Nonaqueous electrolyte and lithium secondary battery comprising same
By using non-aqueous electrolyte additives in lithium secondary batteries to form a polymer-type SEI coating, the problems of positive electrode degradation and negative electrode expansion under high temperatures and high voltages are solved, significantly improving the stability and life of the battery.
Patent Information
- Application Number
- CN202380024063.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-10-07
- Filing Date
- 2023-10-06
- Publication Date
- 2024-10-29
AI Technical Summary
Lithium secondary batteries are prone to problems such as positive electrode degradation, negative electrode expansion and SEI film passivation under high temperature and high voltage conditions, resulting in reduced battery stability and lifespan.
A non-aqueous electrolyte additive is used to form a uniform and dense polymer solid electrolyte (SEI) coating on the positive and negative electrodes to inhibit metal ion elution and SEI passivation, thereby improving the high-temperature cycle characteristics and storage performance of the battery.
It effectively prevents the deterioration of the positive and negative electrodes, improves the high-temperature durability and life characteristics of lithium secondary batteries, and enhances the overall performance of the battery.
Smart Images

Figure CN118872115A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of Korean Patent Application No. 10-2022-0129125 filed on October 7, 2022, in the Korean Intellectual Property Office, the contents of which are incorporated herein by reference. Technical Field
[0003] The present invention relates to a non-aqueous electrolyte and a lithium secondary battery including the same. Background Art
[0004] Recently, as the application fields of lithium secondary batteries in various application fields are expanding, demands for secondary batteries having high capacity, high output, and high stability are increasing.
[0005] In particular, in order to achieve a high capacity of a secondary battery, if the secondary battery is operated at a high voltage, the transition metal ions may be eluted from the surface of the positive electrode due to the degradation of the coating film formed on the positive / negative electrode surface or the degradation of the surface structure of the electrode due to the side reaction of the electrolyte degradation during the charging and discharging process. The transition metal ions eluted in this way may be electrodeposited on the negative electrode, and the passivation ability of the SEI may be reduced, thereby causing the defect of negative electrode degradation.
[0006] If the potential of the positive electrode increases, or the battery is exposed to high temperature, the deterioration phenomenon of the secondary battery tends to be further accelerated.
[0007] Furthermore, if a lithium secondary battery is continuously used for a long time or at a high temperature, gas may be generated to increase the thickness of the battery, thereby causing a so-called swelling phenomenon, and the amount of gas generated is known to depend on the state of SEI.
[0008] Therefore, in order to solve these defects, research is being conducted to develop a method for reducing the swelling phenomenon of secondary batteries and improving stability at high temperatures by suppressing the elution of metal ions at the positive electrode and forming a stable SEI film on the negative electrode. Summary of the invention
[0009] Technical issues
[0010] Based on studies conducted from various perspectives to solve these tasks, the present invention provides an additive for a non-aqueous electrolyte that can suppress degradation of a positive electrode, reduce side reactions between a positive electrode and an electrolyte, and form a uniform and dense SEI film on a negative electrode.
[0011] Furthermore, in the present invention, there is provided a nonaqueous electrolyte having improved high-temperature durability by containing the above-mentioned additive for a nonaqueous electrolyte.
[0012] Furthermore, in the present invention, there is provided a lithium secondary battery whose high temperature cycle characteristics and high temperature storage performance are improved by including the above-mentioned nonaqueous electrolyte, thereby having improved overall performance.
[0013] Technical Solution
[0014] To achieve the object, the present invention provides a non-aqueous electrolyte including an additive for a non-aqueous electrolyte represented by Formula 1.
[0015] [Formula 1]
[0016]
[0017] In Formula 1, R1 is one selected from the group consisting of H, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an aryl group having 6 to 8 carbon atoms, and R2 is one selected from the group consisting of an alkylene group having 1 to 10 carbon atoms and -OR3- (R3 is an alkylene group having 1 to 10 carbon atoms).
[0018] In addition, the present invention provides a lithium secondary battery, which includes: a positive electrode; a negative electrode; and the non-aqueous electrolyte.
[0019] Beneficial effects
[0020] The compound represented by Formula 1 provided as the additive for the non-aqueous electrolyte of the present invention can form a uniform and dense polymer-type solid electrolyte interphase (SEI) coating on the negative electrode. In particular, the glycolide matrix is substituted with propargyl groups, so that the ring-opening reaction of glycolide and the reductive decomposition of propargyl groups occur simultaneously, and a more solid polymer coating can be formed. In addition, if the positive electrode reaches a high potential, the additive of Formula 1 of the present invention can be decomposed at the positive electrode to form a positive electrode coating.
[0021] That is, if a non-aqueous electrolyte containing a compound represented by Formula 1 provided as an additive for a non-aqueous electrolyte of the present invention is included in a lithium secondary battery, the deterioration of the passivation ability of SEI at high temperatures can be suppressed, the degradation of the negative electrode can be prevented, and the life characteristics of the battery can be improved.
