Resin composition, insulating resin cured body, laminate, and circuit board
By using a resin composition of thermosetting resin, inorganic filler material, copolymer and inorganic ion capture agent on the metal substrate circuit substrate, the problem of insufficient insulation reliability under high temperature and high humidity is solved, and high voltage for DC is achieved The excellent insulation and reduction of solder cracks improve the application and production efficiency of metal-based circuit substrates.
Patent Information
- Application Number
- CN202380029190.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-15
- Publication Date
- 2024-11-05
AI Technical Summary
Ceramic circuit substrates are prone to solder cracks under high temperature and high humidity conditions, and have insufficient insulation reliability to high DC voltage, which limits its application range and is low in productivity.
A resin composition containing a thermosetting resin, an inorganic filler material, a copolymer and an inorganic ion capture agent is used to form an insulating layer with excellent insulation reliability by optimizing the composition and structure of the composition, and is used to manufacture a metal substrate circuit substrate.
Under high temperature and humidity conditions (85°C, 85%RH), it provides excellent insulation reliability to high DC voltage, reduces the incidence of solder cracks, and improves the application range and productivity of metal-based circuit substrates.
Smart Images

Figure CN118900897A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition suitable for use in the production of an insulating layer of a circuit board (metal base circuit board), an insulating resin cured product, a laminate, and a circuit board. Background Art
[0002] Various circuit boards are now in practical use as circuit boards for forming hybrid integrated circuits by mounting electronic and electrical components such as semiconductor elements. Based on the material of the board, circuit boards are classified into resin circuit boards, ceramic circuit boards, metal base circuit boards, etc.
[0003] Although resin circuit boards are cheap, they are limited to applications that can be used with relatively low power due to the low thermal conductivity of the board. Ceramic circuit boards are suitable for applications that can be used with relatively high power due to the characteristics of ceramics such as high electrical insulation and heat resistance, but they have the disadvantage of being expensive. On the other hand, metal-based circuit boards have a compromise between the two and are suitable for general-purpose applications that can be used with relatively high power, such as inverters for refrigerators, inverters for commercial air conditioners, power supplies for industrial robot arms, and power supplies for automobiles.
[0004] For example, Patent Document 1 discloses a method for obtaining a circuit board having excellent stress relaxation properties, heat resistance, moisture resistance, and heat dissipation properties by using a circuit board composition containing a specific epoxy resin, a curing agent, and an inorganic filler as essential components.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2008-266533 Summary of the invention
[0008] Problems to be solved by the invention
[0009] If a metal-based circuit substrate can be used to replace a ceramic circuit substrate, an increase in productivity can be expected. In addition, there is a problem that solder cracks are easily generated on the substrate during thermal cycles, but by replacing it with a metal-based circuit substrate, it can be expected that the generation of solder cracks can be suppressed. On the other hand, ceramic circuits are suitable for uses that can be used with large amounts of electricity, so when a metal-based circuit substrate is used to replace a ceramic circuit substrate, the metal-based circuit substrate is required to improve the insulation reliability of the metal-based circuit substrate when a DC high voltage is applied (especially the insulation reliability under high temperature and high humidity conditions).
[0010] Therefore, the object of the present invention is to provide a resin composition capable of forming an insulating layer having excellent insulation reliability when a DC high voltage is applied under high temperature and high humidity (85°C, 85%RH) conditions. In addition, the object of the present invention is to provide an insulating resin cured body as a cured body of the resin composition, a laminate and a circuit board using the insulating resin cured body.
[0011] Means for solving problems
[0012] The present invention includes the following aspects.
[0013] (1) A resin composition comprising a thermosetting resin, an inorganic filler, a copolymer, and an inorganic ion scavenger, wherein the copolymer comprises: a (meth)acrylic monomer unit A having an anionic group; a (meth)acrylic monomer unit B having a cationic group; and a (meth)acrylic monomer unit C other than the (meth)acrylic monomer unit A and the (meth)acrylic monomer unit B, and the inorganic ion scavenger comprises both an anion exchanger and a cation exchanger, or comprises a zwitterionic ion exchanger, and the content of the inorganic ion scavenger is 0.1 to 50 parts by mass based on 100 parts by mass of the thermosetting resin.
[0014] (2) The resin composition according to (1), wherein the inorganic filler has a thermal conductivity of 20 W / m·K or more.
[0015] (3) The resin composition according to (1) or (2), wherein the content of the inorganic filler is 30 to 70% by volume based on the total volume of the resin composition.
[0016] (4) The resin composition according to any one of (1) to (3), wherein the inorganic ion scavenger contains at least one selected from the group consisting of Bi, Zr, and Sb.
[0017] (5) The resin composition according to any one of (1) to (4), wherein the inorganic ion scavenger has an average particle size of 0.05 to 10 μm.
[0018] (6) The resin composition according to any one of (1) to (5), wherein the mass ratio of the inorganic ion scavenger to the copolymer is 0.001 to 10000.
[0019] (7) The resin composition according to any one of (1) to (6), which has a peak in the range of 2θ=11 to 15° in X-ray diffraction measurement.
