Alumina material, hydrogenation catalyst and preparation method thereof

By growing AlOOH in situ on the γ-Al2O3 carrier to form worm-like structures and supported metal components, the problems of existing catalysts being easily poisoned and unstable in the hydrotreatment of heavy oils are solved, and efficient hydronitrition and denitrogenation are achieved. Desulfurization activity and stability.

CN118874449AActive Publication Date: 2024-11-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310457469.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-01
Estimated Expiration
2043-04-26

AI Technical Summary

Technical Problem

The existing hydrogenation catalysts are susceptible to poisoning of impurities such as sulfur, nitrogen and metals during heavy oil hydrotreatment, resulting in catalyst deactivation, especially the removal of nitrogen compounds is difficult, and the pore structure on the surface of the catalyst is not conducive to the diffusion of reactant molecules. Influences catalytic activity.

Method used

Using the mixed phase of γ-Al2O3 and AlOOH as the alumina material, AlOOH is grown in situ on the surface of γ-Al2O3 carrier to form a worm-like structure through hydrothermal treatment, forming a high coverage and open pores, improving the diffusion capacity of reactants, and passing through loading. Group VIB and Group VIII metal components enhance catalytic activity.

Benefits of technology

It improves the hydrodenitrification and desulfurization activities of the catalyst and enhances the activity stability. It is suitable for the heavy oil hydrogenation field, significantly improving the internal reaction activity and stability of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874449A_ABST
    Figure CN118874449A_ABST
Patent Text Reader

Abstract

The invention discloses an alumina material, a hydrogenation catalyst and a preparation method thereof. The alumina material is a mixed phase of gamma-Al2O3 and AlOOH, the AlOOH is worm-shaped and grows on the outer surface of a gamma-Al2O3 carrier in situ, and the coverage rate of worm-shaped AlOOH crystal grains on the outer surface of the gamma-Al2O3 carrier is 85%-100%. The preparation method of the alumina material comprises the following steps: putting a gamma-Al2O3 carrier in an epoxypropane solution, and carrying out hydrothermal treatment under a closed condition: firstly carrying out hydrothermal treatment at 60-100 DEG C for 1-4 hours, then carrying out hydrothermal treatment at 110-180 DEG C, preferably 120-160 DEG C for 2-6 hours, and drying the treated material to obtain the alumina material. The surface particles of the alumina material are wormlike, the content of 8-15nm pore channels is high, the alumina material as the carrier has a wide application prospect in heterogeneous catalyst reaction, especially in the field of heavy oil hydrogenation, and a hydrogenation catalyst prepared from the carrier has high hydrodenitrogenation and desulfurization activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalyst preparation, and specifically relates to an aluminum oxide material, a hydrogenation catalyst and a preparation method thereof. Background Art

[0002] With the increasing trend of heavy crude oil and the development of unconventional oil resources, heavy oil (heavy distillate oil) will become the main target of future oil processing. The main characteristics of heavy oil are high content of sulfur, nitrogen, metals and polycyclic aromatic hydrocarbons, which are easy to cause catalyst poisoning and deactivation during heavy oil hydroprocessing, thus placing higher requirements on hydroprocessing catalysts. The sulfur, nitrogen, metals, etc. of heavy oil are all in the aromatic ring structure, and nitrogen compounds are the most difficult to remove by hydrodenitrification. Therefore, the development of catalysts for hydrodenitrification of inferior heavy distillate oil is the key to improving the technical level of heavy oil hydroprocessing.

[0003] CN105983412A discloses a hydrogenation catalyst with high denitrification performance and a preparation method thereof, wherein silicon-containing pseudo-boehmite is first prepared, a phosphate is added to the silicon-containing pseudo-boehmite during the peptization process to obtain a carrier, and finally an active component is loaded to obtain a catalyst. Although the catalyst prepared by the method has a high pore volume, specific surface area, a certain 20-30 nm pore content and suitable acid properties, the pore structure on the catalyst surface is not conducive to the diffusion of reactant molecules.