[0022] Furthermore, if exposed to a high potential, the compound represented by Formula 1 provided as the additive for the nonaqueous electrolyte of the present invention can form a coating film on the positive electrode and can prevent the degradation of the positive electrode.
[0023] Therefore, if the nonaqueous electrolyte including the compound of Formula 1 of the present invention is used, a stable electrode-electrolyte interface can be formed at high temperature, high temperature cycle characteristics and high temperature storage performance can be improved, and a lithium secondary battery with improved overall performance can be realized. DETAILED DESCRIPTION
[0024] It should be understood that the words or terms used in the present disclosure and claims should not be interpreted as the meanings defined in commonly used dictionaries. It should also be understood that based on the inventors can appropriately define the meanings of words or terms to best explain the principles of the present invention, the words or terms should be interpreted as having a meaning consistent with the technical ideas of the present invention.
[0025] It should also be understood that when used in this specification, the terms "comprising", "provided with" or "having" specify the presence of stated features, numbers, steps, elements or a combination thereof, but do not exclude the presence or addition of one or more other features, numbers, steps, elements or a combination thereof.
[0026] In addition, in the term "a to b carbon atoms" in the specification, "a" and "b" refer to the number of carbon atoms contained in a particular functional group. That is, the functional group may include "a" to "b" carbon atoms. For example, "alkylene having 1 to 5 carbon atoms" refers to an alkylene containing 1 to 5 carbon atoms, i.e., -CH2-, -CH2CH2-, -CH2CH2CH2-, -CH2(CH3)CH-, -CH(CH3)CH2- or -CH(CH3)CH2CH2-, etc.
[0027] In addition, in the specification, the alkyl group may be substituted or unsubstituted. Unless otherwise defined separately, "substituted" means that at least one or more hydrogens bonded to the carbon are replaced by elements other than hydrogen, for example, substituted by the following groups: alkyl groups having 1 to 20 carbon atoms, alkenyl groups having 2 to 20 carbon atoms, alkynyl groups having 2 to 20 carbon atoms, alkoxy groups having 1 to 20 carbon atoms, cycloalkyl groups having 3 to 12 carbon atoms, cycloalkenyl groups having 3 to 12 carbon atoms, heterocycloalkyl groups having 3 to 12 carbon atoms, heterocycloalkenyl groups having 3 to 12 carbon atoms, aryloxy groups having 6 to 12 carbon atoms, halogen atoms, fluoroalkyl groups having 1 to 20 carbon atoms, nitro groups, aryl groups having 6 to 20 carbon atoms, heteroaryl groups having 2 to 20 carbon atoms, or halogenated aryl groups having 6 to 20 carbon atoms, etc.
[0028] Hereinafter, the present invention will be explained in more detail.
[0029] Non-aqueous electrolytes
[0030] The nonaqueous electrolyte of the present invention includes, as an additive, a compound represented by Formula 1. A lithium secondary battery using the nonaqueous electrolyte including the additive of the present invention can suppress degradation caused by interface reaction at high temperatures and exhibit excellent high temperature cycle characteristics and high temperature storage performance.
[0031] [Formula 1]
[0032]
[0033] The compound of formula 1 can be decomposed and polymerized into a polymer type, and a uniform and dense polymer type coating can be formed on the surface of the negative electrode. The coating thus formed can prevent precipitation and plating caused by the elution of the transition metal at the positive electrode, and can improve the durability and life characteristics at high temperatures. In addition, if the lithium secondary battery is exposed to a high potential, the residue of the compound of formula 1 remaining after the coating is formed on the negative electrode can also form a coating on the positive electrode, and can prevent the degradation caused by the oxidative decomposition of the electrolyte at the positive electrode surface.
[0034] In Formula 1, R1 may be one selected from the group consisting of H, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an aryl group having 6 to 8 carbon atoms. Preferably, in Formula 1, R1 may be H or an alkyl group having 1 to 10 carbon atoms, and in this case, the substituent has a smaller volume and a denser coating film may be formed.
[0035] In Formula 2, R2 may be one selected from the group consisting of an alkylene group having 1 to 10 carbon atoms and -OR3- (R3 is an alkylene group having 1 to 10 carbon atoms), and preferably, R2 may be one selected from the group consisting of an alkylene group having 1 to 5 carbon atoms and -OR3- (R3 is an alkylene group having 1 to 5 carbon atoms).
[0036] Particularly, the compound of Formula 1 of the present invention may be one selected from Formulae 1a to 1d.
[0037] [Formula 1a]
[0038]
[0039] [Formula 1b]
[0040]
[0041] [Formula 1c]
[0042]
[0043] [Formula 1d]
[0044]
[0045] Based on 100 parts by weight of the non-aqueous electrolyte, the content of the non-aqueous electrolyte additive of the present invention may be 0.01 parts by weight to 5.0 parts by weight, preferably 0.1 parts by weight to 3.0 parts by weight, and more preferably 0.5 parts by weight to 1.0 parts by weight. If the above range is met, a sufficient amount of SEI can be formed, the viscosity of the electrolyte can be maintained at a suitable level, and excellent rate performance and capacity performance can be achieved during storage at high temperatures.
