Segmented pyrolysis recycling method and device for siloxane waste liquid

Through efficient steam pyrolysis reforming and electrical pulse Joule thermal coupling technology, the problems of process complexity and low resource utilization efficiency in silicone waste liquid treatment are solved, and efficient resource utilization and high value-added products are realized. generate.

CN118877893AActive Publication Date: 2024-11-01ZHEJIANG UNIV

Patent Information

Application Number
CN202411056688.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-01
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

The prior art has problems such as high process complexity, low resource utilization efficiency, and secondary pollutants when treating silicone waste liquid, making it difficult to effectively remove pollutants in high-concentration silicone waste liquid.

Method used

Using a two-stage heat treatment method of high-efficiency steam pyrolysis reforming and electrical pulse Joule thermal coupling, the silicone waste liquid is converted into syngas and silicon carbide-graphene composite materials through hydrolysis and flash heating, achieving catalyst-free and free Resource utilization of waste.

Benefits of technology

The full component resource utilization of silicone waste liquid is realized, the carbon conversion rate and synthesis gas yield are improved, the processing time and energy consumption are reduced, and the waste generation is not generated, which increases the added value of the overall technical solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118877893A_ABST
    Figure CN118877893A_ABST
Patent Text Reader

Abstract

The invention discloses a pyrolysis method and device for siloxane waste liquid. The method comprises the steps that the siloxane waste liquid is preheated, atomized and evaporated to obtain siloxane waste liquid steam, the siloxane waste liquid steam and water vapor are mixed to obtain mixed steam, and the mixed steam is hydrolyzed and filtered in the inert gas atmosphere to obtain synthesis gas and pyrolysis ash; mixing the pyrolytic ash and conductive carbon black, compacting to obtain a fixed material, putting the fixed material into a Joule thermal reactor, and performing flash evaporation heating on the fixed material through pulse discharge to obtain the silicon carbide-graphene composite material. According to the method, the reaction process is rapid, the decomposed siloxane waste liquid generated by secondary pollutants is avoided, the method has the advantages of being good in adaptability, high in speed, high in efficiency, free of catalyst and free of waste generation, and resource conversion of the organic siloxane waste liquid can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to industrial hazardous waste treatment technology, and specifically relates to a segmented pyrolysis resource recovery method and device for siloxane waste liquid. Background Art

[0002] Silicone refers to an organic polymer of siloxane formed by cross-linking of silicon and oxygen. It mainly includes chemicals such as silicone rubber, silicone oil, and silicone-based coupling agents. It has a wide range of downstream applications, and the industry has a large scale and a complete industrial chain. In 2022, product output has reached 1.48 million tons and shows a rapid growth trend.

[0003] Siloxane monomer is one of the upstream basic raw materials for the deep processing of synthetic silicone products. It can form long-chain structures of silicon-oxygen and silicon-carbon-oxygen through various substitution or polymerization methods, and realize the synthesis of various silicone products such as silicone oil and silicone rubber. The synthesis process of siloxane involves the alcoholysis and distillation separation of chlorosilane, and waste is inevitably generated in the production process, with waste liquid of siloxane with dimethyldiethoxysilane, hexamethylcyclotrisiloxane and low degree of polymerization as typical representatives.

[0004] On the one hand, due to its unique large bond energy of silicon-oxygen bonds, it has strong chemical stability, and chemical oxidation methods are difficult to effectively remove siloxane; traditional incineration has high carbon emissions, making it difficult to achieve resource utilization of waste siloxane liquid. If this type of waste liquid is directly separated by distillation and other means, the separation cost is high and the separation efficiency is difficult to guarantee due to the unstable source of raw materials and complex components.

[0005] The invention patent application with the publication number CN 113880358 A discloses "a method for effectively removing siloxane and COD from organic silicon wastewater" and provides a method for removing siloxane from wastewater. By utilizing mechanical separation, Fenton oxidation, electro-flocculation, evaporative desalination, and terminal biodegradation methods, the pollutants in wastewater containing siloxane are removed and discharged. However, this method has high process complexity, involving more than thirty unit operations, and the treatment process has high process complexity. It is only applicable to siloxane substances with a content of no more than 10,000 ppm. The removal process mainly relies on front-end Fenton oxidation and flocculation separation, and it is difficult to dispose of and utilize waste liquid with organic silicon as the main component.

