Transparent conductive oxide electrode, preparation method thereof and perovskite battery
The transparent conductive oxide electrode was prepared by wet method, and nanoparticles were generated by reacting metal salts with alkalis, which solved the problem of sputtering damage to the perovskite active layer, and achieved a combination of low resistivity and high carrier mobility. And improve the optical and electrical properties of perovskite batteries.
Patent Information
- Application Number
- CN202411389919.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-10-08
AI Technical Summary
The existing transparent conductive oxide electrodes are prone to damage the perovskite active layer during sputtering preparation, resulting in a degradation of battery performance and difficulty in having both low resistivity and high carrier mobility.
Nanoparticles are generated by reacting metal salts with alkalis, transparent conductive oxide electrodes are prepared by wet method, and amorphous structures are formed using conductive elements, anchoring elements and structural elements to avoid energy damage and improve carrier mobility.
It achieves a combination of low resistivity and high carrier mobility, and ensures the transmittance of the infrared region, avoids substrate damage and shortens the preparation time.
Smart Images

Figure CN118900610A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solar cells, and in particular to a transparent conductive oxide electrode and a preparation method thereof, and a perovskite cell. Background Art
[0002] Perovskite solar cells have attracted great attention due to their unique optoelectronic properties and simple process and low cost. In just a few years after the emergence of perovskite solar cells, their efficiency has achieved rapid development. The top transparent electrode has a huge impact on the performance of semi-transparent perovskite and tandem solar cells. For semi-transparent perovskite and tandem solar cells, the ideal top transparent electrode should have high transmittance, low resistance, high conductivity, good chemical stability and the ability to be prepared at low temperature. So far, a variety of transparent electrodes have been used in semi-transparent perovskite and tandem solar cells, such as transparent conductive oxides. Transparent conductive oxides have good optoelectronic properties and stability, but are often prepared by sputtering, which can easily damage the perovskite active layer during the sputtering process.
[0003] It should be noted that the above content is not necessarily prior art, nor is it intended to limit the scope of patent protection of this application. Summary of the invention
[0004] The embodiments of the present application provide a transparent conductive oxide electrode and a preparation method thereof and a perovskite battery to solve or alleviate one or more of the technical problems raised above.
[0005] A first aspect of an embodiment of the present application provides a method for preparing a transparent conductive oxide electrode, comprising: A metal salt is reacted with an alkali, and then a precipitate is sintered to obtain nanoparticles; dispersing the nanoparticles in a solvent to prepare a nanoparticle dispersion; The nanoparticle dispersion is prepared into a transparent conductive oxide electrode on a substrate by a wet method; Wherein, the metal salt is used to provide a conductive element, an anchoring element and a structural element; the conductive element includes at least one of Sn, In and Ce; The anchor element includes at least one of Ga, Al, Zr, Hf, and Ti; The structural element includes at least one of Zn and Cd.
[0006] In the first aspect of the embodiment of the present application, a transparent conductive oxide electrode is prepared by a wet method. This preparation method is gentle and will not cause any energy damage to the substrate due to the preparation of the transparent conductive oxide electrode. In addition, the transparent conductive oxide electrode can have both low resistivity and high carrier mobility. In addition, the presence of anchoring elements can also ensure the transmittance in the IR region (infrared). This preparation method has flexible components and a shorter preparation time. The final material can be obtained from the raw materials within one day.
[0007] The second aspect of the embodiment of the present application provides a transparent conductive oxide electrode, which is prepared by the preparation method described in the first aspect of the embodiment of the present application. Thus, the transparent conductive oxide electrode is prepared by a wet method without damaging the substrate, and the transparent conductive oxide electrode has both low resistivity and high carrier mobility, and can also ensure transmittance in the IR region.
[0008] The third aspect of the embodiment of the present application provides a perovskite cell, comprising the transparent conductive oxide electrode described in the second aspect of the embodiment of the present application. Thus, the efficiency of the perovskite cell is improved by combining excellent optical and electrical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in the present application and should not be regarded as limiting the scope of the present application.
[0010] Figure 1 It is a schematic diagram of the structure of a single-junction perovskite cell provided in an embodiment of the present application.
[0011] Figure 2 It is a schematic diagram of the structure of the stacked perovskite battery provided in the embodiment of the present application.
