Anisotropic conductive poly (3-thiopheneacetic acid) / methacrylated gelatin hydrogel patch as well as preparation method and application thereof
The preparation of anisotropic conductive poly(3-thiophene acetic acid)/methacrylylated gelatin hydrogel patches with dual network structures through 3D printing, which solved the problem of unclear mechanical and electrical indicators of cell-free myocardial patches, and achieved The conductivity and mechanical properties matching myocardial tissue are repaired and cardiac function is suppressed.
Patent Information
- Application Number
- CN202410966171.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
The existing cell-free myocardial patches are unclear in mechanics and electrical indicators, and do not have anisotropy, and cannot effectively repair myocardial electroconduction and mechanical properties, adapting to the needs of myocardial tissue.
The anisotropic conductive poly(3-thiophene acetic acid)/methacrylic gelatin hydrogel patches with dual network structure were prepared by 3D printing. The directional fiber microstructure was formed by dehydration treatment, combining photocuring and rehydration treatment. , obtain conductive and mechanical properties matching myocardial tissue.
It achieves the matching of the conductivity and mechanical properties of myocardial tissue, reduces the resistivity of the myocardial infarction area, restores normal electrical conduction and synchronous contraction of the heart, provides mechanical support matching with normal myocardial muscle, repairs cardiac function and inhibits arrhythmia, has a heart in the myocardial muscle In the early stage of infarction, it plays a role in functional recovery and promoting repair.
Smart Images

Figure BDA0004951835870000111 
Figure BDA0004951835870000112 
Figure BDA0004951835870000113
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bioengineering materials, and in particular to an anisotropic conductive poly (3-thiopheneacetic acid) / methacrylylated gelatin hydrogel patch and a preparation method and application thereof. Background Art
[0002] Myocardial infarction (MI) is one of the most common causes of morbidity and mortality worldwide. After MI occurs, it will cause damage to the structure and function of myocardial cells, leading to changes in the electrophysiological and mechanical properties of the myocardium. In addition, necrotic myocardial cells will gradually be replaced by scar tissue that lacks conductivity and elasticity. Scar tissue divides normal myocardial cells, causing myocardial electrical signal conduction block and contraction asynchrony, leading to impaired cardiac pumping function and the occurrence of arrhythmias, which will subsequently cause pathological ventricular remodeling and may further develop into heart failure. Because adult myocardial cells are non-regenerative, traditional treatments (such as drug therapy and interventional therapy) are difficult to repair damaged myocardium. Therefore, researchers are committed to finding new materials to repair damaged myocardium.
[0003] Cardiac patches made of biomaterials can be combined with cells or drugs to provide a potential treatment for MI and subsequent heart failure. There are two main research directions for cardiac patches: one is to prepare patches using biomaterials combined with various cells, such as cardiomyocytes derived from embryonic stem cells (ESCs), mesenchymal stem cells (MSCs) or induced pluripotent stem cells (iPSCs), etc., to treat MI using the paracrine effect of stem cells, or to hope that artificially induced cardiomyocytes can colonize in the MI area to repair the myocardium. However, the cell components in the patch reported so far have extremely low retention and survival rates at the MI site, and cannot be effectively integrated into autologous myocardial tissue to repair cardiac function (Zhang J, Zhu W, Radisic M, Vunjak-Novakovic G. Can We Engineer a Human Cardiac Patch for Therapy?. Circ Res. 2018; 123(2): 244-265). At the same time, because the problems of cell source and safety have not been fully resolved, cell-containing cardiac patches are still far from clinical transformation (Augustine R, Dan P, Hasan A, et al. Stem cell-based approaches in cardiac tissue engineering: controlling the microenvironment for autologous cells. Biomed Pharmacother. 2021; 138: 111425). Another type is a cell-free myocardial patch made of pure materials, which can passively limit excessive expansion of the myocardial infarct area, reduce myocardial wall stress, and prevent left ventricular expansion and remodeling; or the patch itself has a certain conductivity, which can enhance electrical conduction in the myocardial infarction area. Studies have shown that after MI occurs, acellular myocardial patches provide mechanical support for the infarcted myocardial area and restore its conductivity, which has a positive effect on repairing cardiac function (Holmes JW, Borg TK, Covell JW. Structure and mechanics of healing myocardial infarcts. Annu Rev Biomed Eng. 2005; 7: 223-253). Since this type of patch does not contain cells, its safety and stability are more controllable, it is more practical, and it is more likely to be used in clinical practice.