[0006] The invention patent application with publication number CN 104672452A discloses "A method for recycling and reusing waste polysiloxane materials" and provides a method for preparing large-scale polysiloxane materials using waste polysiloxane materials, thereby realizing the recycling of waste. However, this solution requires the use of precious metal catalysts and a large amount of organic solvents for more than ten hours, and requires secondary separation by column chromatography and other methods. The waste disposal efficiency is low and secondary waste is still generated. From the above analysis, it can be seen that the existing technology is mainly aimed at the purification of low-concentration siloxanes, and there are problems such as complex process operation, low resource utilization efficiency, and the generation of secondary pollutants. Summary of the invention

[0007] The present invention provides a method for the resource recovery of siloxane waste liquid by staged pyrolysis. The method can decompose the siloxane waste liquid with a rapid reaction process and without generating secondary pollutants. The method has the advantages of good adaptability, fast speed, high efficiency, no use of catalyst, no generation of waste, and can realize the resource recovery of organic siloxane waste liquid.

[0008] The present invention provides a method for recycling siloxane waste liquid by staged pyrolysis, comprising:

[0009] (1) preheating and atomizing siloxane waste liquid to obtain siloxane waste liquid vapor, mixing the siloxane waste liquid vapor with water vapor to obtain mixed vapor, and hydrolyzing and filtering the mixed vapor under an inert gas atmosphere to obtain synthesis gas and pyrolysis ash;

[0010] (2) The pyrolysis ash and conductive carbon black are mixed, ball-milled, and compacted to obtain a fixed material, and the fixed material is placed in a Joule heat reactor, and the fixed material is flash-heated by pulse discharge to obtain a silicon carbide-graphene composite material.

[0011] The present invention adopts a two-stage thermal treatment method for high-value utilization of waste liquid by coupling high-efficiency steam pyrolysis reforming and electric pulse Joule heat, which can obtain synthesis gas through water vapor pyrolysis reforming of waste liquid without using a catalyst, and at the same time utilize Joule heat flash evaporation to convert pyrolysis ash into a high-value-added silicon carbide-graphene composite material.

[0012] Preferably, the mass ratio of the siloxane waste liquid vapor to the water vapor is 1:1 to 3. If the water vapor content is too low, the hydrolysis will be insufficient, resulting in a significant decrease in the efficiency of producing synthesis gas by pyrolysis of the siloxane waste liquid vapor; if the water vapor content is too high, the specific heat of the mixed steam will increase, resulting in a decrease in the efficiency of the pyrolysis process.

[0013] Preferably, the hydrolysis temperature is 600-900°C, and the reaction residence time is 60-600 seconds. Too low a temperature is not conducive to the steam pyrolysis process and the decomposition of the hydrolysis product, and too low a reaction residence time causes insufficient hydrolysis and pyrolysis reactions, which is not conducive to the pyrolysis of waste siloxane to produce synthesis gas; too high a temperature and too long a residence time have no obvious promoting effect on the carbon conversion rate of the siloxane waste liquid steam.

[0014] Preferably, the components of the siloxane waste liquid include one or more of dimethyldiethoxysilane, hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane and dodecamethylcyclohexasiloxane.

[0015] Preferably, the resistivity of the fixing material is 2.51-200.96 Ω·cm, and the capacitance ratio of the fixing material to the Joule heat reactor is 0.5-1.5 g / F, so as to achieve efficient heating of the fixing material.

[0016] Preferably, the voltage of the flash heating is 100-170V.

[0017] Preferably, the fixed material is preheated at a voltage of 20 to 30 V to improve the stability of the flash evaporation, otherwise the flash evaporation temperature may be too low or a large amount of gas may be produced during the flash evaporation process, resulting in the explosion of the reaction quartz tube.

[0018] Preferably, the main components of the obtained synthesis gas are one or more of H2, CO, CO2, CH4, C2H6, C2H4, C3H8, and C3H6.

[0019] On the other hand, the present invention also provides a device for recycling siloxane waste liquid by staged pyrolysis, comprising:

[0020] A material pretreatment unit, used for preheating and atomizing the siloxane waste liquid to obtain siloxane waste liquid vapor;

[0021] A water vapor generating unit, used for generating water vapor;

[0022] A pyrolysis gasification furnace, the top of which is respectively connected to a siloxane waste liquid pretreatment unit and a water vapor generation unit, for mixing siloxane waste liquid vapor with water vapor to obtain mixed vapor, and hydrolyzing the mixed vapor under an inert gas atmosphere to obtain synthesis gas and pyrolysis gas;

[0023] An ash filter, which is connected to the bottom of the pyrolysis gasifier and is used to filter the pyrolysis gas to obtain pyrolysis ash and discharge the synthesis gas;

[0024] A ball mill is used to mix the pyrolysis ash collected in the filter with the conductive carbon black and grind them fully to obtain the material to be disposed;

[0025] The Joule heat reactor is used to compact the material to be disposed to obtain a fixed material, and flash heat the fixed material through pulse discharge to obtain a silicon carbide-graphene composite material.