[0046] The lithium salt contained in the nonaqueous electrolyte of the present invention is used as an electrolyte salt in a lithium secondary battery and as a medium for transferring ions. Generally, the lithium salt includes, for example, Li + and as an anion at least one selected from the group consisting of: F - , Cl - Br - ,I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - , B 10 Cl 10 - 、AlCl4 - 、AlO2 - PF6 - CF3SO3 - 、CH3CO2 - CF3CO2 - 、AsF6 - 、SbF6 - 、CH3SO3 - 、(CF3CF2SO2)2N - 、(CF3SO2)2N - 、(FSO2)2N - 、BF2C2O4 - , BC4O8 - PF4C2O4 - PF2C4O8 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - 、C4F9SO3 - CF3CF2SO3 - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - CF3(CF2)7SO3- and SCN - .
[0047] In particular, the lithium salt may include a single material selected from the group consisting of LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10 , LiAlCl4, LiAlO2, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, lithium bis(fluorosulfonyl)imide (LiFSI; LiN(SO2F)2), lithium bis(perfluoroethanesulfonyl)imide (LiBETI; LiN(SO2CF2CF3)2) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI; LiN(SO2CF3)2), or a mixture of two or more thereof. In addition, lithium salts commonly used in electrolytes for lithium secondary batteries can be used without limitation.
[0048] The concentration of the lithium salt may be appropriately changed within a generally used range, but may be included in the electrolyte at a concentration of 0.5 M to 3 M, preferably 0.5 M to 2.5 M, more preferably 0.8 M to 2 M, to obtain the best formation effect of a coating film for preventing corrosion of the electrode surface. If the concentration of the lithium salt satisfies the above range, when the lithium secondary battery is stored at high temperature, the improvement effect of the cycle characteristics may be sufficient, and the viscosity of the nonaqueous electrolyte may be appropriate, and therefore, the impregnation property of the electrolyte may be improved.
[0049] The organic solvent contained in the nonaqueous electrolyte of the present invention may include at least one organic solvent selected from the group consisting of cyclic carbonate organic solvents, linear carbonate organic solvents, linear ester organic solvents, and cyclic ester organic solvents.
[0050] In particular, the organic solvent may include a cyclic carbonate-based organic solvent, a linear carbonate-based organic solvent, or a mixed organic solvent thereof.
[0051] The cyclic carbonate organic solvent is an organic solvent with high viscosity, and is an organic solvent with a high dielectric constant and good dissociation of lithium salts in the electrolyte. It can specifically include at least one organic solvent selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate and vinylene carbonate, and ethylene carbonate can be included therein.
[0052] In addition, the straight-chain carbonate organic solvent is an organic solvent having low viscosity and low dielectric constant, and generally at least one organic solvent selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methylpropyl carbonate and ethylpropyl carbonate can be used, in particular ethyl methyl carbonate (EMC).
[0053] In addition, in order to prepare an electrolyte with high ionic conductivity, in addition to at least one carbonate organic solvent selected from the group consisting of cyclic carbonate organic solvents and linear carbonate organic solvents, the organic solvent may also additionally include one or more ester organic solvents selected from the group consisting of linear ester organic solvents and cyclic ester organic solvents.
[0054] The linear ester organic solvent may specifically include at least one organic solvent selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate.
[0055] In addition, the cyclic ester organic solvent may include at least one organic solvent selected from the group consisting of γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone.
[0056] Meanwhile, the organic solvent may be an organic solvent commonly used in non-aqueous electrolytes as needed without limitation, for example, at least one organic solvent selected from ether organic solvents, glyme organic solvents, and nitrile organic solvents may be additionally included.
[0057] The ether solvent may be selected from the group consisting of dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether, ethyl propyl ether, 1,3-dioxolane (DOL) and 2,2-bis(trifluoromethyl)-1,3-dioxolane (TFDOL), or a mixture of two or more thereof without limitation.
[0058] The glycol dimethyl ether organic solvent has a higher dielectric constant and lower surface tension than the linear carbonate organic solvent and is less reactive with metals, and may include at least one selected from the group consisting of dimethoxyethane (glycol dimethyl ether, DME), diethoxyethane, diglyme, triglyme, and tetraglyme (TEGDME) without limitation.
[0059] The nitrile solvent may be one or more selected from the group consisting of acetonitrile, propionitrile, butyronitrile, valeronitrile, octanonitrile, heptanenitrile, cyclopentanenitrile, cyclohexanenitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, benzyl cyanide, 2-fluorophenyl cyanide and 4-fluorophenyl cyanide without limitation.
[0060] The non-aqueous electrolyte of the present invention may additionally include known electrolyte additives in the non-aqueous electrolyte as needed to prevent the collapse of the negative electrode induced by the decomposition of the non-aqueous electrolyte in a high-output environment, or to further improve the high-rate discharge performance at low temperatures, high-temperature stability, prevent overcharging, and inhibit the expansion of the battery at high temperatures.