[0012] Description of reference numerals: 1-back electrode layer; 2-transparent conductive oxide electrode; 3-electron transport layer; 4-passivation layer; 5-perovskite active layer; 6-hole transport layer; 7-transparent conductive electrode layer; 8-transparent substrate; 9-composite tunneling layer; 10-crystalline silicon cell. DETAILED DESCRIPTION
[0013] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings. In the accompanying drawings, for clarity, the sizes of layers, regions, elements and their relative sizes may be exaggerated. Wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limitations on the present application. It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments can be combined with each other.
[0014] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "directly adjacent to ...", "directly connected to" or "directly coupled to" other elements or layers, there is no intervening element or layer. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings of the present disclosure, the first element, component, region, layer or part discussed below can be represented as the second element, component, region, layer or part. And when the second element, component, region, layer or part is discussed, it does not mean that the present disclosure necessarily has the first element, component, region, layer or part.
[0015] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0016] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0017] In the present application, when it comes to a numerical interval (i.e., a numerical range), unless otherwise specified, the distribution of the optional numerical values in the numerical interval is considered to be continuous, and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to an integer in the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints, which is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be merged. In other words, unless otherwise specified, the numerical range disclosed in the present application should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows for broadly including quantitative intervals such as percentage intervals, ratio intervals, and ratio intervals.
[0018] The following provides an explanation of the terms used in this application.
[0019] TCO materials: Transparent conductive oxide materials are a type of thin film material with high visible light transmittance and low resistivity, and are widely used in optoelectronic devices such as liquid crystal displays, touch screens, flexible OLED screens, optical waveguide components, and thin film solar cells. TCO materials mainly include oxides such as CdO, In2O3, SnO2, and ZnO and their corresponding composite multi-compound semiconductor materials. They have high transmittance and low resistivity.
[0020] In the related art, the silver nanowire transparent electrode has good photoelectric performance, but poor stability. It is easy to react with the halide ions in the perovskite, resulting in deterioration of the device performance, and it is easy to be oxidized and corroded in the air. Ultra-thin metal electrodes often cannot have high conductivity and optical transmittance at the same time, and a buffer layer needs to be introduced to promote its uniform growth. There is also a problem of poor stability. The stability of carbon-based transparent electrodes is very strong, but the photoelectric performance needs to be improved. Transparent conductive oxides have good photoelectric properties and stability, but are often prepared by sputtering, which easily damages the perovskite active layer during the sputtering process. To avoid this situation, a buffer layer needs to be introduced. Specifically, the following problems exist in the sputtering process of transparent conductive oxides: In order to obtain a high-quality dense film, the traditional physical vapor deposition (PVD) sputtering film requires a certain sputtering power, and the plasma sputtering particles carrying a large amount of energy may cause certain damage to the perovskite active layer substrate, thereby damaging the battery performance. Based on this, a protective layer needs to be introduced on the perovskite active layer substrate in advance.
[0021] For some low-density materials, such as tungsten-doped indium oxide (IWO) and tin-doped indium oxide (ICO), the tap density is only 60%, which cannot be rolled into high-density PVD targets. The firing of plasma deposition (RPD) targets also requires powder making and other process steps, and the preparation time is at least 2 weeks. Therefore, the preparation of transparent conductive oxides by sputtering requires the corresponding target material to be obtained first, and the preparation cycle is long.
[0022] In addition, for TCO materials with a crystalline structure, under certain resistivity conditions, the mobility is inversely proportional to the carrier concentration, but the resistivity is directly proportional to the carrier concentration, which means that when TCO materials with a crystalline structure are used as top electrode materials, it is difficult to have both low resistivity and high carrier mobility at the same time.
[0023] Accordingly, the embodiments of the present application provide a transparent conductive oxide electrode, a preparation method and a related battery. Based on this, at least some of the problems in the related art are solved. See below for details.