[0026] Preferably, the material pretreatment unit comprises:

[0027] Siloxane waste liquid storage tank, used for storing siloxane waste liquid;

[0028] A material pump, connected to the siloxane waste liquid storage tank, is used to pump out the siloxane waste liquid at a set flow rate;

[0029] The material preheating device comprises a vertically arranged material pipeline and a heating device arranged outside the pipeline, wherein the material pipeline is connected to a material pump, and the heating device is used to heat the siloxane waste liquid in the material pipeline to obtain siloxane waste liquid vapor.

[0030] The pyrolysis gasification furnace reactor is a vertical pyrolysis furnace, with a material inlet and a carrier gas inlet at the top, a material outlet at the bottom, and a heating device arranged on the side wall. The premixed material enters the pyrolysis furnace from the top pipeline of the gasification furnace, and the pyrolysis product flows out of the gasification furnace from the bottom; the ash filter is provided with a multi-layer metal filter screen inside, and the pyrolysis furnace gas is filtered and collected from the filter screen to obtain pyrolysis ash; the Joule heat reactor is composed of a high-voltage power supply, a control system, a high-voltage capacitor, a material discharge heating tube, and a discharge electrode;

[0031] Preferably, the high-voltage capacitor capacity of the Joule heat reactor is 90 mF, and the control system can realize discharge at a maximum current of 600 A under different voltages;

[0032] Preferably, the Joule heat reactor includes a material discharge heating tube, which is made of quartz and can be replaced. The material discharge heating tube includes a graphite plug and a contact discharge electrode. The pyrolysis ash is loaded into the heating tube and compacted, and graphite plugs are added at both ends to contact the discharge electrode.

[0033] The technical principle of the present invention, which couples high-efficiency steam pyrolysis reforming and electric pulse Joule heat two-stage thermal treatment to achieve the treatment and high-value utilization of siloxane waste liquid, is as follows:

[0034] (1) The organic siloxane waste liquid is atomized after preheating, and then mixed with water vapor and introduced into a pyrolysis gasifier for pyrolysis. On the one hand, the organic siloxane can undergo hydrolysis reaction in this environment, promoting the cleavage of Si-OC bonds and generating Si-OH and C-OH structures, which promotes the decomposition of siloxane substances in the waste liquid and converts the carbon element from the chemically stable siloxane form to the alcohol form that is easy to undergo thermal cracking, thereby improving its carbon conversion efficiency. On the other hand, water vapor has weak oxidizing properties under high temperature conditions. In the high-temperature pyrolysis gasification process, it acts as an oxidant and a hydrogen and oxygen source, inhibiting the formation of coke in the high-temperature pyrolysis process, thereby promoting the increase of synthesis gas yield and the increase of CO and H2 content. By adjusting the amount of water vapor and the pyrolysis temperature, the pyrolysis atmosphere in the gasifier is controlled, the pyrolysis of siloxane under high temperature conditions is promoted, and the pyrolysis of the main components of the siloxane waste liquid and the conversion into hydrogen and methane, the main components of synthesis gas, are achieved.

[0035] (2) The main components of pyrolysis ash are a non-conductive mixture of amorphous silicon dioxide and coke. High-temperature heat treatment can cause silicon dioxide to react with carbon to form silicon carbide, so that the silicon and carbon elements remaining in the ash can be reused. The reaction process is mainly represented by the following reaction equation:

[0036] SiO2+2C→SiC+CO2 (1)

[0037] SiO2+3C→SiC+2CO (2)

[0038] Reaction (1) can proceed spontaneously when the temperature reaches above 2500°C, and reaction (2) can proceed spontaneously when the temperature reaches above 1500°C. This indicates that a higher carbon-silicon ratio is conducive to lowering the formation temperature of silicon carbide. The pyrolysis and gasification process converts a large amount of carbon elements into synthesis gas components. Therefore, it is necessary to add a carbon source to the pyrolysis ash to promote the formation of silicon carbide.