[0061] Other electrolyte additives may include at least one additive for forming a SEI layer selected from the group consisting of: cyclic carbonate compounds, sultone compounds, sulfate compounds, phosphate compounds, borate compounds, nitrile compounds, benzene compounds, amine compounds, silane compounds and lithium salt compounds.
[0062] The cyclic carbonate-based compound may include vinylene carbonate (VC), vinylethylene carbonate, or fluoroethylene carbonate.
[0063] The sultone compound may be at least one compound selected from the group consisting of 1,3-propane sultone (PS), 1,4-butane sultone, ethylene sultone, 1,3-propene sultone (PRS), 1,4-butene sultone and 1-methyl-1,3-propene sultone.
[0064] The sulfate compound may include ethylene sulfate (Esa), trimethylene sulfate (TMS) or tripropylene methyl sulfate (MTMS).
[0065] The phosphate compound may include one or more compounds selected from the group consisting of lithium difluorobis(oxalato)phosphate, lithium difluorophosphate, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, tris(2,2,2-trifluoroethyl)phosphate and tris(2,2,2-trifluoroethyl)phosphite.
[0066] Borate compounds may include tetraphenylborate and lithium oxalyldifluoroborate (LiODFB) and lithium bis(oxalate)borate (LiB(C2O4)2, LiBOB).
[0067] The nitrile compound may include at least one compound selected from the group consisting of succinonitrile, adiponitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, octanonitrile, heptanecarbonitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, benzyl cyanide, 2-fluorophenyl cyanide and 4-fluorophenyl cyanide.
[0068] The benzene compound may include fluorobenzene, the amine compound may include triethanolamine or ethylenediamine, and the silane compound may include tetravinylsilane.
[0069] The lithium salt-based compound is a compound other than the lithium salt contained in the non-aqueous electrolyte, and may include lithium difluorophosphate (LiDFP), LiPO2F2, LiBF4, and the like.
[0070] Among other electrolyte additives, if a combination of vinylene carbonate (VC), 1,3-propane sultone and ethylene sulfate is additionally included, a stronger SEI coating can be formed on the negative electrode surface during the initial activation of the secondary battery, gas generation due to decomposition of the electrolyte at high temperature can be suppressed, and the high temperature stability of the secondary battery can be improved.
[0071] Meanwhile, the additional electrolyte additive may be used by mixing two or more types at 0.1 wt % to 10 wt %, particularly 0.2 wt % to 8 wt %, preferably 0.5 wt % to 8 wt % based on the total weight of the nonaqueous electrolyte. If the content of the additional electrolyte additive satisfies the above range, the improvement effect of ion conductivity and cycle characteristics will be better.
[0072] Lithium secondary battery
[0073] The present invention provides a lithium secondary battery comprising the above nonaqueous electrolyte.
[0074] In particular, the lithium secondary battery includes a positive electrode including a positive electrode active material, a negative electrode including a negative electrode active material, a separator provided between the positive electrode and the negative electrode, and the above-mentioned nonaqueous electrolyte.
[0075] In this case, the lithium secondary battery of the present invention can be manufactured by a common method known in the art. For example, a positive electrode, a negative electrode and a separator between the positive electrode and the negative electrode can be stacked to manufacture an electrode assembly, the electrode assembly can be inserted into a battery case, and a nonaqueous electrolyte of the present invention can be injected to manufacture a lithium secondary battery.
[0076] The lithium secondary battery of the present invention may have a driving voltage of 4.47 V or more and may operate at a high voltage.
[0077] (1) Cathode materials
[0078] The positive electrode may be manufactured by applying a positive electrode mixture slurry including a positive electrode active material, a binder, a conductive agent, and a solvent onto a positive electrode collector.
[0079] The positive electrode current collector is not particularly limited as long as it does not cause chemical changes in the battery and has conductivity, for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. can be used.
[0080] The positive electrode active material may be a compound capable of reversibly intercalating and deintercalating lithium, particularly a lithium metal oxide including one or more metals such as cobalt, manganese, nickel, and aluminum, and lithium. More specifically, the lithium metal oxide may be a lithium manganese-based oxide (such as LiMnO2, LiMn2O4, etc.), a lithium cobalt-based oxide (such as LiCoO2, etc.), a lithium nickel-based oxide (such as LiNiO2, etc.), a lithium nickel manganese-based oxide (such as, LiNi 1-Y Mn Y O2 (where 0 < Y < 1), LiMn 2-z Ni z O4 (where 0 < z < 2), etc.), a lithium nickel cobalt-based oxide (such as LiNi 1-Y1 Co Y1 O2 (where 0 < Y1 < 1), etc.), a lithium manganese cobalt-based oxide (such as, LiCo 1-Y2 Mn Y2 O2 (where 0 < Y2 < 1), LiMn 2-z1 Co z1 O4 (where 0 < z1 < 2), etc.), a lithium nickel manganese cobalt-based oxide (such as, Li(Ni p Co q Mn r )O2 (where 0 < p < 1, 0 < q < 1, 0 < r < 1, and p + q + r = 1) or Li(Ni p1 Co q1 Mn r1 )O4 (where 0 < p1 < 2, 0 < q1 < 2, 0 < r1 < 2, and p1 + q1 + r1 = 2), etc.), or a lithium nickel cobalt transition metal (M) oxide (such as, Li(Ni p2 Co q2 Mn r2 M s2 )O2 (where M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, and Mo, and p2, q2, r2, and s2 are the atomic fractions of the respective independent elements, where 0 < p2 < 1, 0 < q2 < 1, 0 < r2 < 1, 0 < s2 < 1, and p2 + q2 + r2 + s2 = 1), etc.), etc., and may include one or more than two of these compounds.
