Positive electrode lithium supplement agent and preparation and application thereof
By adopting a double-layer clad structure on the positive electrode lithium supplement agent, and using acid compounds to isolate moisture and carbon dioxide from the carbon layer, the problems of poor air stability and poor conductivity are solved, and the application performance of lithium supplement agents is significantly improved.
Patent Information
- Application Number
- CN202411358112.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-29
AI Technical Summary
The existing positive electrode lithium supplement agents are limited in large-scale applications in lithium-ion batteries due to poor air stability, high surface residual alkali content and poor conductivity.
Using a double-layer clad structure, the first layer is formed of a lithium salt formed by acidic compounds and the residual alkali on the surface, and the second layer is a carbon layer, effectively isolating the reaction between the core of the lithium supplement agent and moisture and carbon dioxide, and reducing the resistivity.
It improves the air stability and conductivity of lithium supplement agents, improves storage, transportation and processing performance, and significantly improves the lithium supplement effect.
Smart Images

Figure CN119050367A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a positive electrode lithium supplement and a preparation and application thereof. Background Art
[0002] Lithium-ion batteries are widely used in various fields due to their high energy density, long cycle life, and environmental friendliness. However, most existing high-capacity materials lose a large amount of active lithium during the first charge and discharge due to the formation of SEI film. This loss will lead to permanent loss of lithium in the positive electrode material, resulting in reduced battery capacity, reduced coulombic efficiency, and poor cycle performance, which limits their widespread use. Lithium replenishment technology is an effective means to improve the above problems because it can compensate for the first irreversible lithium loss in the electrode material, thereby improving the initial coulombic efficiency, cycle capacity, cycle life, and actual energy density of the battery.
[0003] Lithium replenishment methods can be divided into two categories according to the technical route: negative electrode lithium replenishment and positive electrode lithium replenishment. The research and development of negative electrode lithium replenishment technology started earlier, including physical mixed lithium replenishment based on metallic lithium, self-discharge lithiation, chemical lithium replenishment, and electrochemical lithiation. This lithium replenishment method is simple and efficient, but due to the safety risks and process difficulties of metallic lithium itself, negative electrode lithium replenishment technology still cannot be applied on a large scale. Positive electrode lithium replenishment adds lithium replenishment materials to the positive electrode of lithium-ion batteries. During the battery charging process, the lithium replenishment materials decompose and release active lithium to make up for the irreversible active lithium loss caused by the growth of negative electrode SEI. Positive electrode lithium replenishment materials have the advantages of relatively stable chemical properties, easy synthesis, low price and high lithium replenishment capacity. At the same time, the positive electrode lithium replenishment process is well compatible with the existing lithium-ion battery manufacturing process, providing a new solution for the commercial application of lithium replenishment technology.
[0004] There are many types of positive electrode lithium supplements reported so far, such as Li 3 N.Li 2 S. Li 2 NiO 2 , Li 5 FeO 4 , Li 2 MnO 2 etc. Li-rich metal oxides such as Li 5 FeO 4 , Li 6 CoO 4 , Li 2 NiO 2 , Li 5 MnO 4 etc., have high lithium replenishment capacity, moderate working voltage and little impact on existing battery manufacturing process, among which lithium ferrite (Li 5 FeO 4) has a theoretical specific capacity of up to 867mAh·g-1, and a low discharge specific capacity. It has a very high lithium replenishment capacity, which can largely compensate for the lithium loss during the charge and discharge process; but it also has poor air stability and is easily exposed to H in the air. 2 O、CO 2 The reaction deteriorates; the residual alkali content on the surface is high, resulting in unstable slurry process, large polarization, side reactions with the electrolyte leading to abnormal gas production and poor conductivity; and poor conductivity leading to increased decomposition voltage. These problems prevent it from fully exerting its high lithium replenishment capacity, limiting its large-scale application in lithium-ion batteries. Summary of the invention
[0005] The present invention provides a positive electrode lithium supplement agent and its preparation and application. A uniform and dense coating layer is formed on the surface of the lithium supplement agent, which can effectively isolate the reaction between the lithium supplement agent core and moisture and carbon dioxide, improve the problem of poor air stability of the lithium supplement agent, and enhance the storage, transportation and processing performance; moreover, the outer coating layer of the lithium supplement agent has good conductivity, which can effectively reduce the resistivity of the lithium supplement agent, exert a more excellent lithium supplement effect, and solve the technical problem of poor conductivity.