[0020] (8) The resin composition according to any one of (1) to (7), wherein the thermosetting resin is an epoxy resin.
[0021] (9) An insulating resin cured product, which is a cured product of the resin composition according to any one of (1) to (8).
[0022] (10) A laminate comprising: a first metal layer; an insulating layer disposed on one surface of the first metal layer; and a second metal layer disposed on a surface of the insulating layer opposite to the first metal layer, wherein the insulating layer is a cured insulating resin as described in (9).
[0023] (11) A circuit board comprising: a metal layer; an insulating layer arranged on one surface of the metal layer; and a metal circuit portion arranged on a surface of the insulating layer opposite to the metal layer, wherein the insulating layer is a cured insulating resin as described in (9).
[0024] Effects of the Invention
[0025] According to the present invention, a resin composition is provided, which can form an insulating layer having excellent insulation reliability when a DC high voltage is applied under high temperature and high humidity (85°C, 85%RH) conditions. In addition, according to the present invention, an insulating resin cured body as a cured body of the resin composition, a laminate and a circuit board using the insulating resin cured body are provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] [ Figure 1 ] is a cross-sectional view showing one embodiment of a laminate.
[0027] [ Figure 2 ] is a cross-sectional view showing one embodiment of a circuit substrate. DETAILED DESCRIPTION
[0028] Hereinafter, preferred embodiments of the present invention will be described in detail.
[0029] One embodiment of the present invention is a resin composition containing a thermosetting resin, an inorganic filler, a copolymer, and an inorganic ion scavenger.
[0030] As the thermosetting resin, for example, silicone resin, epoxy resin, phenolic resin, cyanate resin, melamine resin, urea resin, thermosetting polyimide resin, and unsaturated polyester resin can be cited. The thermosetting resin may include epoxy resin. The thermosetting resin can be used alone or in combination of two or more.
[0031] From the viewpoint of further improving insulation, the content of the thermosetting resin may be 10% by mass or more, 20% by mass or more, or 25% by mass or more relative to the total mass of the resin composition. From the viewpoint of improving thermal conductivity, the content of the thermosetting resin may be 50% by mass or less, 40% by mass or less, or 30% by mass or less relative to the total mass of the resin composition.
[0032] The inorganic filler material may be, for example, a known inorganic filler material used in applications requiring insulation and thermal conductivity (excluding materials belonging to inorganic ion capture agents described later). The inorganic filler material may include, for example, one or more selected from the group consisting of aluminum oxide (alumina), silicon oxide, silicon nitride, boron nitride, aluminum nitride, and magnesium oxide. From the perspective of better insulation reliability in a high humidity environment, it may include one or more selected from the group consisting of aluminum oxide, silicon oxide, silicon nitride, boron nitride, and aluminum nitride. It may include one or more selected from the group consisting of aluminum oxide, boron nitride, and aluminum nitride.
[0033] The shape of the inorganic filler material can be, for example, a particle, a flaky, a polygonal shape, etc. With regard to the average particle size of the inorganic filler material, from the viewpoint of improving thermal conductivity, it can be 0.05 μm or more, 0.1 μm or more, 5 μm or more, 10 μm or more, 20 μm or more, 30 μm or more, or 40 μm or more, and from the viewpoint of further improving insulation, it can be 200 μm or less, 150 μm or less, 100 μm or less, 80 μm or less, 60 μm or less, or 40 μm or less. In this specification, the average particle size of the inorganic filler material refers to the d50 diameter in the volume-based particle size distribution of the inorganic filler material. The volume-based particle size distribution of the inorganic filler material can be measured using a laser diffraction particle size distribution measuring device.
[0034] The thermal conductivity of the inorganic filler material may be 20 W / m·K or more, 50 W / m·K or more, 100 W / m·K or more, or 150 W / m·K or less, and 35000 W / m·K or less, 2000 W / m·K or less, 600 W / m·K or less, 300 W / m·K or less, or 200 W / m·K or less.
[0035] The inorganic filler material may contain two or more inorganic fillers having different average particle sizes. For example, the inorganic filler material may include a first inorganic filler material having an average particle size of 25 μm or more, and a second inorganic filler material having an average particle size of 4 μm or less. According to such an inorganic filler material, the second inorganic filler material is filled in the gaps between the first inorganic fillers, thereby increasing the filling density and contributing to improving thermal conductivity.
[0036] The average particle size of the first inorganic filler may be 30 μm or 40 μm, or 200 μm or 150 μm. The average particle size of the second inorganic filler may be 3.5 μm or 3 μm, or 0.05 μm or 0.1 μm.
[0037] From the viewpoint of improving thermal conductivity, the content of the inorganic filler relative to the total mass of the resin composition may be 30% by mass or more, 40% by mass or more, 50% by mass or more, or 60% by mass or more. From the viewpoint of further improving insulation, the content of the inorganic filler relative to the total mass of the resin composition may be 80% by mass or less, 75% by mass or less, 70% by mass or less, or 65% by mass or less, and from the viewpoint of obtaining a metal base substrate having better insulation reliability for high voltage under high temperature or high temperature and high humidity environment, it is preferably 65% by mass or less.