[0081] Among them, in terms of improving the capacity characteristics and stability of the battery, the lithium metal oxide may include LiCoO2, LiMnO2, LiNiO2, lithium nickel manganese cobalt oxides (such as Li(Ni 1 / 3 Mn 1 / 3 Co 1 / 3 )O2, Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5Mn 0.3 Co 0.2 )O2、Li(Ni 0.7 Mn 0.15 Co 0.15 )O2、Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc.), lithium nickel cobalt aluminum oxide (such as Li(Ni 0.8 Co 0.15 Al 0.05 )O2, etc.) or lithium nickel manganese aluminum oxide (e.g. Li(Ni 0.86 Co 0.05 Mn 0.07 Al 0.02 )O2) etc., and one or a mixture of two or more thereof can be used.
[0082] In order to maximize the improvement of the capacity performance of the battery, a positive electrode active material having a nickel content of 80 atomic % or more may be used. For example, the lithium transition metal oxide may include the following [Formula 2].
[0083] [Formula 2]
[0084] Li x Ni a Co b M 1 c M 2 d O2
[0085] In formula 2, M 1 The metal may be one or more selected from Mn and Al. In view of durability, Mn or a combination of Mn and Al is preferred.
[0086] M 2 It may be one or more selected from Zr, B, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, F, P and S.
[0087] x represents the atomic fraction of lithium in the lithium transition metal oxide, and may satisfy 0.90≤x≤1.1, preferably 0.95≤x≤1.08, and more preferably 1.0≤x≤1.08.
[0088] a represents the atomic fraction of nickel in the metal elements other than lithium in the lithium transition metal oxide, and may satisfy 0.80≤a≤1.0, preferably 0.80≤a≤0.95, and more preferably 0.80≤a≤0.90. If the nickel content satisfies the above range, high capacity performance may be achieved.
[0089] b represents the atomic fraction of cobalt among the metal elements other than lithium in the lithium transition metal oxide, and can satisfy 0 ≤ b ≤ 0.2, 0 ≤ b ≤ 0.15 or 0.01 ≤ b ≤ 0.10.
[0090] c represents the atomic fraction of M among the metal elements other than lithium in the lithium transition metal oxide 1 and can satisfy 0 < c < 0.2, 0 < c ≤ 0.15 or 0.01 ≤ c ≤ 0.10.
[0091] d represents the atomic fraction of M among the metal elements other than lithium in the lithium transition metal oxide 2 and can satisfy 0 ≤ d ≤ 0.1 or 0 ≤ d ≤ 0.05.
[0092] Based on the total weight of the solids other than the solvent in the positive electrode mixture slurry, the content of the positive electrode active material can be 60% by weight to 99% by weight, preferably 70% by weight to 99% by weight, and more preferably 80% by weight to 98% by weight.
[0093] The binder is a component that aids in the adhesion of the active material, conductive agent, etc. and the adhesion to the current collector.
[0094] The binder can include, for example, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene (PE), polypropylene, ethylene - propylene - diene monomer, sulfonated ethylene - propylene - diene monomer, styrene - butadiene rubber, fluororubber, or various copolymers, etc.
[0095] Generally, based on the total weight of the solids other than the solvent in the positive electrode mixture slurry, the content of the binder can be 1% by weight to 20% by weight, preferably 1% by weight to 15% by weight, and more preferably 1% by weight to 10% by weight.
[0096] The conductive agent is a component used to further improve the conductivity of the positive electrode active material, and the addition amount can be 1% by weight to 20% by weight based on the total weight of the solids in the positive electrode mixture slurry. There is no specific limitation on the conductive agent as long as it does not cause chemical changes in the battery and has conductivity, and it can include: for example, carbon powders such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal cracking carbon black; graphite powders such as natural graphite, artificial graphite, and graphite with a very developed crystal structure; conductive fibers such as carbon fibers and metal fibers; fluorocarbon powders; conductive powders such as aluminum powder and nickel powder; conductive whiskers such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0097] Generally, the content of the conductive agent may be 1 wt % to 20 wt %, preferably 1 wt % to 15 wt %, and more preferably 1 wt % to 10 wt %, based on the total weight of solids excluding the solvent in the positive electrode mixture slurry.
[0098] The solvent may include an organic solvent, such as N-methyl-2-pyrrolidone (NMP), etc., and its amount may provide a preferred viscosity together with the positive electrode active material and the optional binder and the conductive agent. For example, the solvent may be included so that the concentration of the solids containing the positive electrode active material and the optional binder and the conductive agent may be 50% to 95% by weight, preferably 70% to 95% by weight, and more preferably 70% to 90% by weight.