[0039] (3) Electric pulse Joule thermal flash evaporation utilizes the Joule heating effect of electric current to allow the current generated by the instantaneous discharge of the capacitor to pass through the material. According to Joule's law, the material itself generates a large amount of heat at the moment of discharge, and the heat generation area is concentrated, which can heat the temperature of this area from room temperature to above 2500°C within tens of milliseconds, reaching the spontaneous generation temperature range of silicon carbide materials; when the capacitor is completely discharged, no current passes through the material. At this time, the material itself no longer generates heat, and the heated area quickly dissipates heat through air convection, so that its temperature returns to room temperature within a few seconds.

[0040] By adding conductive carbon black to the pyrolysis ash, the conductivity of the material is not only improved, but also the carbon black as a carbon source greatly promotes the reaction of silicon dioxide to silicon carbide. By adjusting the capacitor charging voltage, the energy input to the flash circuit material area can be accurately controlled, and the material heating temperature can be controlled under the condition of rapid response at the millisecond scale to reach the silicon carbide generation temperature range.

[0041] Based on the above principle, the yield and carbon conversion rate of pyrolysis synthesis gas of organic siloxane waste liquid are improved, and the pyrolysis ash and conductive carbon black materials are precisely heated at high temperature in milliseconds through the Joule thermal flash evaporation method, so that the silicon element in the pyrolysis ash is quickly and efficiently converted into high-value-added carbon-silicon composite materials, achieving waste reduction and control in the disposal process.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] (1) The present invention utilizes all components of organic siloxane waste liquid as resources, effectively controlling the migration and utilization pathways of major elements such as carbon, hydrogen, oxygen and silicon;

[0044] (2) The present invention precisely controls the pyrolysis process of organic siloxane waste liquid, and improves the pyrolysis performance and carbon conversion rate of siloxane by utilizing the weak oxidizing property of water vapor to obtain high-content synthesis gas;

[0045] (3) The present invention further utilizes the by-product ash of gasification at a high value, synthesizes SiC-graphene composite materials through a high-temperature heat treatment method, realizes no waste generation in the whole process, and improves the added value of the entire technical solution;

[0046] (4) The present invention utilizes a direct flash electric heating process to heat the gasified ash, and the input electric energy is almost entirely used for high-temperature pyrolysis of the material, which has the characteristics of short processing time and high energy utilization rate;

[0047] (5) The method of the present invention has simple process, convenient raw material source, high energy utilization rate and good economic benefit. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 A schematic diagram of a process flow of a method for recycling siloxane waste liquid by staged pyrolysis provided in a specific embodiment of the present invention;

[0049] Figure 2 A schematic diagram of a staged pyrolysis resource recovery device for siloxane waste liquid provided in a specific embodiment of the present invention.

[0050] In the figure: 1- inert gas cylinder (gas source); 2- organic siloxane waste liquid storage tank; 3- material pump; 4- material heater; 5- water storage tank; 6- water pump; 7- steam generator; 8- pyrolysis gasification furnace; 9- ash filter; 10- ball mill; 11- Joule heat reactor. DETAILED DESCRIPTION

[0051] The following embodiments are only listed as examples of the implementation of the present invention and do not constitute a limitation to the present invention. Any modification and optimization based on the essence and concept of the present invention belong to the protection scope of the present invention.

[0052] The specific embodiment of the present invention provides a method for recycling siloxane waste liquid by pyrolysis. Figure 1 As shown, the following steps are included:

[0053] (1) preheating the gasifier to 600-900° C., using nitrogen, argon or helium as a carrier gas and purging to fully replace the air in the gasifier during the heating process and before pumping in the siloxane waste liquid, and maintaining the reaction residence time in the gasifier at 60-600 seconds;

[0054] (2) When the gasifier reaches the set temperature, the siloxane waste liquid containing any one or more components such as dimethyldiethoxysilane, hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, etc. is preheated and atomized and evaporated at a constant flow rate, and then mixed with water vapor at a mass ratio of 1:1.0 to 3.0 and pumped into the gasifier, followed by a pyrolysis reaction. After purification by a gas filter, a synthesis gas product is obtained, and pyrolysis ash is collected from the gasifier and the filter;