[0024] A first aspect of an embodiment of the present application provides a method for preparing a transparent conductive oxide electrode, comprising: A metal salt is reacted with an alkali, and then a precipitate is sintered to obtain nanoparticles; dispersing the nanoparticles in a solvent to prepare a nanoparticle dispersion; The nanoparticle dispersion is prepared into a transparent conductive oxide electrode on a substrate by a wet method; Wherein, the metal salt is used to provide a conductive element, an anchoring element and a structural element; the conductive element includes at least one of Sn, In and Ce; The anchor element includes at least one of Ga, Al, Zr, Hf, and Ti; The structural element includes at least one of Zn and Cd.
[0025] In the first aspect of the embodiments of the present application, a transparent conductive oxide electrode is prepared by a wet method. This preparation method is gentle and will not cause any energy damage to the substrate due to the preparation of the transparent conductive oxide electrode. In the embodiments of the present application, a metal salt solution is reacted with an alkali to obtain a metal hydroxide compound, which is then sintered to form nanoparticles. The nanoparticle dispersion is formed on the substrate by a wet method. In addition, the formed transparent conductive oxide electrode includes a conductive element oxide doped with a structural element and an anchoring element, and also contains a very small amount of conductive element oxide, anchoring element metal salt oxide and structural element metal salt oxide, and the nanoparticles exist in an amorphous form. Specifically, the atomic radius difference between the conductive element and the structural element is large, so that an amorphous structure is formed in the transparent conductive oxide electrode; for the amorphous TCO film, since the conduction band of the conductive element therein is fully extended in width, electrons can be transported in a very wide conduction band and are not affected by the long-range disordered grain boundaries in the amorphous. Thus, the seesaw problem of carrier concentration and mobility is solved, so that the transparent conductive oxide electrode can have both low resistivity and high carrier mobility; in addition, the anchor element can be doped into the conductive element oxide to control the carrier concentration not to be too high so as to affect the transmittance in the IR region (infrared). This preparation method has flexible components and shorter preparation time, and the final material can be obtained from the raw materials within one day.
[0026] In some embodiments, in the method for preparing the transparent conductive oxide electrode, the metal salt may include a conductive element metal salt, an anchor element metal salt, and a structural element metal salt to provide a conductive element, an anchor element, and a structural element.
[0027] It is worth noting that the conductive elements include at least one of Sn, In, and Ce; the conductive elements are all elements with relatively large atomic nuclei, and all have the form of 5s4p electronic orbits, and the s orbits are fully extended, resulting in a very wide conduction band, and electrons can be transported in a very wide conduction band, and are not affected by the long-range disordered grain boundaries in amorphous materials. For example, the s orbital radius of the In outer electron layer arrangement is relatively large, so that the orbits in the next adjacent In-In bonds overlap, and the conduction band is fully extended in width, and electrons can be transported in a very wide conduction band, and are not affected by the long-range disordered grain boundaries in amorphous materials.
[0028] The anchoring element includes at least one of Ga, Al, Zr, Hf, and Ti; the anchoring elements are all selected from elements with relatively small nuclei (relative to conductive elements) and elements of the same group as Ti, and their electronic configuration range is not as wide as that of conductive elements. Their presence will cause blockage in electron transfer, thereby playing a role in controlling carrier concentration.
[0029] The structural element includes at least one of Zn and Cd. The difference between the atomic nucleus radius of the structural element and the radius of the conductive element is large, which is conducive to forming an amorphous structure.
[0030] In some embodiments, in the preparation method of the transparent conductive oxide electrode, the molar fraction of the conductive element in the conductive element metal salt is 30 to 99 parts, the molar fraction of the anchor element in the anchor element metal salt is 1 to 30 parts, for example, 1 part, 5 parts, 10 parts, 15 parts, 25 parts, 30 parts, etc.; the molar fraction of the structural element in the structural element metal salt is 1 to 30 parts, for example, 1 part, 5 parts, 10 parts, 15 parts, 25 parts, 30 parts, etc. Thus, on the basis of forming an amorphous state, the carrier concentration is guaranteed and good infrared light transmittance is obtained.
[0031] Furthermore, the types of metal salts include but are not limited to hydrochlorides, nitrates, carbonates, etc. The base used may include strong bases, medium-strong bases, and weak bases, such as NaOH, Mg(OH)2, and the like.
[0032] Preferably, the molar number of the conductive element in the conductive element metal salt is 50 to 95 parts, for example, 50 parts, 75 parts, 80 parts, 95 parts, etc.; the molar number of the anchor element in the anchor element metal salt is 1 to 5 parts, for example, 1 part, 2 parts, 5 parts, etc. Thus, the carrier conductivity is further improved.