[0099] (2) Negative electrode
[0100] The negative electrode may be manufactured by coating a negative electrode mixture slurry including, for example, a negative electrode active material, a binder, and a solvent onto a negative electrode collector, or a graphite electrode composed of carbon (C) or a metal itself may be used as the negative electrode.
[0101] For example, if the negative electrode is manufactured by coating the negative electrode mixture slurry onto the negative electrode current collector, the negative electrode current collector generally has a thickness of 3 to 500 μm. The negative electrode current collector is not particularly limited as long as it does not cause chemical changes in the battery and has conductivity, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., or aluminum-cadmium alloy, etc. can be used. In addition, as with the positive electrode current collector, micro-concave and convex objects can be formed on its surface to enhance the adhesion of the negative electrode active material, and various types such as films, sheets, foils, nets, porous bodies, foams, and non-woven fabrics can be used.
[0102] In addition, the negative electrode active material may include at least one selected from the group consisting of lithium metal, carbon materials that can reversibly intercalate / deintercalate lithium ions, metals or alloys of the metals and lithium, metal composite oxides, materials that can be doped or dedoped with lithium, and transition metal oxides.
[0103] As a carbon material that can reversibly embed / deintercalate lithium ions, a carbon-based negative electrode active material commonly used in lithium ion secondary batteries can be used without specific restrictions, typically crystalline carbon, amorphous carbon or both. Examples of crystalline carbon may include graphite, such as natural graphite and artificial graphite of amorphous type, plate-like type, flake type, spherical type or fiber type, and examples of amorphous carbon may include soft carbon (carbon baked at low temperatures), hard carbon, mesophase pitch carbide or baked coke, etc.
[0104] As the metal or an alloy of the metal and lithium, a metal selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn, or an alloy of the metal and lithium can be used.
[0105] As the metal composite oxide, one selected from the group consisting of PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5, Li x Fe2O3 (0 ≤ x ≤ 1), Li x WO2 (0 ≤ x ≤ 1), and Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, or Ge; Me': Al, B, P, Si, elements of Groups 1, 2, and 3 of the periodic table, or a halogen; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8).
[0106] The material capable of doping and de-doping lithium can include Si, SiO x (0 < x ≤ 2), Si-Y alloy (where Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, but excluding Si), Sn, SnO2, and Sn-Y (where Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, but excluding Sn), and SiO2 and at least one of them can be used in combination. The element Y can be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.
[0107] As the transition metal oxide, a lithium-containing titanium composite oxide (LTO), vanadium oxide, lithium vanadium oxide, etc. can be used.
[0108] Among them, the negative electrode active material can be composed of SiO x (0 < x ≤ 2) or a mixture of graphite and SiO x (0 < x ≤ 2). Considering increasing the capacity of the lithium secondary battery, graphite and SiO can be included in a weight ratio of 100:0 to 70:30.x (0 <x≤2)。
[0109] The content of the negative electrode active material may be 60 wt % to 99 wt %, preferably 70 wt % to 99 wt %, and more preferably 80 wt % to 98 wt %, based on the total weight of the solid in the negative electrode mixture slurry.
[0110] The binder is a component that assists the bonding between the conductive agent, the active material and the current collector. The binder may include, for example, polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber or various copolymers.
[0111] Generally, the binder may be contained in an amount of 1 to 20 wt %, preferably 1 to 15 wt %, and more preferably 1 to 10 wt %, based on the total weight of solids excluding the solvent in the negative electrode mixture slurry.
[0112] The conductive agent is a component for further improving the conductivity of the negative electrode active material, and its content can be 1% to 20% by weight based on the total weight of the solid content of the negative electrode mixture slurry. The conductive agent is not specifically limited as long as it does not cause chemical changes in the battery and has conductivity, and can include: for example, carbon powders such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; graphite powders such as natural graphite, artificial graphite, and graphite having a very developed crystal structure; conductive fibers such as carbon fibers and metal fibers; fluorocarbon powders; conductive powders such as aluminum powder and nickel powder; conductive whiskers such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0113] The content of the conductive agent may be 1 wt % to 20 wt %, preferably 1 wt % to 15 wt %, and more preferably 1 wt % to 10 wt %, based on the total weight of the solid matter excluding the solvent in the negative electrode mixture slurry.
[0114] The solvent may include water or an organic solvent such as N-methyl-2-pyrrolidone (NMP), and its amount may provide a preferred viscosity together with the negative electrode active material and the optional binder and conductive agent. For example, the solvent may be included so that the concentration of the solids containing the negative electrode active material and the optional binder and conductive agent may be 50 wt % to 95 wt %, preferably 70 wt % to 90 wt %.
[0115] If the metal itself is used as the negative electrode, the metal thin film itself can be used, or the negative electrode can be manufactured by physically bonding, rolling or depositing the metal on the negative electrode current collector. The deposition method can use electrodeposition or chemical vapor deposition of the metal.