[0004] In recent years, many studies have been devoted to the development of such acellular myocardial patches, and one of the commonly used materials is various types of hydrogels. Hydrogels can contain a large amount of water while maintaining their own morphology, have adjustable physical and chemical properties and can be environmentally responsive, can carry drugs and cells, and have flexible preparation methods. Therefore, they have been widely studied in the field of tissue engineering. However, the hydrogel myocardial patches currently prepared often cannot take into account good conductivity, biocompatibility and mechanical properties. For example, some studies have prepared patches by adding conductive materials such as metal nanoparticles and carbon nanomaterials to biological hydrogels in order to restore the conductivity of tissues in the myocardial infarction area and reconstruct synchronous myocardial contraction. However, on the one hand, biomaterials (such as alginate, hyaluronic acid, etc.) used as matrix materials have insufficient mechanical strength and cannot provide mechanical support that matches myocardial tissue (Venugopal JR, Prabhakaran MP, Mukherjee S, Ravichandran R, Dan K, Ramakrishna S. Biomaterial strategies for alleviation of myocardial infarction. JR Soc Interface. 2012; 9(66): 1-19). On the other hand, metal materials (such as gold nanorods) or carbon nanomaterials (such as carbon nanotubes) added to hydrogels are non-degradable and have poor long-term biocompatibility (Mao, HY; Laurent, S.; Chen, W.; Akhavan, O.; Imani, M.; Ashkarran, AA; Mahmoudi, M. Graphene: Promises, Facts, Opportunities, and Challenges in Nanomedicine. Chem Rev. 2013,113,3407-3424). In order to solve the contradiction that inorganic conductive materials are not suitable for flexible tissues, in recent years, some studies have turned their attention to high molecular conductive polymers, such as polypyrrole and polyaniline. Compared with inorganic materials such as metals, these materials are soft and degradable, and they are conductive due to the π-π conjugation effect.A study synthesized a polypyrrole-chitosan hydrogel patch and studied its effect on improving cardiac function by improving electrical conduction in the myocardial infarction area (He S, Wu J, Li SH, et al. The conductive function of biopolymer corrects myocardial scar conduction blockage and resynchronizes contraction to prevent heart failure. Biomaterials. 2020; 258: 120285), but the patch did not consider the effects of mechanical factors on the heart.
[0005] Since normal electrical conduction and mechanical properties are crucial to cardiac function, some studies have given the patch conductivity or high strength when designing it. However, the mechanical and electrical indicators of the patch are still unclear. First, the conductivity of the patch with the best mechanical strength is still unknown. Second, myocardial fibers are directional. Myocardial tissue has obvious anisotropy at the electrical and mechanical levels. Along the direction parallel or perpendicular to the myocardial fibers, the conductivity of the myocardium can range from 5×10 -5 S / cm to 1.6×10 - 3 S / cm, spanning two orders of magnitude, with a tensile strength of 3-15 kPa and a Young's modulus of 0.2-0.5 MPa. However, the patches reported so far are often uniform in all directions, which does not conform to the anisotropy of myocardial tissue. Summary of the invention
[0006] The purpose of the present invention is to provide an anisotropic conductive poly (3-thiopheneacetic acid) / methacryloyl gelatin hydrogel patch and its preparation method and application, so as to solve the problems that the mechanical and electrical indicators of the existing acellular myocardial patch are unclear and lack anisotropy.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing an anisotropic conductive poly (3-thiopheneacetic acid) / methacrylylated gelatin hydrogel patch, comprising the following steps:
[0009] (1) mixing methacryloyl gelatin, poly (3-thiopheneacetic acid), a cross-linking agent and a solvent; 3D printing the obtained mixed solution; and photocuring the obtained 3D printed part to obtain a poly (3-thiopheneacetic acid) / methacryloyl gelatin hydrogel patch;
[0010] (2) The poly (3-thiopheneacetic acid) / methacrylic acid gelatin hydrogel patch described in step (1) is subjected to dehydration treatment and rehydration treatment in sequence to obtain an anisotropic conductive poly (3-thiopheneacetic acid) / methacrylic acid gelatin hydrogel patch.