[0004] CN111821989A discloses a residual oil hydrodenitrogenation catalyst and a preparation method thereof. The catalyst comprises a modified alumina-based carrier, molybdenum and nickel metal components, the modified alumina-based carrier contains tungsten and cobalt metal components, the modified alumina-based carrier comprises a main body modified alumina and a rod-shaped modified alumina, the main body modified alumina is a modified alumina with micron-sized pores, wherein at least part of the rod-shaped modified alumina is distributed on the outer surface of the main body modified alumina and in the micron-sized pores with a pore diameter D of 3-7 μm. The surface of the catalyst prepared by this method is a rod-shaped structure, but the firmness of the bonding between the rod-shaped alumina grown on the surface and the main body alumina needs to be further improved. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides an alumina material, a hydrogenation catalyst and a preparation method thereof. The surface particle morphology of the alumina material is worm-like and the content of 8-15 nm pores is relatively high. The alumina as a carrier has broad application prospects in multiphase catalyst reactions, especially in the field of heavy oil hydrogenation. The hydrogenation catalyst prepared with the carrier has high hydrogenation denitrogenation and desulfurization activity.

[0006] The aluminum oxide material of the present invention is a mixed phase of γ-Al2O3 and AlOOH, wherein the AlOOH morphology is worm-like, in-situ grown on the outer surface of the γ-Al2O3 carrier, and the coverage rate of the worm-like AlOOH grains on the outer surface of the γ-Al2O3 carrier is 85%-100%, wherein the coverage rate refers to the percentage of the surface occupied by the worm-like AlOOH particles on the outer surface of the γ-Al2O3 carrier to the outer surface of the γ-Al2O3 carrier. The worm-like AlOOH grain size is 80-350nm, and the accumulation forms an open channel of 30-100nm.

[0007] In the alumina material of the present invention, the ratio H of the grain size of the crystal face corresponding to the peak of the crystalline phase AlOOH (120) to the grain size of the crystal face corresponding to the peak of γ-Al2O3 (440) is 1.5-2.5, H=D AlOOH (120) / D γ-Al2O3 (440), wherein D(120) represents the grain size of the crystal plane corresponding to the AlOOH (120) peak in the XRD spectrum; the 120 peak refers to the characteristic peak with 2θ of 25.5-29.9° in the XRD spectrum; the D(440) represents the grain size of the crystal plane corresponding to the γ-Al2O3 (440) peak in the XRD spectrum; the 440 peak refers to the characteristic peak with 2θ of 63.6-69.1° in the XRD spectrum.

[0008] The specific surface area of ​​the alumina material of the present invention is 220-380m 2 / g, the pore volume is 0.6-1.3mL / g, the most probable pore diameter is 8-15nm, and the pores of 8-15nm account for 60%-80% of the total pore volume.

[0009] The preparation method of the alumina material of the present invention comprises the following contents: placing a γ-Al2O3 carrier in a propylene oxide solution under closed conditions for hydrothermal treatment: first, hydrothermal treatment at 60-100°C for 1-4 hours, then hydrothermal treatment at 110-180°C, preferably 120-160°C, for 2-6 hours, and the treated material is dried to obtain the alumina material.

[0010] In the method of the present invention, the γ-Al2O3 carrier described in step (1) can be a commercial product or prepared according to an existing method, and its shape can be the shape of a conventional alumina carrier, such as a sphere, and its particle size is generally 2-8.0 mm, such as a cylindrical bar, a clover, a four-leaf clover, etc., with a diameter of about 0.2-3.0 mm and a length of about 3-8.0 mm. For example, the γ-phase alumina carrier is generally obtained by kneading, molding, drying, and roasting pseudo-boehmite. The pseudo-boehmite can be pseudo-boehmite prepared by any method, and an extrusion aid and a peptizing agent can be added as needed during molding. The extrusion aid is sesbania powder, and the amount added is 0.1wt%-0.5wt% of the weight of the alumina carrier. The peptizing agent is one or more of hydrochloric acid, nitric acid, sulfuric acid, acetic acid, oxalic acid, etc., and the amount of the peptizing agent added is 0.5wt%-1.5wt% of the weight of the alumina carrier. The drying temperature is 100-160° C., the drying time is 1-8 hours, the roasting temperature is 450-600° C., and the roasting time is 1-8 hours.