[0116] For example, the metal film itself or the metal bonded / rolled / deposited on the negative electrode current collector can be a type of metal selected from the group consisting of lithium (Li), nickel (Ni), tin (Sn), copper (Cu) and indium (In), or an alloy of two of the metals.
[0117] (3) Diaphragm
[0118] In addition, as a separator, a porous polymer film used as a common separator can be used, for example, a porous polymer film formed by a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer and an ethylene / methacrylate copolymer can be used, which can be used alone or as its stacked structure. In addition, commonly used porous non-woven fabrics can be used, such as non-woven fabrics of glass fibers, polyethylene terephthalate fibers with high melting points, but are not limited thereto. In addition, in order to ensure heat resistance and mechanical strength, a coated separator including a ceramic component or a polymer material can be optionally used in a monolayer or multilayer structure.
[0119] The appearance of the lithium secondary battery of the present invention is not particularly limited, but may be a cylindrical type using a can, a prismatic type, a pouch type, or a coin type.
[0120] Hereinafter, the present invention will be explained in more detail with reference to specific embodiments. However, the embodiments are only for the purpose of helping to understand the present invention, rather than limiting the scope of the present invention. It will be apparent to those skilled in the art that various changes and modifications may be made within the scope and technical spirit of this specification sheet, and these changes and modifications are included in the claims appended hereto.
[0121] Example
[0122] Example 1
[0123] (Preparation of non-aqueous electrolyte)
[0124] In an organic solvent (ethylene carbonate (EC): dimethyl carbonate (DMC) = 20:80 (volume ratio)), LiPF6 was dissolved to 1 M to prepare a nonaqueous solvent, and 1 g of the compound of the following formula 1a was injected into 99 g of the nonaqueous solvent to prepare a nonaqueous electrolyte.
[0125] [Formula 1a]
[0126]
[0127] (Manufacturing of lithium secondary batteries)
[0128] The positive electrode active material (LiNi 0.90 Co 0.03 Mn 0.06 Al 0.01 O2): conductive agent (carbon black): binder (polyvinylidene fluoride) was added to N-methyl-2-pyrrolidone (NMP) solvent at a weight ratio of 97.5:1.3:1.2 to prepare a positive electrode slurry (solid content of 74 wt%). The positive electrode slurry was coated on one side of a positive electrode collector (Al film) with a thickness of 130 μm, dried and rolled to manufacture a positive electrode.
[0129] The negative electrode active material (graphite: SiO = 97: 3 (weight ratio)): conductive agent (carbon black): binder (polyvinylidene fluoride) was added to N-methyl-2-pyrrolidone (NMP) solvent at a weight ratio of 96.8: 0.2: 3.0 to prepare a negative electrode slurry (solid content 60 weight%). The negative electrode slurry was coated on one side of a negative electrode current collector (Cu film) with a thickness of 128 μm, dried and rolled to manufacture a negative electrode.
[0130] In a drying chamber, a porous polymer separator manufactured using a polyolefin-based polymer was disposed between the positive electrode and the negative electrode thus formed, and the prepared nonaqueous electrolyte was injected to manufacture a secondary battery.
[0131] Example 2
[0132] A secondary battery was prepared by the same method as in Example 1, except that a nonaqueous electrolyte was prepared by injecting 1 g of the compound of Formula 1d into 99 g of the nonaqueous solvent prepared in Example 1.
[0133] [Formula 1d]
[0134]
[0135] Example 3
[0136] A secondary battery was prepared by the same method as in Example 1, except that a nonaqueous electrolyte was prepared by injecting 0.5 g of the compound of Formula 1a into 99.5 g of the nonaqueous solvent prepared in Example 1.
[0137] Example 4
[0138] A secondary battery was prepared by the same method as in Example 1, except that a nonaqueous electrolyte was prepared by injecting 3 g of the compound of Formula 1a into 97.5 g of the nonaqueous solvent prepared in Example 1.
[0139] Example 5
[0140] A secondary battery was prepared by the same method as in Example 1, except that a nonaqueous electrolyte was prepared by injecting 5 g of the compound of Formula 1a into 95 g of the nonaqueous solvent prepared in Example 1.
[0141] Comparative Example 1
[0142] A secondary battery was manufactured by the same method as in Example 1, except that 100 g of the nonaqueous solvent prepared in Example 1 was used to prepare the nonaqueous electrolyte.
[0143] Comparative Example 2
[0144] A secondary battery was manufactured by the same method as in Example 1, except that the nonaqueous electrolyte was prepared by injecting 0.5 g of 3,6-dimethyl-1,4-dioxane-2,5-dione into 99.5 g of the nonaqueous solvent prepared in Example 1.
[0145] Experimental Example 1-Evaluation of High Temperature Cycle Characteristics
[0146] The secondary batteries manufactured in Examples 1 to 5 and Comparative Examples 1 and 2 were evaluated for cycle characteristics.