[0055] (3) After drying for 24 hours, the pyrolysis ash is uniformly mixed with carbon black and compacted to make the material resistivity 2.51-200.96 Ω·cm, and the material is placed in a Joule heat reactor at 0.5-1.5 g / F, and then the mixed ash is preheated and discharged at a voltage of 20-30 V and flash heated and discharged at a voltage of 100-170 V by pulse discharge to complete the reaction, and finally a silicon carbide-graphene composite material is obtained;

[0056] To achieve the above method, the present invention provides a system for efficient pyrolysis and resource disposal of siloxane waste liquid, such as Figure 2As shown, the system specifically includes: a material pump, a material preheating device, a pyrolysis gasification furnace reactor, an ash filter, a ball mill, and a Joule heat reactor. Among them, a material preheating device is set at the front end of the pyrolysis gasification furnace reactor. After the material is pumped into the preheating device at a constant flow rate by the material pump to achieve preheating, it is atomized at the outlet and mixed with water vapor in a constant proportion before entering the pyrolysis gasification furnace reactor. An ash filter is set at the rear end to collect the ash produced by pyrolysis; after the ash is collected, it is transferred into the ball mill and evenly mixed with conductive carbon black, and then placed in the Joule heat reactor for disposal. The Joule heat reactor consists of a high-voltage power supply, a control system, a high-voltage capacitor, a material discharge heating tube, and a discharge electrode. The high-voltage capacitor capacity is 90mF, and it can be controlled by the control system to achieve discharge with a maximum current of 600A at different voltages; the material discharge heating tube is made of quartz and can be replaced. The ash material to be disposed is compacted after being loaded into the heating tube, and graphite plugs are added at both ends to contact the discharge electrode.

[0057] Embodiment 1:

[0058] The elemental analysis of the organic siloxane waste liquid used in this example was obtained by industrial analysis and ICP-OES spectroscopy, and the main element contents are shown in the following table:

[0059] Table 1 Element analysis results of organosiloxane waste liquid

[0060]

[0061] Through gas chromatography-mass spectrometry detection, it can be known that the waste liquid sample is a mixture of various organic siloxanes such as dimethyldiethoxysilane, hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, and dodecamethylcyclohexasiloxane.

[0062] (1) preheating the gasifier to 900° C., using nitrogen as a carrier gas and purging to fully replace the air in the gasifier during the heating process and before pumping in the siloxane waste liquid, and maintaining the reaction residence time in the gasifier for 60 seconds;

[0063] (2) When the gasifier reaches the set temperature, the siloxane waste liquid is preheated, atomized and evaporated at a constant flow rate, mixed with water vapor at a mass ratio of 1:2.0, and then pumped into the gasifier, whereupon a pyrolysis reaction occurs, and a synthesis gas product is obtained after purification by a gas filter, and pyrolysis ash is collected from the gasifier and the filter;

[0064] (3) After drying for 24 hours, the pyrolysis ash was uniformly mixed with carbon black, ball-milled, and filled into a quartz tube with graphite plugs at both ends at a material-capacitor ratio of 1.0 g / F and compacted to make the material resistivity 2.51 Ω·cm. The ash was placed in a Joule thermal reactor, and then the mixed ash was preheated and discharged at a voltage of 20 V and flash heated and discharged at a voltage of 170 V by pulse discharge to complete the reaction, and finally a silicon carbide-graphene composite material was obtained.

[0065] Analyze the test results:

[0066] A 10L aluminum foil gas bag was used to collect the filtered synthesis gas, and a gas chromatograph was used to detect the synthesis gas components and the contents of the corresponding components. The total synthesis gas yield was calculated to be 40.91mmol / g[waste liquid], the carbon conversion rate was 72.99%, and the hydrogen volume content was 42.82%. Powder XRD was used to characterize the composite material after flash heating, and the characteristic peaks of graphene and 3C-SiC were observed in the obtained diffraction spectrum, among which the characteristic peak intensity value of the (1 1 1) crystal plane of 3C-SiC was 862037cps.

[0067] Example 2

[0068] The siloxane waste liquid described in this embodiment is the same as that described in Example 1.