[0011] In the method of the present invention, the concentration of the propylene oxide aqueous solution in step (2) is 2.5wt%-12wt%, preferably 4wt%-8wt%, and the mass ratio of the propylene oxide aqueous solution to the γ-Al2O3 carrier is 3:1-10:1, preferably 4:1-8:1. The sealed heat treatment is carried out in a closed container, which is preferably an autoclave. The sealed heat treatment is a two-step sealed heat treatment, i.e., firstly sealed heat treatment at 60-100°C for 1-4 hours, and then at 110-180°C, preferably 120-160°C, for 2-6 hours.

[0012] In the method of the present invention, the drying temperature in step (2) is 100-160°C, the drying time is 2-8 hours, the roasting temperature is 600-750°C, the roasting time is 4-6 hours, and the roasting is carried out in an oxygen-containing atmosphere, preferably in an air atmosphere.

[0013] The present invention also provides an alumina carrier, which is obtained by calcining the alumina material. The calcination conditions are: the calcination temperature is 450-700° C., and the calcination time is 4-10 hours.

[0014] The present invention also provides a hydrogenation catalyst, which comprises the above-mentioned alumina carrier or the above-mentioned alumina material. The hydrogenation catalyst is obtained by loading the hydrogenation active component on the alumina carrier or the alumina material.

[0015] Wherein, the loading can be carried out by impregnation, kneading and the like. For example, the alumina carrier is impregnated with a hydrogenation active component impregnation solution, and the impregnated material is dried and calcined to obtain a hydrogenation catalyst. The hydrogenation active component impregnation solution is a solution containing group VIB and group VIII metals, the group VIB metals are selected from one or more of W and Mo, and the group VIII metals are selected from one or more of Co and Ni. The content of group VIB metals in the impregnation solution is 8.5%-22.5g / 100mL in terms of metal oxide, and the content of group VIII metals is 2.5%-6.5g / 100mL in terms of metal oxide. The drying temperature is 100-160°C, the drying time is 2-8 hours, the calcination temperature is 450-550°C, and the calcination time is 4-6 hours.

[0016] Compared with the prior art, the present invention has the following advantages: the present invention places the γ-Al2O3 carrier in a propylene oxide solution for sealed heat treatment. During the low-temperature sealed heat treatment, the propylene oxide is hydrolyzed to form an alcohol solution, and the solution is weakly alkaline. During the high-temperature sealed hydrothermal treatment, the surface grains of the γ-Al2O3 carrier grow in situ into worm-like AlOOH in an alkaline and alcohol solution environment. The worm-like AlOOH particles are uniformly and highly covered on the surface of the carrier. The particles are accumulated to form open channels of 30-100nm. The channel structure is conducive to the diffusion of reactant molecules into the interior of the catalyst, thereby improving the internal reaction activity of the catalyst. The alumina can be used as a carrier for multiphase catalytic reactions. After the alumina is calcined, the worm-like AlOOH grains on the surface of the carrier are phase-transformed into γ-Al2O3. The active metal components impregnated on the surface of the AlOOH grains cooperate with the phase change process of the AlOOH grains, effectively regulating the effect of the active metal components and the alumina carrier, reducing the formation of the nickel-aluminum spinel phase, and making the catalyst have higher denitrification and desulfurization activities while having higher activity stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] FIG. 1 is an XRD spectrum of the alumina support precursor (A) and the alumina support (B) prepared in Example 1.