[0011] Preferably, in the preparation method, in step (1), the molecular weight of the poly(3-thiopheneacetic acid) is 10,000 to 20,000, and the crosslinking agent is a mixture of N,N'-carbonyldiimidazole (CDI) and a photoinitiator.
[0012] Preferably, in the preparation method, in step (1), the concentration of the methacrylated gelatin in the mixed solution is 5 to 20 wt %, and the concentration of the poly (3-thiopheneacetic acid) in the mixed solution is 5 to 20 wt %.
[0013] Preferably, in the preparation method, the concentration of the N,N'-carbonyldiimidazole in the mixed solution of step (1) is 2-7 wt %, and the concentration of the photoinitiator 2959 in the mixed solution of step (1) is 0.1-0.5 wt %.
[0014] Preferably, in the preparation method, in step (1), the extrusion temperature of the 3D printing is 20 to 30° C., the extrusion pressure is 80 to 100 kPa, the printing speed is 0.5 to 1 mm / s, and the number of printing layers is 1 to 20 layers.
[0015] Preferably, in the preparation method, in step (1), the light intensity of the light curing is 500 to 1500 mW / cm 2 The light wavelength is 380-420nm and the irradiation time is 30-60s.
[0016] Preferably, in the preparation method, in step (2), the initial stress of the dehydration treatment is 10 to 100 kPa, the temperature is 20 to 30° C., the humidity is 30 to 50%, and the time is 24 to 48 hours.
[0017] Preferably, in the preparation method, in step (2), the reagent used for the rehydration treatment is Dulbecco's phosphate buffered saline (DPBS buffer), the temperature of the rehydration treatment is 20 to 30° C., and the time is 12 to 48 hours.
[0018] The invention also provides an anisotropic conductive poly (3-thiopheneacetic acid) / methacrylylated gelatin hydrogel patch prepared by the preparation method.
[0019] The present invention also provides an application of the anisotropic conductive poly (3-thiopheneacetic acid) / methacrylylated gelatin hydrogel patch in preparing myocardial repair materials.
[0020] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0021] (1) The present invention combines the polymer conductive material poly(3-thiopheneacetic acid) (PTAA) with the biogenic photocurable material methacryloyl gelatin (GelMA) to prepare a double network hydrogel. PTAA, as a derivative of polythiophene, has stable chemical properties and good conductivity. The presence of carboxyl groups enables it to form a cross-linked network hydrogel, which can be used as a conductive rigid network in the system. GelMA is olefin double-bond modified gelatin. It is a photo-crosslinked GelMA that is a soft / plastic network with excellent biocompatibility, cell response characteristics and good mechanical property adjustability. It can be rapidly cured into gel by ultraviolet or visible light under the action of a photoinitiator. It is used to improve the mechanical properties and tissue compatibility of PTAA, so that the toughness of PTAA can withstand a deformation degree of 15-22% due to myocardial beating. At the same time, gelatin is amidated to reduce the number of carboxyl groups, and then reacted with methacrylic anhydride to prepare GelMA, which can reduce the crosslinking of anhydride bonds between the GelMA network and the PTAA network through carboxyl groups, thereby retaining the properties of each hydrogel network, so that the two hydrogel networks penetrate each other without chemical crosslinking, thereby giving the whole a performance superior to that of a single component.
[0022] (2) The present invention adopts a one-step 3D printing method to prepare a double-network structure hydrogel, which is helpful for further personalized patch customization and complex shape patch preparation, and without reducing the biocompatibility of the hydrogel, it can initially obtain conductivity and mechanical properties that match myocardial tissue. Since the shape of the infarct area after myocardial infarction is irregular, the infarct area can be imaged after ligation surgery, followed by 3D modeling, and 3D printing rapid prototyping is achieved using an extrusion printer and the light-curing properties of synthetic hydrogels, and then commercially available biological glue is used to achieve adhesion of the patch to the surface of the heart without causing secondary damage.
[0023] (3) The present invention utilizes dehydration treatment, i.e., restricted dehydration method, to generate stress in a specific direction inside the hydrogel during the dehydration process, so that the high molecular polymers in the dehydration process self-assemble under stress through supramolecular interaction to form a fiber microstructure with directional arrangement similar to myocardial fibers, thereby obtaining anisotropic mechanical properties. The fiber microstructure mimics myocardial fibers, making the electrical and mechanical properties of the hydrogel patch closer to those of normal myocardium, solving the problems of low strength, uniformity in all directions, and difficulty in achieving anisotropy in existing hydrogel materials.