[0069] (1) preheating the gasifier at 800° C., using argon as a carrier gas and purging to fully replace the air in the gasifier during the heating process and before pumping in the siloxane waste liquid, and maintaining the reaction residence time in the gasifier at 150 seconds;

[0070] (2) When the gasifier reaches the set temperature, the siloxane waste liquid is preheated, atomized and evaporated at a constant flow rate, mixed with water vapor at a mass ratio of 1:1.0, and then pumped into the gasifier, whereupon a pyrolysis reaction occurs, and a syngas product is obtained after purification by a gas filter, and pyrolysis ash is collected from the gasifier and the filter;

[0071] (3) After drying for 24 hours, the pyrolysis ash is uniformly mixed with carbon black, and filled into a quartz tube with graphite plugs at both ends at a material-capacitor ratio of 0.5 g / F and compacted to make the material resistivity 10.15 Ω·cm. The ash is placed in a Joule thermal reactor, and then the mixed ash is preheated and discharged at a voltage of 30 V and flash heated and discharged at a voltage of 150 V by pulse discharge to complete the reaction, and finally a silicon carbide-graphene composite material is obtained.

[0072] Analyze the test results:

[0073] A 10L aluminum foil gas bag was used to collect the filtered synthesis gas, and a gas chromatograph was used to detect the synthesis gas components and the contents of the corresponding components. The total synthesis gas yield was calculated to be 18.49 mmol / g [waste liquid], the carbon conversion rate was 37.81%, and the hydrogen volume content was 35.20%. Powder XRD was used to characterize the composite material after flash heating, and the characteristic peaks of graphene and 3C-SiC were observed in the obtained diffraction spectrum, among which the characteristic peak intensity value of the (1 1 1) crystal plane of 3C-SiC was 553704 cps.

[0074] Example 3

[0075] The siloxane waste liquid described in this embodiment is the same as that described in Example 1.

[0076] (1) preheating the gasifier at 700° C., using helium as a carrier gas and purging to fully replace the air in the gasifier during the heating process and before pumping in the siloxane waste liquid, and maintaining the reaction residence time in the gasifier for 300 seconds;

[0077] (2) When the gasifier reaches the set temperature, the siloxane waste liquid is preheated, atomized and evaporated at a constant flow rate, mixed with water vapor at a mass ratio of 1:2.0, and then pumped into the gasifier, whereupon a pyrolysis reaction occurs, and a synthesis gas product is obtained after purification by a gas filter, and pyrolysis ash is collected from the gasifier and the filter;

[0078] (3) After drying for 24 hours, the pyrolysis ash was uniformly mixed with carbon black, and filled into a quartz tube with graphite plugs at both ends at a material-capacitor ratio of 1.5 g / F and compacted to make the material resistivity 53.65 Ω·cm. The ash was placed in a Joule thermal reactor, and then the mixed ash was preheated and discharged at a voltage of 20 V and flash heated and discharged at a voltage of 130 V by pulse discharge to complete the reaction, and finally a silicon carbide-graphene composite material was obtained.

[0079] Analyze the test results:

[0080] A 10L aluminum foil gas bag was used to collect the filtered synthesis gas, and a gas chromatograph was used to detect the synthesis gas components and the contents of the corresponding components. Calculation showed that the total synthesis gas yield was 32.01mmol / g[waste liquid], the carbon conversion rate was 73.30%, and the hydrogen volume content was 28.08%. Powder XRD was used to characterize the composite material after flash heating, and the characteristic peaks of graphene and 3C-SiC were observed in the obtained diffraction spectrum, among which the characteristic peak intensity value of the (1 1 1) crystal plane of 3C-SiC was 362845cps.

[0081] Example 4

[0082] The siloxane waste liquid described in this embodiment is the same as that described in Example 1.

[0083] (1) preheating the gasifier at 600° C., using nitrogen as a carrier gas and purging to fully replace the air in the gasifier during the heating process and before pumping in the siloxane waste liquid, and maintaining the reaction residence time in the gasifier at 600 seconds;

[0084] (2) When the gasifier reaches the set temperature, the siloxane waste liquid is preheated, atomized and evaporated at a constant flow rate, mixed with water vapor at a mass ratio of 1:3.0, and then pumped into the gasifier, whereupon a pyrolysis reaction occurs, and a syngas product is obtained after purification by a gas filter, and pyrolysis ash is collected from the gasifier and the filter;

[0085] (3) After drying for 24 hours, the pyrolysis ash was evenly mixed with carbon black, and filled into a quartz tube with graphite plugs at both ends at a material-capacitor ratio of 1.0 g / F and compacted to make the material resistivity 200.96 Ω·cm. The ash was placed in a Joule thermal reactor, and then the mixed ash was preheated and discharged at a voltage of 30 V and flash heated and discharged at a voltage of 100 V by pulse discharge to complete the reaction, and finally a silicon carbide-graphene composite material was obtained.