[0033] Further, the sum of the molar fractions of the conductive element in the conductive element metal salt, the anchor element in the anchor element metal salt, and the structural element in the structural element metal salt is 100 parts. For example, the sum of the molar fractions of the conductive element in the conductive element metal salt, the anchor element in the anchor element metal salt, and the structural element in the structural element metal salt is 100 parts, the molar fraction of the conductive element in the conductive element metal salt is 50 to 95 parts, the molar fraction of the anchor element in the anchor element metal salt is 1 to 30 parts, and the molar fraction of the structural element in the structural element metal salt is 1 to 30 parts.
[0034] In some embodiments, the method for preparing the transparent conductive oxide electrode, the wet method includes at least one of coating, spin coating, and scraping. For example, the nanoparticle dispersion can be spin-coated on the substrate by spin coating, and the excess solvent can be removed by drying or vacuum extraction, so that the nanoparticles are evenly distributed on the substrate. In this way, no energy impact is used, avoiding damage to the substrate during the preparation of the transparent conductive oxide electrode.
[0035] In some embodiments, the preparation method of the transparent conductive oxide electrode, the sintering of the precipitate to obtain nanoparticles includes: the sintering temperature is 200°C to 500°C, for example, the temperature is 200°C, 300°C, 400°C, 500°C, etc.; the sintering time is 2h to 8h, for example, 2h, 4h, 5h, 7h, 8h, etc.; the sintering atmosphere is air, oxygen, or a mixed gas of argon and oxygen. Thus, the transformation from the precipitate to the nanoparticles is completed.
[0036] In some embodiments, in the method for preparing the transparent conductive oxide electrode, the solvent is at least one of deionized water, ethanol, and isopropanol, thereby facilitating obtaining a uniformly dispersed dispersion.
[0037] In some embodiments, in the method for preparing the transparent conductive oxide electrode, the concentration of the nanoparticle dispersion is 10 mg / mL to 50 mg / mL, for example, 10 mg / mL, 20 mg / mL, 30 mg / mL, 40 mg / mL, 50 mg / mL, etc. This facilitates the subsequent wet method to prepare a uniform thin film.
[0038] In some embodiments, the method for preparing the transparent conductive oxide electrode further includes: annealing the transparent conductive oxide electrode, thereby partially crystallizing the transparent conductive oxide electrode, reducing grain boundaries, and making the twin directions therein more uniform.
[0039] Furthermore, the annealing treatment includes: The annealing atmosphere is an inert gas atmosphere, where the inert gas refers to an atmosphere that does not participate in the reaction during the annealing process, for example, it may be N2, Ar or a vacuum atmosphere.
[0040] The annealing temperature is 50° C. to 150° C., for example, 50° C., 80° C., 100° C., 120° C., 150° C., etc., thereby avoiding damage to the battery while performing stress relief annealing.
[0041] Furthermore, the annealing time can be 1 min to 30 min, for example, 1 min, 10 min, 15 min, 20 min, 25 min, 30 min, etc.
[0042] In some embodiments, in the method for preparing the transparent conductive oxide electrode, the substrate includes a perovskite active layer, a crystalline silicon cell, a cadmium telluride thin film solar cell (CdTe cell) or a copper indium gallium selenide solar cell (CIGS cell). Thus, the top electrode and bottom electrode of various cells can be obtained. For example, after preparing a transparent conductive oxide electrode on the perovskite active layer, other operations can be superimposed to prepare a perovskite single junction cell. For another example, after preparing a transparent conductive oxide electrode on a crystalline silicon cell, other operations can be superimposed to prepare a perovskite stacked cell.
[0043] In some embodiments, in the method for preparing the transparent conductive oxide electrode, the thickness of the transparent conductive oxide electrode is 30 nm to 200 nm, for example, 30 nm, 80 nm, 130 nm, 200 nm, etc. Therefore, within this range, both excellent optical properties and electrical properties are achieved, specifically, the refractive index, reflectivity, carrier concentration and mobility are all good.
[0044] Preferably, the thickness of the transparent conductive oxide electrode is 50 nm to 70 nm, thereby achieving better optical and electrical properties.