[0018] Figure 2 This is a low-magnification SEM image of the surface of the alumina support prepared in Example 1.

[0019] Figure 3 This is a high-magnification SEM image of the surface of the alumina support prepared in Example 1.

[0020] Figure 4 Low magnification SEM image of the surface of the alumina support prepared in Comparative Example 2. DETAILED DESCRIPTION

[0021] The technical scheme and technical effect of the present invention are further described below in conjunction with the embodiments, but are not limited to the following embodiments. In the present invention, wt% represents mass fraction.

[0022] BET method: N2 physical adsorption-desorption was used to characterize the pore structure of the carriers of the embodiment and the comparative example. The specific operation was as follows: The pore structure of the sample was characterized by using an ASAP-2420 N2 physical adsorption-desorption instrument. A small amount of sample was vacuum treated at 300°C for 3-4 hours, and finally the product was placed under liquid nitrogen low temperature (-200°C) for nitrogen adsorption-desorption test. The specific surface area was obtained according to the BET equation, and the pore volume and the distribution rate of pore diameters below 30nm were obtained according to the BJH model.

[0023] Scanning electron microscopy was used to characterize the microstructure of the alumina carrier. The specific operation was as follows: a JSM-7500F scanning electron microscope was used to characterize the microstructure of the carrier, with an accelerating voltage of 5 KV, an accelerating current of 20 µA, and a working distance of 8 mm. Example 1

[0024] (1) Weigh 500 g of pseudo-boehmite, add 3 g of sesbania powder and mix well. Then add an appropriate amount of 0.5% acetic acid solution to the mixture and knead well. Extrusion molding is performed. The molded material is dried at 120°C for 5 hours and calcined at 600°C for 5 hours to obtain an alumina carrier precursor. The carrier XRD spectrum is shown in Figure 1 The A curve in .

[0025] (2) Weigh 100 g of the alumina carrier precursor prepared in step (1), add 660 g of a 5.3% propylene oxide aqueous solution, transfer the mixture into an autoclave, seal the autoclave, place it in an oven at 75° C. for 2.5 hours, then heat it to 130° C. for 5 hours, cool, wash, and filter the treated material, and dry the solid material at 130° C. for 6 hours to obtain an alumina carrier S1. The XRD spectrum of the carrier is shown in FIG. Figure 1 The B curve in the figure, the carrier properties are shown in Table 1, and the SEM image of the carrier surface is shown in Figure 2 , Figure 3 .

[0026] (3) Weigh 50 g of the alumina carrier S1 prepared in step (2) and impregnate the alumina carrier by saturated impregnation using an impregnation solution having a molybdenum oxide concentration of 18.3 g / 100 mL and a nickel oxide concentration of 4.9 g / 100 mL. The impregnated material is dried at 120° C. for 6 hours and calcined at 500° C. for 5 hours to obtain a hydrodenitrogenation catalyst Cat-1. Example 2

[0027] The same as Example 1, except that the concentration of propylene oxide in step (2) is 6.8%, the amount of solution used is 560 g, and the hydrothermal treatment is first performed at 80° C. for 2 hours and then at 145° C. for 4 hours to obtain the alumina carrier S2 and the hydrodenitrogenation catalyst Cat-2 of the present invention. The properties of the carrier are shown in Table 1. Example 3

[0028] The same as Example 1, except that the concentration of propylene oxide in step (2) is 4.6%, the amount of solution used is 720 g, and the hydrothermal treatment is first performed at 60° C. for 3.5 hours and then at 160° C. for 2.5 hours to obtain the alumina carrier S3 and the hydrodenitrogenation catalyst Cat-3 of the present invention. The properties of the carrier are shown in Table 1. Example 4

[0029] The same as Example 1, except that the concentration of propylene oxide in step (2) is 7.5%, the amount of solution used is 510 g, and the hydrothermal treatment is first performed at 90° C. for 1.5 hours and then at 125° C. for 5.5 hours to obtain the alumina carrier S4 and the hydrodenitrogenation catalyst Cat-4 of the present invention. The properties of the carrier are shown in Table 1.