[0024] (4) The anisotropic conductive poly (3-thiopheneacetic acid) / methacryloyl gelatin hydrogel patch prepared by the present invention can reduce the resistivity of the myocardial infarction area, restore normal electrical conduction and synchronous contraction of the heart, and provide mechanical support that matches the normal myocardium, thereby repairing cardiac function and inhibiting the occurrence of arrhythmias, which has positive significance for the recovery of early myocardial pumping function after myocardial infarction and the long-term prevention of heart failure. The biomaterial patch prepared by the present invention is a tool that can be quickly prepared, easy to store and quickly take effect. It is expected to play a role in restoring the function and promoting repair of the damaged heart in the early stage of MI. In addition, the preparation method of the patch is simple, rapid, and bio-friendly, laying a good foundation for further research on cellular conductive hydrogel patches. DETAILED DESCRIPTION
[0025] The present invention provides a method for preparing an anisotropic conductive poly (3-thiopheneacetic acid) / methacrylylated gelatin hydrogel patch, comprising the following steps:
[0026] (1) mixing methacryloyl gelatin, poly (3-thiopheneacetic acid), a cross-linking agent and a solvent; 3D printing the obtained mixed solution; and photocuring the obtained 3D printed part to obtain a poly (3-thiopheneacetic acid) / methacryloyl gelatin hydrogel patch;
[0027] (2) The poly (3-thiopheneacetic acid) / methacrylic acid gelatin hydrogel patch described in step (1) is subjected to dehydration treatment and rehydration treatment in sequence to obtain an anisotropic conductive poly (3-thiopheneacetic acid) / methacrylic acid gelatin hydrogel patch.
[0028] In the present invention, in step (1), the method of mixing the methacryloyl gelatin, poly (3-thiopheneacetic acid), cross-linking agent and solvent is preferably: mixing the methacryloyl gelatin, poly (3-thiopheneacetic acid) and solvent, and adding the cross-linking agent.
[0029] In the present invention, in step (1), the method for preparing methacryloyl gelatin comprises the following steps:
[0030] The method comprises the following steps: mixing gelatin, adipic acid dihydrazide and water to obtain a first solution; mixing a condensing agent with a mixed solvent of DMSO-water to obtain a second solution; mixing the first solution with the second solution, performing an amidation reaction, and obtaining aminated gelatin; mixing the aminated gelatin, methacrylic anhydride and DPBS buffer solution, and performing a methacrylation reaction; and dialyzing and freeze-drying the obtained product in sequence to obtain methacrylated gelatin.
[0031] In the present invention, the condensing agent is preferably a mixture of EDC (1-ethyl-(3-dimethylaminopropyl)carbodiimide) and HOBt (1-hydroxybenzotriazole).
[0032] In the present invention, the parameters in the preparation method of the methacryloyl gelatin are not limited, and the schemes well known to those skilled in the art can be adopted.
[0033] In the present invention, in step (1), the method for preparing poly (3-thiopheneacetic acid) comprises the following steps:
[0034] 3-Thiopheneacetic acid, methanol and sulfuric acid are mixed to carry out esterification reaction to obtain 3-thiophenemethyl acetate (3TMA); the 3TMA, catalyst FeCl3 and chloroform are mixed to carry out oxidative polymerization reaction to obtain poly (3-thiophenemethyl acetate) (P3TMA); the P3TMA is hydrolyzed in NaOH solution to obtain poly (3-thiopheneacetic acid) (PTAA).
[0035] In the present invention, the parameters in the preparation method of poly(3-thiopheneacetic acid) are not limited, and the schemes well known to those skilled in the art can be adopted.
[0036] In the present invention, the molecular weight of the poly(3-thiopheneacetic acid) in step (1) is preferably 10,000 to 20,000, more preferably 10,000 to 15,000, and even more preferably 12,000.
[0037] In the present invention, in step (1), the crosslinking agent is preferably a mixture of N,N'-carbonyldiimidazole and photoinitiator 2959.
[0038] In the present invention, in step (1), the solvent is preferably DMSO (dimethyl sulfoxide).