[0006] In order to achieve the above object, the present invention provides a positive electrode lithium supplement agent, which is composed of a lithium supplement agent core and a double coating layer; the lithium supplement agent core is lithium ferrite Li 5 FeO 4 The first coating layer of the double coating layer from the inside to the outside contains at least one of an acidic compound and a lithium salt generated by an acidic compound and residual alkali, and the second coating layer is a carbon layer.
[0007] In the above scheme, the positive electrode lithium supplement agent adopts a double-layer coating. Specifically, an acidic compound is used to react with the residual alkali on the surface to convert it into a first coating layer, and then a carbon layer is introduced as a second coating layer. The introduction of the acidic compound not only reduces the residual alkali on the surface, but also effectively blocks the carbon reduction reaction caused by the CVD method. The formation of a uniform and dense coating layer on the surface of the lithium supplement agent can effectively isolate the reaction between the lithium supplement agent core and moisture and carbon dioxide, improve the problem of poor air stability of the lithium supplement agent, and improve the storage, transportation and processing performance. In addition, its outer coating layer has good conductivity, which can also effectively reduce the resistivity of the lithium supplement agent and exert a better lithium supplement effect.
[0008] Preferably, the positive electrode lithium replenisher has an alkali value of ≤0.5% and a powder resistivity of ≤0.05 kΩ·cm.
[0009] Preferably, the core size of the lithium supplement agent is 5 to 20 μm, and the coating layer thickness is 20 to 80 nm.
[0010] Preferably, the acidic compound is selected from B 2 O 3 、AlCl3 、Al 2 O 3 、FeCl 3 、TiO 2 CrO 3 , Mn 2 O 7 、SiO 2 At least one of;
[0011] The particle size of the acidic compound is less than 500 nm, so that it is more conducive to forming a uniform coating layer on the surface of lithium ferrite;
[0012] The added amount of the acidic compound is 0.1% to 1%.
[0013] The present invention also provides a method for preparing a positive electrode lithium supplement according to any one of the above technical solutions, comprising the following steps:
[0014] The iron source and the lithium source are dissolved in water respectively, and then the lithium salt aqueous solution is slowly added into the iron salt aqueous solution to form a uniform colloid, which is spray-dried to obtain a precursor powder;
[0015] The obtained precursor powder is sintered at high temperature in a vacuum atmosphere to obtain a lithium supplement material;
[0016] The obtained lithium supplement material is evenly mixed with the acidic compound, loaded into a CVD furnace, introduced with an inert gas, heated to a set temperature, introduced with an organic gas, maintained for a certain period of time for carbonization, and cooled with the furnace to obtain a positive electrode lithium supplement agent.
[0017] Preferably, the iron source is at least one of iron hydroxide, sulfate, chlorate, and nitrate, including Fe(NO 3 ) 3 、FeCl 3 , Fe 2 (SO 4 ) 3 、Fe(NO 3 ) 3 9H 2 O, preferably Fe(NO 3 ) 3 9H 2 O; the lithium source is at least one of lithium oxides, hydroxides, peroxides, inorganic salts, and organic salts, including Li 2 O, LiOH, LiOH·H 2 O. Li 2 CO 3 、LiNO 3 , Li 2 C 2 O 4At least one of the following, preferably LiNO 3 .
[0018] Preferably, the high temperature sintering temperature is 600-950°C, the sintering time is 1-20h; the vacuum degree of the vacuum atmosphere is 1×10 -5 Pa;
[0019] The organic gas introduced is selected from at least one of acetylene, ethylene, methane, propane and butane; the carbonization temperature is 500-650° C., and the carbonization time is 5-40 minutes.