[0030] Comparative Example 1 The same method as Example 1 was used, except that in step (2), the propylene oxide aqueous solution was replaced with an ammonia aqueous solution of the same mass concentration to prepare a comparative alumina support S5 and a comparative hydrodenitrogenation catalyst Cat-5. The properties of the alumina support are shown in Table 1.

[0031] Comparative Example 2 The same as Example 1, except that in step (2), the propylene oxide aqueous solution was replaced with an ethylene oxide solution of the same concentration, to prepare a comparative alumina support S6 and a comparative hydrodenitrogenation catalyst Cat-6. The properties of the alumina support are shown in Table 1, and the scanning electron micrograph of the outer surface of the support is shown in Figure 4 .

[0032] Comparative Example 3 The same method as Example 1, except that the concentration of propylene oxide in step (2) was 1.5%, produced a comparative alumina carrier S7 and a comparative hydrodenitrogenation catalyst Cat-7. The properties of the alumina carrier are shown in Table 1.

[0033] Comparative Example 4 The same as Example 1, except that the hydrothermal treatment in step (2) is a one-step hydrothermal treatment, the heat treatment temperature is 70° C., and the treatment time is 14 hours, to obtain a comparative alumina carrier S8 and a comparative hydrodenitrogenation catalyst Cat-8. The properties of the alumina carrier are shown in Table 1, and the properties of the hydrodemetallization catalyst are shown in Table 3.

[0034] Table 1 Alumina support properties Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Carrier S1 S2 S3 S4 S5 S6 S7 S8 <![CDATA[Specific surface area, m 2 / g]]> 269 284 277 292 220 232 247 239 Pore ​​volume, mL / g 0.95 0.93 0.92 0.94 0.83 0.85 0.88 0.87 8-15nm pore content, % 76.3 73.2 75.5 74.8 53.2 51.5 53.4 52.6 Surface worm-like particle size, nm 95-340 85-345 80-330 85-340 — — — — Surface coverage of worm-like particles, % 95 93 97 98 — — — — Pore ​​size on carrier surface, nm 35-95 35-100 30-95 30-100 10-70 15-75 10-65 10-80 H 1.9 1.7 2.1 2.3 — — — — From the data in Table 1 and Figure 2-4It can be seen that compared with the comparative example alumina carrier, the alumina carrier prepared by the method of the present invention has a higher content of 8-15 nm pores, and the alumina carrier surface has a high content of macropores and open pores. Example 5

[0035] The hydrodenitrogenation catalysts Cat-1, Cat-2, Cat-3, Cat-4 prepared by the present invention and the hydrodenitrogenation catalysts Cat-5, Cat-6, Cat-7, Cat-8 prepared by the comparative example were respectively loaded into a fixed bed hydrogenation reactor, and a vacuum residue oil was used as a raw material (the sulfur content in the raw material oil was 3.68wt%, the nitrogen content was 0.34wt%, and the residual carbon content was 16.4wt%). The catalytic performance of the catalyst was evaluated, and the reaction conditions were as follows: the reaction temperature was 390°C, the pressure was 14.8MPa, and the liquid hourly volume space velocity was 0.45h -1 , the hydrogen-to-oil volume ratio is 800. After 2000 hours of reaction, the content of each impurity in the generated oil is determined and the impurity removal rate is calculated. The evaluation results are shown in Table 2.

[0036] Table 2 Evaluation results of catalysts

[0037] It can be seen from the results in Table 2 that, compared with the comparative hydrodenitrogenation catalyst, the hydrodenitrogenation catalyst prepared by the method of the present invention has higher desulfurization and denitrification activities and higher activity stability.