[0039] In the present invention, in step (1), the concentration of the methacryloyl gelatin in the mixed solution is preferably 5 to 20 wt %, more preferably 10 to 15 wt %, and more preferably 10 wt %.
[0040] In the present invention, in step (1), the concentration of the poly (3-thiopheneacetic acid) in the mixed solution is preferably 5 to 20 wt %, more preferably 10 to 20 wt %, and more preferably 10 wt %.
[0041] In the present invention, the concentration of the N,N'-carbonyldiimidazole in the mixed solution of step (1) is preferably 2-7 wt%, more preferably 3-6 wt%, and more preferably 6 wt%.
[0042] In the present invention, the concentration of the photoinitiator 2959 in the mixed solution in step (1) is preferably 0.1-0.5 wt %, more preferably 0.2-0.4 wt %, and more preferably 0.2 wt %.
[0043] In the present invention, in step (1), the 3D printed needle is preferably a 27G needle.
[0044] In the present invention, in step (1), the extrusion temperature of the 3D printing is preferably 20-30°C, more preferably 25-30°C, and more preferably 25°C; the extrusion pressure is preferably 80-100kPa, more preferably 90-100kPa, and more preferably 100kPa; the printing speed is preferably 0.5-1mm / s, more preferably 0.8-1mm / s, and more preferably 0.8mm / s; the number of printing layers is preferably 1-20 layers, more preferably 2-12 layers, and more preferably 6 layers.
[0045] In the present invention, in step (1), the light source for photocuring is fixed at the outlet of the 3D printing needle.
[0046] In the present invention, in step (1), the light source for photocuring is preferably ultraviolet light.
[0047] In the present invention, in step (1), the light intensity of the light curing is preferably 500 to 1500 mW / cm 2 , more preferably 800 to 1200 mW / cm 2 , more preferably 1000 mW / cm 2 ; The wavelength of light is preferably 380 to 420 nm, more preferably 380 to 405 nm, and more preferably 405 nm; the irradiation time is preferably 30 to 60 s, more preferably 40 to 60 s, and more preferably 60 s.
[0048] In the present invention, in step (2), the device used for the dehydration treatment (ie, the hydrogel restricted dehydration device) is preferably mainly composed of an acrylic frame and an adjustable position fixture mounted on the frame.
[0049] In the present invention, in step (2), the initial stress of the dehydration treatment is preferably 10 to 100 kPa, more preferably 40 to 100 kPa, and more preferably 60 kPa; the temperature is preferably 20 to 30°C, more preferably 25 to 30°C, and more preferably 25°C; the humidity is preferably 30 to 50%, more preferably 35 to 50%, and more preferably 50%; the time is preferably 24 to 48 h, more preferably 24 to 36 h, and more preferably 24 h.
[0050] In the present invention, in step (2), the reagent used for the rehydration treatment is preferably DPBS buffer.
[0051] In the present invention, in step (2), the temperature of the rehydration treatment is preferably 20-30°C, more preferably 25-30°C, and more preferably 25°C; the time is preferably 12-48h, more preferably 24-36h, and more preferably 24h.
[0052] The invention also provides an anisotropic conductive poly (3-thiopheneacetic acid) / methacrylylated gelatin hydrogel patch prepared by the preparation method.
[0053] The present invention also provides an application of the anisotropic conductive poly (3-thiopheneacetic acid) / methacrylylated gelatin hydrogel patch in preparing myocardial repair materials.
[0054] In the present invention, the application method is not limited, and any method known to those skilled in the art may be used.