[0020] Preferably, the lithium supplement material and the acidic compound are mixed in a solid phase or in a liquid phase; wherein the solid phase mixing is selected from at least one of high mixer mixing, grinding mixing, ball mill mixing, and wall breaking machine mixing; and the solvent used for the liquid phase mixing is selected from at least one of dichloromethane, chloroform, dimethylformamide, ethanol, acetone, tetrahydrofuran, and N-methylpyrrolidone.
[0021] The present invention also provides a lithium ion battery, the positive electrode of which is prepared by homogenizing the positive electrode lithium supplement agent described in any of the above technical solutions as an additive with active materials, conductive agents, and binders.
[0022] Preferably, the amount of the positive electrode lithium supplement added is 0.5 to 5% of the mass of the positive electrode active material.
[0023] Compared with the prior art, the advantages and positive effects of the present invention are:
[0024] The present invention provides a positive electrode lithium supplement agent, which adopts a double-layer coating. On the first aspect, the acidic compound of the first coating raw material can react with the residual alkali on the surface to form a coating layer, which effectively reduces the surface alkali value of the lithium supplement material and effectively blocks the carbon reduction reaction during the carbonization process of the second coating layer; on the second aspect, the formation of a uniform and dense coating layer on the surface of the lithium supplement agent can effectively isolate the reaction between the lithium supplement agent core and moisture and carbon dioxide, improve the problem of poor air stability of the lithium supplement agent, and improve the storage, transportation and processing performance; on the third aspect, the outer coating layer of the lithium supplement agent provided by the present invention has good conductivity, which can effectively reduce the resistivity of the lithium supplement agent and exert a better lithium supplement effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a SEM image of the positive electrode lithium supplement prepared in Example 1 of the present invention;
[0026] Figure 2 This is a performance diagram of the lithium replenishing capacity of the positive electrode lithium replenishing agent prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] 1. Preparation of positive electrode lithium supplement matrix
[0030] Take 0.05 mol of Fe(NO 3 ) 3 9H 2 O is dissolved in 50 ml of deionized water to obtain ferric hydroxide colloid. Take 0.2625 mol LiNO 3 Dissolve in 50 ml of water and gradually add it dropwise to the iron hydroxide colloid to obtain a precursor solution. Spray dry the precursor solution at a drying temperature of 180 ° C, a pressure of 0.3 MPa, and a feed rate of 20 mL / min to obtain precursor particles. The obtained precursor powder is placed under vacuum conditions (vacuum degree of 1×10 -5 Pa) at 850℃ for 3h, and then cooled to obtain Li 5 FeO 4 , particle size D50 is 7.8μm.
[0031] 2. Preparation of positive electrode lithium supplement containing coating layer
[0032] Add 0.5% B 2 O 3 The material was mixed in the lithium supplement agent matrix at 2000 rpm for 30 min in a high-speed mixer, and then placed in a CVD furnace, purged with nitrogen, heated to 550°C, introduced with acetylene, and kept warm for 20 min for carbonization, and cooled with the furnace to obtain a positive electrode lithium supplement agent containing a coating layer. Its SEM image and lithium supplement capacity performance graph are shown as follows: Figure 1 and 2 As shown. Figure 1 It can be seen that the LFO surface coating is uniform; Figure 2 It can be seen that the lithium supplement agent has a low platform potential, high constant current capacity, and excellent lithium supplement performance.
[0033] Example 2
[0034] 1. Preparation of positive electrode lithium supplement matrix
[0035] The preparation method is the same as the method for preparing the positive electrode lithium supplementation agent matrix in Example 1, and Li 5 FeO 4 .
[0036] 2. Preparation of positive electrode lithium supplement containing coating layer
[0037] Add 0.2% Al 2 O 3 In the lithium supplement agent matrix, mix at 2000 rpm in a high-speed mixer for 30 minutes, then place the material in a CVD furnace, purge with nitrogen, heat to 550°C, introduce acetylene, keep warm for 20 minutes for carbonization, and cool with the furnace to obtain a positive electrode lithium supplement agent containing a coating layer.
[0038] Example 3
[0039] 1. Preparation of positive electrode lithium supplement matrix
[0040] The preparation method is the same as the method for preparing the positive electrode lithium supplementation agent matrix in Example 1, and Li 5 FeO 4 .