[0045] The second aspect of the embodiment of the present application provides a transparent conductive oxide electrode, which is prepared by the preparation method described in the first aspect of the embodiment of the present application. Thus, the transparent conductive oxide electrode is prepared by a wet method without damaging the substrate, and the transparent conductive oxide electrode has both low resistivity and high carrier mobility, and can also control the carrier concentration not to be too high so as to affect the transmittance in the IR region.
[0046] The third aspect of the embodiment of the present application provides a perovskite cell, comprising the transparent conductive oxide electrode described in the second aspect of the embodiment of the present application. Thus, the efficiency of the perovskite cell is improved by combining excellent optical and electrical properties.
[0047] In some embodiments, in the perovskite cell, the perovskite cell is a perovskite single junction cell, and the transparent conductive oxide electrode of the second aspect of the embodiment serves as the top electrode of the perovskite single junction cell.
[0048] In some embodiments, in the perovskite cell, the perovskite cell is a perovskite single junction cell, and the transparent conductive oxide electrode of the second aspect of the embodiment serves as the bottom electrode of the perovskite single junction cell.
[0049] In some embodiments, in the perovskite cell, the perovskite cell is a perovskite single junction cell, and the transparent conductive oxide electrode of the second aspect of the embodiment is used as the top electrode of the perovskite single junction cell. Also, the transparent conductive oxide electrode of the second aspect of the embodiment is used as the bottom electrode of the perovskite single junction cell.
[0050] In a specific embodiment, see Figure 1 , Figure 1 : is a schematic diagram of the structure of a single-junction perovskite cell provided in an embodiment of the present application, wherein a transparent conductive electrode layer 7, a hole transport layer 6, a perovskite active layer 5, a passivation layer 4, an electron transport layer 3, a transparent conductive oxide electrode 2 and a back electrode layer 1 are sequentially stacked on a transparent substrate 8. It can be understood that the transparent conductive electrode layer 7 of the transparent substrate 8 can be prepared by sputtering.
[0051] In some embodiments, the perovskite cell is a perovskite stack cell; the transparent conductive oxide electrode obtained by the above preparation method serves as the top electrode of the perovskite stack cell.
[0052] Furthermore, the perovskite tandem cell also includes a crystalline silicon cell, a cadmium telluride thin-film solar cell (CdTe cell) or a copper indium gallium selenide solar cell (CIGS cell). For example, the crystalline silicon cell is the bottom cell and the perovskite cell is the top cell. In this case, the transparent conductive oxide electrode obtained by the above preparation method can be located on the top cell.
[0053] In some specific embodiments, see Figure 2 , Figure 2 It is a schematic diagram of the structure of the stacked perovskite battery provided in an embodiment of the present application, wherein a composite tunneling layer 9, a hole transport layer 6, a perovskite active layer 5, a passivation layer 4, an electron transport layer 3, a transparent conductive oxide electrode 2 and a back electrode layer 1 are sequentially stacked on the crystalline silicon battery 10.
[0054] Hereinafter, exemplary embodiments according to the present application will be described in more detail with reference to the accompanying drawings. It should be noted that these exemplary embodiments can be implemented in many different forms and should not be construed as being limited to the embodiments described herein.
[0055] Example 1 A method for preparing a single-junction perovskite battery is provided. (1) A glass substrate (with an initial square resistance of about 15 Ω / sq) coated with a 150 nm thick ITO film was provided as a transparent substrate. The ITO transparent substrate was ultrasonically cleaned with a detergent, deionized water, ethanol, and acetone for 20 min each. Nitrogen was then used to blow dry the surface of the transparent substrate. The transparent substrate was then sent to a UV-ozone cleaner for 20 min to remove residual organic matter on the surface.
[0056] (2) In a nitrogen-filled glove box, a 0.5 mg / ml 2PACz solution was prepared using (2-(9H-carbazole-9-yl)ethyl)phosphonic acid (2PACz) as the solute and isopropyl alcohol (IPA) as the solvent. The 2PACz solution was spin-coated on a transparent substrate, filtered using a 0.22 μm filter head, and then spin-coated on the transparent substrate at a speed of 5000 rpm / min and an acceleration of 3000 rpm / s. After spin-coating for 30 seconds, the substrate was placed on a hot plate at 100°C for annealing for 5 minutes to form a hole transport layer of a monomolecular layer (SAM) material.