[0055] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0056] Preparation Example 1
[0057] 1 g of gelatin (Rosselot (Guangdong) Gelatin Co., Ltd.) and 2.36 g of adipic acid dihydrazide were dissolved in 100 mL of deionized water to obtain a first solution; 2.79 g of EDC and 1.83 g of HOBt were dissolved in 50 mL of a mixed solvent of DMSO / water (v / v=1:1) to obtain a second solution; the first solution was added to the second solution at a stirring speed of 300 rpm, and an amidation reaction was carried out at 40°C for 24 hours to obtain aminated gelatin, thereby reducing the number of free carboxyl groups in the gelatin; 5 g of aminated gelatin was dissolved in 50 mL of DPBS buffer to obtain a mixed solution, to which methacrylic anhydride (methacrylic anhydride was 1.4% of the volume of the mixed solution) was added dropwise (dropping speed 1.5 mL / min), and the mixture was reacted at 50°C for 6 hours; the obtained product was dialyzed in deionized water at 40°C for 7 days using a dialysis bag with a molecular weight cutoff of 10 kDa, and then freeze-dried to obtain GelMA powder, which was frozen and stored for later use;
[0058] 5 g of 3-thiopheneacetic acid and 3 mL (70 wt%) concentrated sulfuric acid were dissolved in 50 mL of methanol, reacted at 60°C for 24 h, and then the methanol was evaporated to obtain 3-thiophenemethyl acetate (3TMA); 2 g of FeCl3 was used as a catalyst in 30 mL of dry chloroform, and the obtained 3TMA was oxidatively polymerized at 5°C for 24 h to obtain P3TMA; P3TMA was added to 2 mol / L NaOH solution, hydrolyzed at 90°C for 24 h to obtain PTAA with a molecular weight of 12,000.
[0059] Example 1
[0060] This embodiment provides a method for preparing an anisotropic conductive poly (3-thiopheneacetic acid) / methacrylylated gelatin hydrogel patch, comprising the following steps:
[0061] (1) The methacryloyl gelatin of Preparation Example 1 and the poly(3-thiopheneacetic acid) of Preparation Example 1 were mixed with DMSO, and CDI and Irgacure 2959 were added, wherein the concentration of methacryloyl gelatin was 10 wt %, the concentration of poly(3-thiopheneacetic acid) was 10 wt %, the concentration of CDI was 6 wt %, and the concentration of Irgacure 2959 was 0.1 wt %; the above solution system was loaded into the syringe of a 3D printer, and a 27G needle was selected for printing. A UV light source was fixed at the outlet of the needle. The pre-designed shape was imported into a computer and 3D printing was performed. The conditions of 3D printing were: extrusion temperature 25° C., extrusion pressure 90 kPa, printing speed 0.8 mm / s, and printing layer number 6, and then light curing was performed. The conditions of light curing were: light intensity 1000 mW / cm 2 , irradiation wavelength of 405 nm, irradiation time of 50 s, to obtain a poly (3-thiopheneacetic acid) / methacrylylated gelatin hydrogel patch;
[0062] (2) Fixing the two ends of the poly (3-thiopheneacetic acid) / methacryloyl gelatin hydrogel patch described in step (1) on the hydrogel restricted water dehydration device with a clamp, dehydrating the patch for 24 hours at an initial stress of 60 kPa, 25° C., and a humidity of 50%, and then placing the dehydrated patch in DPBS buffer and rehydrating it at 25° C. for 24 hours to obtain an anisotropic conductive poly (3-thiopheneacetic acid) / methacryloyl gelatin hydrogel patch.
[0063] Example 2
[0064] This embodiment provides a method for preparing an anisotropic conductive poly (3-thiopheneacetic acid) / methacrylylated gelatin hydrogel patch, comprising the following steps:
[0065] (1) The methacryloyl gelatin of Preparation Example 1 and the poly(3-thiopheneacetic acid) of Preparation Example 1 were mixed with DMSO, and CDI and Irgacure 2959 were added, wherein the concentration of methacryloyl gelatin was 15 wt %, the concentration of poly(3-thiopheneacetic acid) was 5 wt %, the concentration of CDI was 3 wt %, and the concentration of Irgacure 2959 was 0.5 wt %; the above solution system was loaded into the syringe of a 3D printer, and a 27G needle was selected for printing. A UV light source was fixed at the outlet of the needle. The pre-designed shape was imported into a computer and 3D printing was performed. The conditions of 3D printing were: extrusion temperature 30° C., extrusion pressure 80 kPa, printing speed 1 mm / s, and printing number of 6 layers, and then light curing was performed. The conditions of light curing were: light intensity 800 mW / cm 2 , irradiation wavelength of 420 nm, irradiation time of 40 s, to obtain a poly (3-thiopheneacetic acid) / methacrylylated gelatin hydrogel patch;
[0066] (2) Fixing the two ends of the poly (3-thiopheneacetic acid) / methacryloyl gelatin hydrogel patch in step (1) on a hydrogel restricted water dehydration device with a clamp, dehydrating the patch for 24 h at an initial stress of 100 kPa, 30° C., and a humidity of 40%, and then placing the dehydrated patch in DPBS buffer and rehydrating it at 30° C. for 36 h to obtain an anisotropic conductive poly (3-thiopheneacetic acid) / methacryloyl gelatin hydrogel patch.