[0086] Analyze the test results:

[0087] A 10L aluminum foil gas bag was used to collect the filtered synthesis gas, and a gas chromatograph was used to detect the synthesis gas components and the contents of the corresponding components. The total synthesis gas yield was calculated to be 19.59 mmol / g [waste liquid], the carbon conversion rate was 43.83%, and the hydrogen volume content was 29.63%. Powder XRD was used to characterize the composite material after flash heating, and the characteristic peaks of graphene and 3C-SiC were observed in the obtained diffraction spectrum, among which the characteristic peak intensity value of the (1 1 1) crystal plane of 3C-SiC was 221583 cps.

[0088] Comparative Example 1

[0089] Referring to Specific Example 1, except that water vapor is not added, other material amounts, reaction conditions and operation procedures remain the same as in Example 1.

[0090] Comparative Example 2

[0091] Referring to Specific Example 1, except that conductive carbon black is not added to adjust the conductivity of the gasified ash, other material amounts, reaction conditions and operation procedures remain the same as those in Example 1.

[0092] Performance Analysis:

[0093] The operation and test were carried out in the same manner. The results of Comparative Example 1 were calculated to show that the total yield of synthesis gas was 4.96 mmol / g [waste liquid], the carbon conversion rate was 11.86%, but the carbon monoxide content was significantly reduced, and the volume content of the large molecular weight C3+ component increased from less than 0.20% to 3.27%; the characteristic peaks of graphene and 3C-SiC can still be observed in the powder XRD diffraction spectrum, among which the characteristic peak intensity value of the (1 1 1) crystal plane of 3C-SiC is 669529 cps.

[0094] In Comparative Example 2, the total synthesis gas yield is not less than 40 mmol / g [waste liquid], the carbon conversion rate is not less than 70%, and the hydrogen volume content is not less than 40%; however, the preheating and flash heating discharge described in step (3) cannot be carried out, and the powder XRD diffraction spectrum of the obtained material does not contain graphene and 3C-SiC characteristic peaks.

[0095] Through the analysis results of each embodiment and comparative example, it can be seen that the syngas production efficiency and carbon conversion rate of comparative example 1 decreased, and the SiC content in the composite material obtained by flash evaporation decreased; comparative example 2 could not achieve electric pulse flash heating, resulting in no composite material being generated. The above results show that water vapor pyrolysis can simultaneously promote the pyrolysis of siloxane waste liquid, increase the syngas content, and improve the quality of the material obtained by flash evaporation. The regulation of the resistivity of the material by conductive carbon black directly determines whether electric pulse flash heating can be performed. Therefore, using water vapor to assist pyrolysis and using conductive carbon black to regulate the resistance of the pyrolysis ash can obtain better waste liquid pyrolysis efficiency and composite material yield.

[0096] Through the analysis of each embodiment, it can be known that the two-step thermal conversion method proposed in the present invention can realize the pyrolysis conversion of organic siloxane waste liquid and prepare two products, namely synthesis gas and silicon carbide-graphene composite materials. The method for graded resource utilization of organic siloxane waste liquid based on the two-step thermal conversion method provided by the present invention makes full use of the carbon and silicon elements in this type of waste liquid, reducing the carbon emission problems and secondary ash generation problems in the traditional pyrolysis and incineration process. At the same time, the output synthesis gas product can be used for hydrogen energy production and organic matter synthesis through conversion reactions, Fischer-Tropsch synthesis reactions, etc.; the silicon carbide-graphene composite material prepared by thermal treatment of ash can be used as a new functional material for high-performance electrode material preparation and other high value-added fields. Therefore, the invention is a technology for the disposal and resource utilization of organic silicon waste liquid with industrial application and economic benefit prospects.

[0097] In addition, after reading the above description of the present invention, various types of applications, supplements, modifications, and variations made by technicians in this field to the present invention without departing from the connotation and scope of the present invention shall all fall within the scope defined by the claims attached to this application.

Claims

1. A method for recycling siloxane waste liquid by staged pyrolysis. It is characterized in that include: (1) preheating and atomizing siloxane waste liquid to obtain siloxane waste liquid vapor, mixing the siloxane waste liquid vapor with water vapor to obtain mixed vapor, and hydrolyzing and filtering the mixed vapor under an inert gas atmosphere to obtain synthesis gas and pyrolysis ash; (2) The pyrolysis ash and conductive carbon black are mixed, ball-milled, and compacted to obtain a fixed material, and the fixed material is placed in a Joule heat reactor, and the fixed material is flash-heated by pulse discharge to obtain a silicon carbide-graphene composite material.