[0041] 2. Preparation of positive electrode lithium supplement containing coating layer
[0042] Add 1% SiO 2 In the lithium supplement agent matrix, mix at 2000 rpm in a high-speed mixer for 30 minutes, then place the material in a CVD furnace, purge with nitrogen, heat to 550°C, introduce acetylene, keep warm for 20 minutes for carbonization, and cool with the furnace to obtain a positive electrode lithium supplement agent containing a coating layer.
[0043] Comparative Example 1
[0044] The preparation method is the same as that of Example 1, except that no coating layer is added to the lithium supplement agent matrix.
[0045] Comparative Example 2
[0046] 1. Preparation of positive electrode lithium supplement matrix
[0047] The preparation method is the same as the method for preparing the positive electrode lithium supplementation agent matrix in Example 1, and Li 5 FeO 4 .
[0048] 2. Preparation of positive electrode lithium supplement containing coating layer
[0049] Add 0.5% B 2 O 3 In the lithium supplement agent matrix, the high-speed mixer is mixed at 2000 revolutions for 30 minutes, and then the material is placed in a tubular furnace, purged with nitrogen, heated to 550°C, and kept warm for 20 minutes for carbonization, and cooled with the furnace to obtain the coated lithium supplement agent.
[0050] Comparative Example 3
[0051] 1. Preparation of positive electrode lithium supplement matrix
[0052] The preparation method is the same as the method for preparing the positive electrode lithium supplementation agent matrix in Example 1, and Li 5 FeO4 .
[0053] 2. Preparation of positive electrode lithium supplement containing coating layer
[0054] The material obtained in step 1 is placed in a CVD furnace, purged with nitrogen, heated to 550° C., introduced with acetylene, kept warm for 20 minutes, and cooled with the furnace to obtain a coated lithium supplement agent.
[0055] Alkalinity test
[0056] The positive electrode lithium supplement products of Examples 1 to 3 and Comparative Examples 1 to 3 were dissolved in methanol at a ratio of solid to liquid = 1:20, and the solid material was filtered out after stirring for 10 minutes. The filtrate was transferred to a titration cup and electrochemically titrated with 0.1M hydrochloric acid standard solution. The sum of the two breakpoints was taken as the total base number. The test results are shown in Table 1:
[0057] Table 1
[0058] Total Base Number Example 1 0.243 Example 2 0.372 Example 3 0.293 Comparative Example 1 2.025 Comparative Example 2 0.333 Comparative Example 3 1.801
[0059] It can be seen from Table 1 that the introduction of acidic compounds has a significant improvement effect on reducing the alkalinity of the lithium supplement material, which is mainly due to the in-situ reaction between the acidic compounds and the residual alkali on the surface of the lithium supplement.
[0060] Powder resistivity test
[0061] Table 2
[0062] Powder resistivity (kΩ·cm) Example 1 0.006 Example 2 0.002 Example 3 0.009 Comparative Example 1 >100 Comparative Example 2 >100 Comparative Example 3 0.008
[0063] It can be seen from Table 2 that the introduction of the carbon layer has a significant improvement effect on reducing the powder resistivity of the lithium supplement material.
[0064] Air stability test
[0065] The lithium supplement prepared in each embodiment and each comparative example was mixed with a conductive agent and a binder to form a pole piece, which was assembled with a lithium sheet into a half-cell for testing. The stability data in an air atmosphere with a temperature of 30° C. and a humidity of 30% are shown in Table 3:
[0066] Table 3
[0067] Example 24h capacity retention rate (%) Example 1 92.5 Example 2 91.3 Example 3 91.8 Comparative Example 1 42.0 Comparative Example 2 75.8 Comparative Example 3 80.1
[0068] As shown in Table 3, the double-layer coating can effectively block the lithium supplementation agent matrix from the external H 2 O、CO 2 contact, improving the air stability of lithium-supplementing materials.
[0069] Battery performance test
[0070] In order to further prove the effectiveness of the product of the present invention, the products prepared in each embodiment and each comparative example were used as lithium supplements and mixed with lithium iron phosphate, conductive carbon black and PVDF at 2wt% of the positive electrode active material to make positive electrode sheets. Graphite was used as the negative electrode active material to make negative electrode sheets, and the full battery was assembled for testing. The data are shown in Table 4:
[0071] Table 4
[0072]
[0073] It can be seen from Table 4 that the positive electrode lithium replenisher obtained by the preparation method of the present invention has a more excellent lithium replenishing effect.