Claims

1. An aluminum oxide material, characterized in that: The alumina material is a mixed crystal phase of γ-Al2O3 and AlOOH, wherein the AlOOH has a worm-like morphology and grows in situ on the outer surface of the γ-Al2O3 carrier, and the coverage rate of the worm-like AlOOH grains on the outer surface of the γ-Al2O3 carrier is 85%-100%.

2. The aluminum oxide material according to claim 1, characterized in that: The worm-like AlOOH grain size is 80-350 nm.

3. The aluminum oxide material according to claim 1, characterized in that: The worm-like AlOOH grains accumulate on the outer surface of the γ-Al2O3 carrier to form pores of 30-100 nm.

4. The aluminum oxide material according to claim 1, characterized in that: The ratio of the grain size of the crystal plane corresponding to the peak of the crystalline phase AlOOH (120) to the grain size of the crystal plane corresponding to the peak of γ-Al2O3 (440) is 1.5-2.5, H=D AlOOH (120) / D γ-Al2O3 (440), wherein D(120) represents the grain size of the crystal plane corresponding to the AlOOH (120) peak in the XRD spectrum; the 120 peak refers to the characteristic peak with 2θ of 25.5-29.9° in the XRD spectrum; the D(440) represents the grain size of the crystal plane corresponding to the γ-Al2O3 (440) peak in the XRD spectrum; the 440 peak refers to the characteristic peak with 2θ of 63.6-69.1° in the XRD spectrum.

5. The aluminum oxide material according to claim 1, characterized in that: The specific surface area of ​​alumina material is 220-380m 2 / g, the pore volume is 0.6-1.3mL / g, the most probable pore diameter is 8-15nm, and the pores of 8-15nm account for 60%-80% of the total pore volume.

6. A method for preparing the aluminum oxide material according to any one of claims 1 to 5, characterized in that The method comprises the following contents: placing a γ-Al2O3 carrier in a propylene oxide solution and performing hydrothermal treatment under closed conditions: first, performing hydrothermal treatment at 60-100°C for 1-4 hours, and then performing hydrothermal treatment at 110-180°C, preferably 120-160°C, for 2-6 hours, and drying the treated material to obtain an alumina material.

7. The method according to claim 6, characterized in that: The concentration of the propylene oxide aqueous solution in step (2) is 2.5wt%-12wt%, preferably 4wt%-8wt%, and the mass ratio of the propylene oxide aqueous solution to the γ-Al2O3 carrier is 3:1-10:1, preferably 4:1-8:

1.

8. The method according to claim 6, characterized in that: The drying temperature in step (2) is 100-160°C, and the drying time is 2-8 hours; the roasting temperature is 600-750°C, and the roasting time is 4-6 hours, and the roasting is carried out in an oxygen-containing atmosphere.

9. Use of the alumina material according to any one of claims 1 to 5 in a heterogeneous catalyst reaction.

10. An alumina carrier, characterized in that: The method is obtained by calcining the alumina material according to any one of claims 1 to 5.

11. The alumina carrier according to claim 9, characterized in that: The calcination conditions are as follows: the calcination temperature is 450-700° C. and the calcination time is 4-10 hours.

12. A hydrogenation catalyst, comprising the alumina carrier according to claim 9 and / or the alumina material according to any one of claims 1 to 5.

13. A hydrogenation catalyst according to claim 12, characterized in that: It is obtained by loading the hydrogenation active component on an alumina carrier or an alumina material.

Citation Information

Patent Citations

  • Precious metal hydrogenation catalyst, preparation method and application thereof

    CN104549357A

  • Heavy oil hydrogenation catalyst and preparation method thereof

    CN106140180A

  • Alumina carrier, and nickel-based catalyst using alumina carrier as carrier, preparation method and applications thereof

    CN106622393A

  • Preparation method of hydrodenitrogenation catalyst

    CN111821987A

  • Alkylene oxide catalyst and use thereof

    US20140088316A1