[0057] (3) Formamidine hydroiodide (FAI), lead iodide (PbI2), and cesium iodide (CsI) were weighed to prepare a solution with a concentration of 1.4 M perovskite precursor, 10 wt% PbCl2 and 20 wt% methylamine hydrochloride (MACl) were added as additives, and 0.5 wt% polyethylene dimethacrylate (PEDGMA) was added as a cross-linking agent, and dissolved in a mixed solvent of N,N-dimethylformamide and dimethyl sulfoxide (DMF / DMSO (4:1, v / v)) to obtain FAI. 0.85 MA 0.05 Cs 0.1 Perovskite precursor solution of PbI3.
[0058] (4) Spin-coat the perovskite precursor solution at a speed of 5000 rpm / min and an acceleration of 1000 rpm / s for 50 seconds and apply it on the hole transport layer; during the high-speed spin coating process, add chlorobenzene as an anti-solvent to the spin coating in the last 10 seconds. Then transfer to the annealing hot stage and heat at 150°C for 15 minutes to complete annealing to obtain the perovskite active layer; (5) Deposit a 10nm passivation layer and a 12nm electron transport layer; (6) Preparation of transparent conductive oxide nanoparticles, namely zinc- and gallium-doped indium oxide (In 0.7 Ga 0.2 Zn 0.1 O) Weigh 0.01 mol zinc chloride, 0.02 mol gallium chloride, and 0.07 mol indium chloride to prepare an aqueous solution, wherein the concentration of zinc chloride in the aqueous solution is 0.02 mol / L, the concentration of gallium chloride is 0.04 mol / L, and the concentration of indium chloride is 0.14 mol / L; Under magnetic stirring conditions, 1 mol / L sodium hydroxide solution was added dropwise to the above mixed chloride solution and stirred for about 20 minutes. After the addition was completed, the pH value of the solution was adjusted to 10 and aged for more than 2 hours, filtered, washed, and sintered in an oven at 105°C for 2 hours to obtain transparent conductive oxide nanoparticles.
[0059] (7) Preparation of a transparent conductive oxide electrode on the side of the electron transport layer away from the transparent substrate The transparent conductive oxide nanoparticles were prepared into a transparent conductive oxide nanoparticle dispersion with a concentration of 20 mg / mL, and then spin-coated on the side of the electron transport layer away from the transparent substrate, and the spin coating was continued until the thickness of the transparent conductive oxide electrode was 50 nm.
[0060] (8) Evaporate a 50μm metal grid line as the back electrode layer.
[0061] Embodiments 2 to 5 The rest is the same as Example 1, except that, in step 7, the thicknesses of the transparent conductive oxide electrodes in Examples 2 to 5 are 70 nm, 30 nm, 100 nm, and 200 nm, respectively.
[0062] Examples 6 and 7 The rest is the same as Example 1, except that in step (6), transparent conductive oxide nanoparticles are prepared, and the zinc-doped and gallium-doped indium oxides in Examples 6 and 7 are In 0.95 Ga 0.02 Zn 0.03 O and In 0.4 Ga 0.3 Zn 0.3 O.
[0063] Examples 8 and 9 The rest is the same as Example 1, except that in step (6), transparent conductive oxide nanoparticles are prepared, and in Examples 8 and 9, Ce 0.95 Al 0.02 Cd 0.03 O and Sn 0.95 Zr 0.02 Zn 0.03 O.
[0064] Example 10 A method for preparing a perovskite / crystalline silicon stacked cell is provided. (1) Using chemical vapor deposition, a first i-type amorphous silicon film and an N-type amorphous silicon film are sequentially deposited on the front surface of the single crystal silicon, a second i-type amorphous silicon film and an N-type amorphous silicon film are sequentially deposited on the back surface of the single crystal silicon, and a TCO conductive film is deposited on the back surface of the P-type amorphous silicon film as a second conductive substrate to obtain a crystalline silicon cell; The thickness of the single crystal silicon is 250 μm, the thickness of the first i-type amorphous silicon film and the second i-type amorphous silicon film are 5 nm respectively, the thickness of the N-type amorphous silicon film is 10 nm, and the thickness of the P-type amorphous silicon film is 20 nm. (2) preparing a composite tunneling layer; (3) preparing a hole transport layer, which is the same as step (2) of Example 1; (4) preparing a perovskite photoactive layer, which is the same as steps (3) and (4) of Example 1; (6) Prepare a passivation layer and an electron transport layer, which is the same as step (5) of Example 1.
