WO3 was added, and heat treated at 300°C for 8 hours to obtain the positive electrode active material of Example 1. At this time, WO3 was added so that W was 0.06 mol% relative to the total molar number of metal elements other than Li in the lithium transition metal composite oxide. The analysis result based on the ICP emission spectrophotometer (manufactured by Thermo Fisher Scientific, trade name "iCAP6300") showed that the composition of the positive electrode active material was LiNi 0.91Co 0.04 Al 0.05 Nb 0.0001 W 0.0006 O2.
[0060] [Production of positive electrode]
[0061] 95 parts by mass of positive electrode active material, 3 parts by mass of acetylene black and 2 parts by mass of polyvinylidene fluoride (PVDF) are mixed. Methyl cellulose (weight average molecular weight 50,000) is added to the mixture at 0.01% by mass relative to the mass of the positive electrode active material, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) is added to prepare a positive electrode mixture slurry. Then, the positive electrode mixture slurry is applied to both sides of a strip-shaped positive electrode collector made of aluminum foil, and after drying, it is rolled and cut into a specified electrode plate size to produce a positive electrode with a positive electrode mixture layer formed on both sides of the positive electrode collector. In the approximate central part of the longitudinal direction of the positive electrode, a positive electrode exposure portion is provided where there is no mixture layer and the surface of the collector is exposed, and an aluminum positive electrode lead is welded to the positive electrode exposure portion. The active material density of the positive electrode mixture layer is 3.60 g / cm 3 .
[0062] [Production of negative electrode]
[0063] A mixture of 99 parts by mass of artificial graphite and 1 part by mass of silicon oxide (SiO) is used as a negative electrode active material. 100 parts by mass of the mixture, 1 part by mass of carboxymethyl cellulose (CMC) and 1 part by mass of styrene butadiene rubber (SBR) are mixed, and an appropriate amount of water is added to prepare a negative electrode mixture slurry. Then, the negative electrode mixture slurry is applied to both sides of a strip-shaped negative electrode collector made of copper foil, and after drying, it is rolled and cut into a specified plate size to produce a negative electrode with a negative electrode mixture layer formed on both sides of the negative electrode collector. At the outer end of the winding of the negative electrode, a negative electrode exposed portion where there is no mixture layer and the surface of the collector is exposed is provided, and a negative electrode lead made of nickel is welded to the negative electrode exposed portion.
[0064] [Preparation of electrolyte]
[0065] 2 parts by mass of vinylene carbonate (VC) were added to 100 parts by mass of a mixed solvent containing ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) (EC:EMC:DMC=2:2:6 by volume ratio). LiPF6 was dissolved in the mixed solvent to a concentration of 1.0 mol / L to prepare an electrolyte.
[0066] [Preparation of test battery]
[0067] An aluminum lead was installed on the exposed portion of the positive electrode containing the positive electrode active material of Example 1, and a nickel lead was installed on the exposed portion of the negative electrode, and the positive electrode and the negative electrode were wound into a spiral shape with a polyolefin separator interposed therebetween to produce a wound electrode body. The electrode body was housed in an outer package, the nonaqueous electrolyte was injected, and the opening of the outer package was sealed to obtain a test battery.
[0068] [Evaluation of Capacity Retention Rate]
[0069] At an ambient temperature of 25°C, the test battery was charged at a constant current of 0.3C until the battery voltage reached 4.2V, and further charged at a constant voltage of 4.2V until the current value reached 0.02C. Thereafter, the battery was discharged at a constant current of 0.3C until the battery voltage reached 2.5V. This charge and discharge was set as 1 cycle, and 300 cycles were performed. The capacity retention rate of the test battery was calculated using the following formula to evaluate the charge and discharge cycle characteristics.
[0070] Capacity retention rate (%) = (discharge capacity at the 300th cycle / discharge capacity at the 1st cycle) × 100
[0071] [Evaluation of load characteristics]
[0072] Under a temperature environment of 25°C, the above test battery was charged at a constant current of 0.3C until the battery voltage reached 4.2V, and further charged at a constant voltage of 4.2V until the current value reached 0.02C. Thereafter, the battery was discharged at a constant current of 0.1C until the battery voltage reached 2.5V, and the 0.1C discharge capacity was measured. Then, the battery was charged under the same conditions as above, and then discharged at a constant current of 2C until the battery voltage reached 2.5V, and the 2C discharge capacity was measured. The load characteristics were calculated using the following formula.
[0073] Load characteristics (%) = (2C discharge capacity ÷ 0.1C discharge capacity) × 100
[0074] <Examples 2 to 10, Comparative Examples 1 to 11>
[0075] A test cell was obtained and evaluated in the same manner as in Example 1 except that the type and amount of the Me compound added in the preparation of the positive electrode active material, the amount of WO3 added, and the amount of methylcellulose added in the preparation of the positive electrode were changed as shown in Table 1.
[0076] <Comparative Example 12>
[0077] A test cell was obtained and evaluated in the same manner as in Example 1 except that WO 3 was mixed with LiOH, the above composite oxide and the Me compound instead of adding WO 3 to the lithium transition metal composite oxide in the preparation of the positive electrode active material.
[0078] <Example 11>
[0079] In the preparation of the positive electrode active material, the composition of the composite hydroxide prepared by the coprecipitation method was changed to obtain a Ni 0.85 Co 0.10 Al 0.05 A test cell was obtained and evaluated in the same manner as in Example 2 except that the composite oxide represented by O2 was used.