[0147] Specifically, when 1 cycle includes charging to 4.2V at 1.0C rate in CC / CV mode and discharging to 2.5V at 1.0C rate in CC mode at 45°C, each battery manufactured in Examples 1 to 5 and Comparative Examples 1 and 2 was subjected to 200 charge and discharge cycles, and the capacity retention ratio compared with the initial capacity after 1 cycle was measured. The results are shown in Table 1.
[0148] [Table 1]
[0149] Capacity retention rate (%) Example 1 94.2% Example 2 93.5% Example 3 90.9% Example 4 93.3% Example 5 92.7% Comparative Example 1 87.6% Comparative Example 2 90.3%
[0150] As shown in Table 1, it can be confirmed that Examples 1 to 5 using the additive for non-aqueous electrolyte of the present invention show high capacity retention and improved life characteristics after 200 cycles compared to Comparative Example 1. In particular, it can be confirmed that the life characteristics of the lithium secondary batteries of Examples 1 to 5 using the additive of Formula 1 of the present invention are better than Comparative Example 2 using 3,6-dimethyl-1,4-dioxane-2,5-dione in which the propargyl group is not substituted (different from the additive for non-aqueous electrolyte of the present invention).
[0151] Experimental Example 2-Evaluation of High Temperature Storage Characteristics
[0152] The secondary batteries manufactured in Examples 1 to 5 and Comparative Examples 1 and 2 were evaluated for high-temperature storage performance.
[0153] Specifically, each of the batteries manufactured in Examples 1 to 5 and Comparative Examples 1 and 2 was fully charged to 4.35 V and then stored at 60° C. for 6 weeks.
[0154] Before storage, the capacity of the fully charged secondary battery was measured and set as the initial capacity of the secondary battery.
[0155] After 6 weeks, the capacity of the stored secondary battery was measured, and the capacity reduced during the 6-week storage period was calculated. The percentage of the reduced capacity of the secondary battery relative to the initial capacity was calculated, and the capacity retention rate after 6 weeks was calculated. The results are shown in Table 2.
[0156] [Table 2]
[0157] Capacity retention rate (%) Example 1 92.3% Example 2 92.1% Example 3 90.4% Example 4 93.7% Example 5 94.6% Comparative Example 1 89.5% Comparative Example 2 89.9%
[0158] As shown in Table 2, the secondary batteries of Examples 1 to 5 showed higher capacity retention and stable high temperature performance after 6 weeks compared to the secondary battery of Comparative Example 1. In particular, it can be confirmed that the lithium secondary batteries of Examples 1 to 5 using the additive of Formula 1 of the present invention have better high temperature storage properties than Comparative Example 2 using 3,6-dimethyl-1,4-dioxane-2,5-dione in which the propargyl group is not substituted (different from the additive for non-aqueous electrolyte of the present invention).
Claims
1. A non-aqueous electrolyte comprising: Lithium salts; organic solvents; and The compound of the following formula 1 as an additive: [Formula 1] In formula 1, R1 is one selected from the group consisting of H, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an aryl group having 6 to 8 carbon atoms, and R2 is one selected from the group consisting of an alkylene group having 1 to 10 carbon atoms and -OR3-, wherein R3 is an alkylene group having 1 to 10 carbon atoms.
2. The nonaqueous electrolyte according to claim 1, wherein R1 of Formula 1 is H or an alkyl group having 1 to 10 carbon atoms.
3. The nonaqueous electrolyte according to claim 1, wherein R2 of Formula 1 is one selected from the group consisting of an alkylene group having 1 to 5 carbon atoms and -OR3-, wherein R3 is an alkylene group having 1 to 5 carbon atoms.
4. The nonaqueous electrolyte according to claim 1, wherein The compound of Formula 1 is one selected from the group consisting of the following Formulae 1a to 1d: [Formula 1a] [Formula 1b] [Formula 1c] [Formula 1d] 5. The nonaqueous electrolyte according to claim 1, wherein The compound of Formula 1 may be included in an amount of 0.01 parts by weight to 5 parts by weight based on 100 parts by weight of the non-aqueous electrolyte.
6. The nonaqueous electrolyte according to claim 1, wherein The lithium salt is at least one selected from the group consisting of LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10 , LiAlCl4, LiAlO2, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiN(SO2F)2, LiN(SO2CF2CF3)2 and LiN(SO2CF3)2.
7. The nonaqueous electrolyte according to claim 1, wherein The lithium salt is included in a concentration of 0.5M to 3M.
8. The nonaqueous electrolyte according to claim 1, wherein The organic solvent includes at least one selected from the group consisting of a cyclic carbonate organic solvent, a linear carbonate organic solvent, a linear ester organic solvent, and a cyclic ester organic solvent.
9. A lithium secondary battery comprising: positive electrode; negative electrode; as well as The nonaqueous electrolyte according to any one of claims 1 to 8.
10. The lithium secondary battery according to claim 9, wherein: The positive electrode includes a lithium nickel cobalt manganese-based oxide as a positive electrode active material.
11. The lithium secondary battery according to claim 9, wherein The negative electrode comprises graphite and SiO x As negative electrode active material, where 0≤x<2.