[0065] (7) Preparation of transparent conductive oxide nanoparticles, namely zinc- and gallium-doped indium oxide, In 0.9 Ga 0.05 Zn 0.05 O; For the operation method, please refer to step 6 of Example 1.
[0066] (8) A transparent conductive oxide electrode was prepared on the front side of the electron transport layer by spin coating the nanoparticles until the thickness of the transparent conductive oxide electrode reached 10 nm.
[0067] (9) After completion, anneal at 200 °C in a nitrogen atmosphere for 30 min.
[0068] (10) Prepare a back electrode, similar to step 8 of Example 1.
[0069] Comparative Example 1 The rest is the same as Example 1, except that step (7) is omitted and step (8) uses a sputtering method to deposit zinc- and gallium-doped indium oxide (In 0.7 Ga 0.2 Zn 0.1 O), with a deposition thickness of 50 nm.
[0070] Test Case The optical and electrical properties of the transparent conductive oxide electrodes of Examples 1 to 5 were tested. The MPPT stability of the transparent conductive oxide electrodes of Examples 1 to 5 was tested. MPPT, which stands for Maximum Power Point Tracker, is used to ensure that the solar cell outputs electrical energy at the maximum efficiency. The solar cell is subjected to a light condition (1000 W / m 2 The MPPT stability test was carried out for 250 h under 200 nm spectral range and the data at 633 nm were selected. The results are shown in Table 1.
[0071] The solar cells of Examples 1 to 10 and Comparative Example 1 were subjected to IV testing using a rapid scanning method. The IV testing conditions were as follows: the ambient humidity was not higher than 70% RH, the ambient temperature was maintained at (25 ± 5) °C, and the irradiation received by the solar cell was 1000 W / m 2 , the results are shown in Table 2.
[0072] Table 1
[0073] It can be seen from Table 1 that as the thickness of the transparent conductive oxide electrode increases from thin to thick, the optical absorption of the transparent conductive oxide electrode to light gradually increases, while the carrier mobility increases, indicating that the electrical sheet resistance gradually decreases. For the performance of the transparent conductive oxide electrode on the device, optics and electricity need to be considered comprehensively. The comprehensive performance of Example 1 and Example 2 is the best, and the corresponding 50nm to 70nm is the optimal thickness.
[0074] Table 2
[0075] Note: Voc-open circuit voltage; Jsc-short circuit current; FF-fill factor; PCE-conversion efficiency.
[0076] It can be seen from Table 2 that Examples 1 to 10 are better than Comparative Example 1, which may be because Comparative Example 1 uses a sputtering method to prepare zinc- and gallium-doped indium oxide, which causes damage to the battery itself. The performance of the batteries of Examples 1 to 5 is basically consistent with the optics and electrical properties of the transparent conductive oxide electrodes thereon. The content of the conductive element in Example 7 is slightly lower, and thus the performance is slightly worse than that of Examples 1 to 6. Example 8 is a perovskite / crystalline silicon stacked battery, and the conversion efficiency is the best in Examples 1 to 7 of zinc- and gallium-doped indium oxide. Compared with Examples 1 to 7, Examples 8 and 9 replaced the types of conductive elements, anchoring elements, and structural elements, and the performance of each battery also maintained a good level.
[0077] It should be noted that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. The orientation words "inside" and "outside" refer to the inside and outside relative to the outline of each component itself. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Therefore, the exemplary term "above..." can include both "above..." and "below..." orientations. The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatial relative descriptions used here are interpreted accordingly.
[0078] It should also be noted that "one embodiment", "another embodiment", "embodiment", etc. mentioned in this application refer to the specific features, structures or characteristics described in conjunction with the embodiment included in at least one embodiment generally described in this application. The same expression appearing in multiple places in the specification does not necessarily refer to the same embodiment. Further, when describing a specific feature, structure or characteristic in conjunction with any embodiment, it is claimed that the realization of such feature, structure or characteristic in conjunction with other embodiments also falls within the scope of this application.