[0067] Example 3
[0068] This embodiment provides a method for preparing an anisotropic conductive poly (3-thiopheneacetic acid) / methacrylylated gelatin hydrogel patch, comprising the following steps:
[0069] (1) The methacrylated gelatin of Preparation Example 1 and the poly(3-thiopheneacetic acid) of Preparation Example 1 were mixed with DMSO, and CDI and Irgacure 2959 were added, wherein the concentration of methacrylated gelatin was 10 wt %, the concentration of poly(3-thiopheneacetic acid) was 15 wt %, the concentration of CDI was 2 wt %, and the concentration of Irgacure 2959 was 0.2 wt %; the above solution system was loaded into a 3D printer syringe, and a 27G needle was selected for printing. A UV light source was fixed at the needle outlet, and a pre-designed shape was imported into a computer for 3D printing. The 3D printing conditions were: extrusion temperature 20° C., extrusion pressure 100 kPa, printing speed 0.5 mm / s, and printing layer number 6, and then light curing was performed. The light curing conditions were: light intensity 1200 mW / cm 2 , irradiation wavelength of 380nm, irradiation time of 60s, to obtain poly (3-thiopheneacetic acid) / methacrylylated gelatin hydrogel patch;
[0070] (2) Fixing the two ends of the poly (3-thiopheneacetic acid) / methacrylic acid gelatin hydrogel patch described in step (1) on the hydrogel restricted water dehydration device with a clamp, dehydrating the patch for 24 hours at an initial stress of 40 kPa, 20° C., and a humidity of 35%, and then placing the dehydrated patch in DPBS buffer and rehydrating it at 20° C. for 48 hours to obtain an anisotropic conductive poly (3-thiopheneacetic acid) / methacrylic acid gelatin hydrogel patch.
[0071] Comparative Example 1
[0072] This comparative example provides a method for preparing an isotropically uniform conductive poly (3-thiopheneacetic acid) / methacrylated gelatin hydrogel patch, which differs from Example 1 in that step (2) is deleted, and other conditions and parameters are the same as those in Example 1.
[0073] Comparative Example 2
[0074] This comparative example provides a method for preparing an anisotropic GelMA hydrogel patch, which is different from Example 1 in that poly(3-thiopheneacetic acid) is deleted, and other conditions and parameters are the same as those in Example 1.
[0075] Test Case
[0076] The hydrogel patches obtained in Examples 1 to 3 and Comparative Examples 1 to 2 were subjected to performance tests according to the following method:
[0077] Swelling rate: Cut the hydrogel patch into 5 mm × 5 mm standard samples, use filter paper to absorb the surface moisture, and weigh to obtain W s1 The standard sample was completely immersed in PBS buffer and placed at 37°C for 24 hours. Then it was taken out of the buffer, the surface water was absorbed with filter paper, and the weight was re-weighed to obtain W. s2 The swelling rate SR of the hydrogel patch after implantation in vivo was calculated according to formula 1.
[0078]
[0079] Tensile strength and Young's modulus: tested in accordance with standard GB / T528-2009;
[0080] Conductivity: A dual-probe desktop digital multimeter was used for testing. The distance between the two probes was fixed and the two probes were placed at both ends of the hydrogel patch. The resistance of the hydrogel patch was obtained by taking the average value. The conductivity of the hydrogel patch was calculated using Formula 2.
[0081]
[0082] In formula 2, G is the conductivity S / m, ρ is the resistivity Ω·m, L is the wire length m, R is the resistance value Ω, and S is the cross-sectional area m 2 .
[0083] Myocardial conductivity: The left anterior descending branch of the coronary artery was ligated in SD rats to prepare an MI rat model. A secondary thoracotomy was performed at an appropriate time to expose the gray-white myocardial infarction area, and a hydrogel patch was implanted to span and cover the myocardial infarction area. The rats were killed after 8 weeks of feeding, and the heart was perfused with cardioplegia solution, and the conductivity of the infarction scar was tested using a four-probe resistivity meter within 30 minutes.