2. The method for recycling siloxane waste liquid by staged pyrolysis according to claim 1, It is characterized in that The mass ratio of the siloxane waste liquid vapor to water vapor is 1:1-3.

3. The method for recycling siloxane waste liquid by staged pyrolysis according to claim 1, It is characterized in that The hydrolysis temperature is 600-900° C., and the reaction residence time is 60-600 seconds.

4. The method for recycling siloxane waste liquid by staged pyrolysis according to claim 1, It is characterized in that The components of the siloxane waste liquid include one or more of dimethyldiethoxysilane, hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane and dodecamethylcyclohexasiloxane.

5. The method for recycling siloxane waste liquid by staged pyrolysis according to claim 1, It is characterized in that The resistivity of the fixed material is 2.51-200.96 Ω·cm, and the capacitance ratio of the fixed material to the Joule heat reactor is 0.5-1.5 g / F.

6. The method for recycling siloxane waste liquid by staged pyrolysis according to claim 1, It is characterized in that The voltage of the flash heating is 100-170V.

7. The method for recycling siloxane waste liquid by staged pyrolysis according to claim 1, It is characterized in that Before flash heating, the fixed material is preheated, and the preheating voltage is 20-30V.

8. The method for recycling siloxane waste liquid by staged pyrolysis according to claim 1, It is characterized in that The main component of the obtained synthesis gas is H 2 ,CO,CO 2 , CH 4 , C 2 H 6 , C 2 H 4 , C 3 H 8 , C 3 H 6 One or more of .

9. A device for recycling siloxane waste liquid by staged pyrolysis. It is characterized in that include: A material pretreatment unit, used for preheating and atomizing the siloxane waste liquid to obtain siloxane waste liquid vapor; A water vapor generating unit, used for generating water vapor; A pyrolysis gasification furnace, the top of which is respectively connected to a siloxane waste liquid pretreatment unit and a water vapor generation unit, for mixing siloxane waste liquid vapor with water vapor to obtain mixed vapor, and hydrolyzing the mixed vapor under an inert gas atmosphere to obtain synthesis gas and pyrolysis gas; An ash filter, which is connected to the bottom of the pyrolysis gasifier and is used to filter the pyrolysis gas to obtain pyrolysis ash and discharge the synthesis gas; A ball mill is used to mix the pyrolysis ash collected in the filter with the conductive carbon black and grind them fully to obtain the material to be disposed; The Joule heat reactor is used to compact the material to be disposed to obtain a fixed material, and flash heat the fixed material through pulse discharge to obtain a silicon carbide-graphene composite material.

10. The device for recycling siloxane waste liquid by staged pyrolysis according to claim 9, It is characterized in that The material pre-processing unit comprises: Siloxane waste liquid storage tank, used for storing siloxane waste liquid; A material pump, connected to the siloxane waste liquid storage tank, is used to pump out the siloxane waste liquid at a set flow rate; The material preheating device comprises a vertically arranged material pipeline and a heating device arranged outside the pipeline, wherein the material pipeline is connected to a material pump, and the heating device is used to heat the siloxane waste liquid in the material pipeline to obtain siloxane waste liquid vapor.

Citation Information

Patent Citations

  • Silicon carbide / graphene positive and negative electrode composite materials as well as preparation method and application thereof

    CN113636557A

  • Harmless and recycling method for gasification and high-temperature melting of full-industrial organic hazardous waste

    CN114229800A

  • Method for preparing graphene through carbon black rapid Joule heat and graphene

    CN114735683A

  • Method for efficiently preparing silicon carbide aerogel

    CN118125445A

  • High-temperature clean gasification apparatus and method for achieving high carbon conversion rate of carbonaceous material

    WO2023044858A1

Cited By

  • Method for preparing three-dimensional graphene foam from organic silicon waste liquid, three-dimensional graphene foam and application

    CN121516856A

  • Method for preparing three-dimensional graphene foam from organic silicon waste liquid and three-dimensional graphene foam and application

    CN121516856B

  • Diversified analysis-based silicon removal tail end temperature control adjusting system

    CN121613982A

  • Multivariate analysis based silicon removal end temperature control system

    CN121613982B