[0079] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0080] It should also be noted that the above are only preferred embodiments of the present application, and the patent protection scope of the present application is not limited thereto. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A method for preparing a transparent conductive oxide electrode, characterized in that: include: A metal salt is reacted with an alkali, and then a precipitate is sintered to obtain nanoparticles; dispersing the nanoparticles in a solvent to prepare a nanoparticle dispersion; The nanoparticle dispersion is prepared into a transparent conductive oxide electrode on a substrate by a wet method; Wherein, the metal salt is used to provide conductive elements, anchoring elements and structural elements; The conductive element includes at least one of Sn, In, and Ce; The anchor element includes at least one of Ga, Al, Zr, Hf, and Ti; The structural element includes at least one of Zn and Cd.
2. The method for preparing a transparent conductive oxide electrode according to claim 1, characterized in that: In terms of molar fractions, the molar fraction of the conductive element in the conductive element metal salt is 30 to 99 parts, the molar fraction of the anchor element in the anchor element metal salt is 1 to 30 parts, and the molar fraction of the structural element in the structural element metal salt is 1 to 30 parts.
3. The method for preparing a transparent conductive oxide electrode according to claim 1, characterized in that: The molar number of the conductive element in the conductive element metal salt is 50 to 95 parts; The molar fraction of the anchor element in the anchor element metal salt is 1 to 5 parts.
4. The method for preparing a transparent conductive oxide electrode according to claim 2 or 3, characterized in that: The sum of the molar parts of the conductive element in the conductive element metal salt, the anchor element in the anchor element metal salt and the structural element in the structural element metal salt is 100 parts.
5. The method for preparing a transparent conductive oxide electrode according to claim 1, characterized in that: The sintering of the precipitate to obtain nanoparticles comprises: The sintering temperature is 200°C to 500°C; The sintering time is 2h to 8h.
6. The method for preparing a transparent conductive oxide electrode according to claim 1, characterized in that: The solvent is at least one of deionized water, ethanol, and isopropanol; The concentration of the nanoparticle dispersion is 10 mg / mL to 50 mg / mL.
7. The method for preparing a transparent conductive oxide electrode according to claim 1, characterized in that: The wet method includes at least one of coating, spin coating, and blade coating.
8. The method for preparing a transparent conductive oxide electrode according to claim 1, characterized in that: The preparation method further comprises: Annealing the transparent conductive oxide electrode; The annealing treatment includes: the atmosphere is an inert gas atmosphere; the annealing temperature is 50° C. to 150° C.
9. The method for preparing a transparent conductive oxide electrode according to claim 1, characterized in that: The substrate includes a perovskite active layer, a crystalline silicon cell, a cadmium telluride thin film solar cell or a copper indium gallium selenide solar cell.
10. The method for preparing a transparent conductive oxide electrode according to claim 9, characterized in that: The thickness of the transparent conductive oxide electrode is 30nm-200nm.
11. The method for preparing a transparent conductive oxide electrode according to claim 10, characterized in that: The thickness of the transparent conductive oxide electrode is 50nm-70nm.
12. A transparent conductive oxide electrode, characterized in that: Prepared according to the method for preparing a transparent conductive oxide electrode according to any one of claims 1 to 11; The transparent conductive oxide electrode includes a conductive element oxide doped with the structural element and the anchor element.
13. A perovskite battery, characterized in that: It comprises a transparent substrate (8), a transparent conductive electrode layer (7), a hole transport layer (6), a perovskite active layer (5), a passivation layer (4), an electron transport layer (3), a transparent conductive oxide electrode (2) and a back electrode layer (1) which are stacked in sequence; Wherein, the transparent conductive oxide electrode (2) comprises the transparent conductive oxide electrode according to claim 12.
Citation Information
Patent Citations
Method for preparing ITO film
CN108109722A
Organic electroluminescent element
JP2004014360A
Substrate with transparent conductive film
JP2012018806A
Method for preparing IGZO particles and method for preparing IGZO film by using the IGZO particles
US20110097842A1