Claims
1. A positive electrode lithium supplement, It is characterized in that It is composed of a lithium supplement core and a double coating layer; the lithium supplement core is lithium ferrite Li 5 FeO 4 The first coating layer of the double coating layer from the inside to the outside contains at least one of an acidic compound and a lithium salt generated by an acidic compound and residual alkali, and the second coating layer is a carbon layer.
2. The positive electrode lithium supplement according to claim 1, It is characterized in that The alkalinity value of the positive electrode lithium supplement is ≤0.5%, and the powder resistivity is ≤0.05 kΩ·cm.
3. The positive electrode lithium supplement according to claim 1 or 2, It is characterized in that The core size of the lithium supplement agent is 5 to 20 μm, and the coating layer thickness is 20 to 80 nm.
4. The positive electrode lithium supplement according to claim 1, It is characterized in that The acidic compound is selected from B 2 O 3 、AlCl 3 、Al 2 O 3 、FeCl 3 、TiO 2 CrO 3 , Mn 2 O 7 、SiO 2 At least one of; The particle size of the acidic compound is less than 500 nm; The added amount of the acidic compound is 0.1% to 1%.
5. A method for preparing a positive electrode lithium supplement according to any one of claims 1 to 4, It is characterized in that The following steps are involved: The iron source and the lithium source are dissolved in water respectively, and then the lithium salt aqueous solution is slowly added into the iron salt aqueous solution to form a uniform colloid, which is then spray-dried to obtain a precursor powder; The obtained precursor powder is sintered at high temperature in a vacuum atmosphere to obtain a lithium supplement material; The obtained lithium supplement material is evenly mixed with the acidic compound, loaded into a CVD furnace, introduced with an inert gas, heated to a set temperature, introduced with an organic gas, maintained for a certain period of time for carbonization, and cooled with the furnace to obtain a positive electrode lithium supplement agent.
6. The preparation method according to claim 5, It is characterized in that The iron source is at least one of iron hydroxide, sulfate, chlorate, and nitrate, including Fe(NO 3 ) 3 、FeCl 3 , Fe 2 (SO 4 ) 3 、Fe(NO 3 ) 3 9H 2 O; the lithium source is at least one of lithium oxides, hydroxides, peroxides, inorganic salts, and organic salts, including Li 2 O, LiOH, LiOH·H 2 O. Li 2 CO 3 、LiNO 3 , Li 2 C 2 O 4 At least one of .
7. The preparation method according to claim 5, It is characterized in that The high temperature sintering temperature is 600-950℃, the sintering time is 1-20h; the vacuum degree of the vacuum atmosphere is 1×10 -5 Pa; The organic gas introduced is selected from at least one of acetylene, ethylene, methane, propane and butane; the carbonization temperature is 500-650° C., and the carbonization time is 5-40 minutes.
8. The preparation method according to claim 5, It is characterized in that The lithium supplement material and the acidic compound are mixed in a solid phase or in a liquid phase; wherein the solid phase mixing is selected from at least one of high mixer mixing, grinding mixing, ball mill mixing, and wall breaking machine mixing; and the solvent used for the liquid phase mixing is selected from at least one of dichloromethane, chloroform, dimethylformamide, ethanol, acetone, tetrahydrofuran, and N-methylpyrrolidone.
9. Lithium-ion battery, It is characterized in that The positive electrode is prepared by homogenizing the positive electrode lithium supplement agent described in any one of claims 1 to 5 as an additive with active materials, conductive agents and binders.
10. The lithium ion battery according to claim 9, It is characterized in that The amount of positive electrode lithium supplement added is 0.5-5% of the mass of the positive electrode active material.
Citation Information
Cited By
Double-layer coated lithium supplement material and preparation method thereof, positive pole piece and battery
CN120149594A
Lithium supplement intermediate as well as preparation method and application thereof
CN120328625A