[0084] Table 1. Performance test results of the hydrogel patches obtained in Examples 1 to 3 and Comparative Examples 1 to 2
[0085]
[0086]
[0087] Note: In Table 1, longitudinal direction refers to the measurement parallel to the straight line connecting the two fixed ends of the hydrogel patch during water loss treatment; radial direction refers to the measurement perpendicular to the straight line connecting the two fixed ends.
[0088] As can be seen from Table 1, the double network hydrogel patches prepared in Examples 1 to 3 achieve highly similar simulations of natural myocardial tissue in terms of tensile strength, Young's modulus and conductivity, have excellent anisotropy, and show mechanical and electrical responses similar to real myocardium, which is crucial for replacing or assisting damaged myocardial tissue. However, Comparative Example 1, which did not use dehydration and rehydration treatment, did not have anisotropy because it could not directional arrange the internal fibers of the hydrogel. Comparative Example 2 had a significantly reduced conductivity because it did not contain poly (3-thiopheneacetic acid). Therefore, the present invention successfully prepared a hydrogel patch containing a directional fiber microstructure using the method, which enhanced the strength of the hydrogel while matching the anisotropy of the myocardium, providing innovative ideas and technical support for solving many difficult problems in the field of cardiac tissue engineering.
[0089] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing an anisotropic conductive poly (3-thiopheneacetic acid) / methacrylylated gelatin hydrogel patch, It is characterized in that The following steps are involved: (1) mixing methacryloyl gelatin, poly (3-thiopheneacetic acid), a cross-linking agent and a solvent; 3D printing the obtained mixed solution; and photocuring the obtained 3D printed part to obtain a poly (3-thiopheneacetic acid) / methacryloyl gelatin hydrogel patch; (2) The poly (3-thiopheneacetic acid) / methacrylic acid gelatin hydrogel patch described in step (1) is subjected to dehydration treatment and rehydration treatment in sequence to obtain an anisotropic conductive poly (3-thiopheneacetic acid) / methacrylic acid gelatin hydrogel patch.
2. The preparation method according to claim 1, It is characterized in that In step (1), the molecular weight of the poly (3-thiopheneacetic acid) is 10,000 to 20,000, and the cross-linking agent is a mixture of N,N'-carbonyldiimidazole and photoinitiator 2959.
3. The preparation method according to claim 1, It is characterized in that In step (1), the concentration of the methacrylated gelatin in the mixed solution is 5 to 20 wt %, and the concentration of the poly (3-thiopheneacetic acid) in the mixed solution is 5 to 20 wt %.
4. The preparation method according to claim 2, It is characterized in that The concentration of the N,N'-carbonyldiimidazole in the mixed solution of step (1) is 2-7 wt %, and the concentration of the photoinitiator 2959 in the mixed solution of step (1) is 0.1-0.5 wt %.
5. The preparation method according to claim 1, 3 or 4, It is characterized in that In step (1), the extrusion temperature of the 3D printing is 20-30° C., the extrusion pressure is 80-100 kPa, the printing speed is 0.5-1 mm / s, and the number of printing layers is 1-20 layers.
6. The preparation method according to claim 5, It is characterized in that In step (1), the light intensity of the photocuring is 500 to 1500 mW / cm 2 The light wavelength is 380-420nm and the irradiation time is 30-60s.
7. The preparation method according to claim 1, It is characterized in that In step (2), the initial stress of the dehydration treatment is 10 to 100 kPa, the temperature is 20 to 30° C., the humidity is 30 to 50%, and the time is 24 to 48 hours.
8. The preparation method according to claim 1 or 7, It is characterized in that In step (2), the reagent used for the rehydration treatment is Dulbecco's phosphate buffered saline, the temperature of the rehydration treatment is 20 to 30° C., and the time is 12 to 48 hours.
9. An anisotropic conductive poly (3-thiopheneacetic acid) / methacrylylated gelatin hydrogel patch prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the anisotropic conductive poly (3-thiopheneacetic acid) / methacrylylated gelatin hydrogel patch according to claim 9 in the preparation of myocardial repair materials.
Citation Information
Cited By
Oral rehabilitation membrane material and preparation method thereof
CN121891626A
Oral repair membrane material and method of making same
CN121891626B