[0080] <Comparative Examples 13 to 17>
[0081] A test cell was obtained and evaluated in the same manner as in Example 11 except that the addition amount of Nb2O5 in the preparation of the positive electrode active material, the addition amount of WO3, and the addition amount of methyl cellulose in the preparation of the positive electrode were changed as shown in Table 1.
[0082] <Example 12>
[0083] In the preparation of the positive electrode active material, the composition of the composite hydroxide prepared by the coprecipitation method was changed to obtain a Ni 0.85 Co 0.10 Al 0.05 A test cell was obtained and evaluated in the same manner as in Example 2 except that the composite oxide represented by O2 was used.
[0084] <Comparative Examples 18 to 22>
[0085] A test cell was obtained and evaluated in the same manner as in Example 12 except that the addition amount of Nb2O5 in the preparation of the positive electrode active material, the addition amount of WO3, and the addition amount of methyl cellulose in the preparation of the positive electrode were changed as shown in Table 1.
[0086] The evaluation results of the test batteries of the examples and comparative examples are shown in Tables 1 to 3. The capacity retention rates and load characteristics of the test batteries of Examples 1 to 10 and Comparative Examples 2 to 12 shown in Table 1 are values expressed relative to the capacity retention rate and load characteristics of the test battery of Comparative Example 1 as 100. The capacity retention rates and load characteristics of the test batteries of Example 11 and Comparative Examples 14 to 17 shown in Table 2 are values expressed relative to the capacity retention rate and load characteristics of the test battery of Comparative Example 13 as 100. The capacity retention rates and load characteristics of the test batteries of Example 12 and Comparative Examples 19 to 22 shown in Table 3 are values expressed relative to the capacity retention rate and load characteristics of the test battery of Comparative Example 18 as 100. It should be noted that "-" in the column "Presence or absence of W on the surface of Me" in Tables 1 to 3 means that Me or W does not exist. In addition, "-" other than the column "Presence or absence of W on the surface of Me" in Tables 1 to 3 means 0.
[0087] [Table 1]
[0088]
[0089] [Table 2]
[0090]
[0091] [Table 3]
[0092]
[0093] In any of Tables 1 to 3, the test battery of the embodiment has higher capacity retention and load characteristics than the test battery of the comparative example, and both the charge-discharge cycle characteristics and the load characteristics are excellent. Comparative Example 2 shows the results when methyl cellulose is contained in the positive electrode mixture layer, and there is no Me-containing layer and no W-containing layer on the surface of the primary particles of the lithium transition metal composite oxide. Comparative Example 3 shows the results when there is no Me-containing layer on the surface of the primary particles of the lithium transition metal composite oxide, but there is a W-containing layer, and the positive electrode mixture layer does not contain methyl cellulose. Comparative Example 5 shows the results when there is no W-containing layer on the surface of the primary particles of the lithium transition metal composite oxide, but there is a Me-containing layer, and the positive electrode mixture layer does not contain methyl cellulose. The capacity retention rate and load characteristics of the test battery of Example 2 are improved to a level greater than the sum of the respective effects of the cellulose derivative, the W-containing layer, and the Me-containing layer calculated according to Comparative Examples 2, 3, and 5, confirming an excellent synergistic effect.
[0094] Description of Reference Numerals
[0095] 10 secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 15 outer packaging body, 16 sealing body, 17, 18 insulating plates, 19 positive electrode lead, 20 negative electrode lead, 21 slotted portion, 22 filter, 23 lower valve body, 24 insulating member, 25 upper valve body, 26 cap, 27 gasket.
Claims
1. A non-aqueous electrolyte secondary battery, It has a positive electrode, a negative electrode and a non-aqueous electrolyte. The positive electrode comprises a positive electrode current collector and a positive electrode mixture layer formed on a surface of the positive electrode current collector. The positive electrode mixture layer comprises a positive electrode active material and a cellulose derivative. The positive electrode active material contains a lithium transition metal composite oxide containing 80 mol % or more of Ni based on the total molar number of metal elements excluding Li, The lithium transition metal composite oxide has secondary particles formed by agglomeration of primary particles. On the surface of the primary particle, a Me-containing layer containing Me and a W-containing layer containing W are formed, wherein: Me is at least one element selected from Nb, Sr, Mo and Ca, The content of Me in the Me-containing layer is 0.005 mol% to 1 mol% relative to the total molar number of metal elements excluding Li in the lithium transition metal composite oxide. The W-containing layer covers at least a portion of the Me-containing layer.
2. The nonaqueous electrolyte secondary battery according to claim 1, wherein The lithium transition metal composite oxide has the general formula Li a Ni b Co 1-b-c X c O d Represented by, wherein 0.9≤a≤1.25, 0.80≤b≤0.96, 0≤c≤0.20, 1.9≤d≤2.1, and X is at least one element selected from Mn and Al.
3. The nonaqueous electrolyte secondary battery according to claim 1 or 2, wherein: The content of W in the W-containing layer is 0.2 mol % or less based on the total number of moles of metal elements excluding Li in the lithium-transition metal composite oxide.
4. The nonaqueous electrolyte secondary battery according to any one of claims 1 to 3, wherein The content of the cellulose derivative in the positive electrode mixture layer is 0.005 mass % to 0.5 mass % based on the total mass of the positive electrode active material.
5. The nonaqueous electrolyte secondary battery according to any one of claims 1 to 4, wherein The cellulose derivative comprises methyl cellulose having a weight average molecular weight of 10,000 to 150,000.