[0038] From the viewpoint of improving thermal conductivity, the content of inorganic filler can be 20 volume % or more, 30 volume % or more, 40 volume % or more, 45 volume % or more, or 50 volume % or more relative to the total volume of resin composition. From the viewpoint of further improving insulation, the content of inorganic filler can be 80 volume % or less, 70 volume % or less, 60 volume % or less, 55 volume % or less, or 50 volume % or less relative to the total volume of resin composition, and is preferably 55 volume % or less from the viewpoint of obtaining a metal base substrate having a higher insulation reliability for high voltage under high temperature or high temperature and high humidity environment. The content of inorganic filler can be 20 to 80 volume % or 30 to 70 volume % relative to the total volume of resin composition.
[0039] The copolymer includes: a (meth)acrylic monomer unit A having an anionic group (hereinafter, also referred to as "unit A", and the monomer providing unit A is also referred to as "monomer A"); a (meth)acrylic monomer unit B having a cationic group (hereinafter, also referred to as "unit B", and the monomer providing unit B is also referred to as "monomer B"); and a (meth)acrylic monomer unit C other than the (meth)acrylic monomer unit A and the (meth)acrylic monomer unit B (hereinafter, also referred to as "unit C", and the monomer providing unit C is also referred to as "monomer C"). It should be noted that the copolymer may also include a (meth)acrylic monomer unit (unit X) having both anionic groups and cationic groups. In this case, unit X is regarded as a unit belonging to unit A and also belonging to unit B. In other words, a copolymer having unit X is regarded as a copolymer having both unit A and unit B.
[0040] In this specification, "monomer" refers to a monomer having a polymerizable group before polymerization. "Monomer unit" refers to a structural unit derived from the monomer and constituting a copolymer. "(Meth)acrylic monomer" refers to a monomer having a (meth)acryloyl group. "(Meth)acrylic monomer" refers to an acrylic monomer and its corresponding methacrylic monomer, and similar expressions such as "(meth)acryloyl group" have the same meaning.
[0041] The copolymer has one or more types of unit A, unit B, and unit C. The copolymer may be a random copolymer or a block copolymer. Monomer A, monomer B, and monomer C may each be a monomer having one (meth)acryloyl group (monofunctional (meth)acrylic monomer) or a monomer having two or more (meth)acryloyl groups (multifunctional (meth)acrylic monomer), preferably a monofunctional (meth)acrylic monomer.
[0042] The anionic group possessed by unit A is, for example, one or more selected from the group consisting of a carboxyl group, a phosphoric acid group, a phenolic hydroxyl group, and a sulfonic acid group. From the viewpoint of further improving the dispersibility of the inorganic filler, the anionic group is preferably one or more selected from the group consisting of a carboxyl group, a phosphoric acid group, and a phenolic hydroxyl group.
[0043] From the viewpoint of further improving the dispersibility of the inorganic filler, unit A preferably also has an electron-withdrawing group bonded to the anionic group. The electron-withdrawing group has the effect of stabilizing the anions of the anionic group. As the electron-withdrawing group, for example, a halogen group (also referred to as a halide) can be cited. As the anionic group bonded to the electron-withdrawing group, for example, a group having a halogen group bonded to the α-position carbon atom of the carboxyl group can be cited.
[0044] Unit A may not have an electron donating group bonded to an anionic group. An electron donating group may destabilize the anion of an anionic group. Examples of the electron donating group include a methyl group.
[0045] As monomer A, for example, acrylic acid, methacrylic acid, methacrylic acid (acid phosphoryloxy) propyl ester, acid phosphoryloxy polyoxyethylene glycol monomethacrylate, acid phosphoryloxy polyoxypropylene glycol monomethacrylate, phosphoric acid-modified epoxy acrylate, acid 2-acryloyloxyethyl phosphate, acid 2-methacryloyloxyethyl phosphate, 4-hydroxyphenyl acrylate, 4-hydroxyphenyl methacrylate, succinic acid 2-methacryloyloxyethyl ester, 2-acrylamide-2-methylpropanesulfonic acid, etc. can be cited. From the viewpoint of further improving the dispersibility of the inorganic filler, monomer A is preferably selected from one or more of the group consisting of acrylic acid, 2-methacryloyloxyethyl phosphate, 4-hydroxyphenyl methacrylate, and 2-acrylamide-2-methylpropanesulfonic acid, and more preferably acrylic acid.
[0046] The cationic group contained in the unit B is, for example, one or more selected from the group consisting of a primary amino group, a secondary amino group, a tertiary amino group, and a quaternary ammonium salt group. From the viewpoint of further improving the dispersibility of the inorganic filler, the cationic group is preferably a tertiary amino group.
[0047] From the viewpoint of further improving the dispersibility of the inorganic filler, the unit B preferably further has an electron donating group bonded to the cationic group. The electron donating group has the function of stabilizing the cation of the cationic group. As the electron donating group, for example, a methyl group can be cited. As the cationic group bonded to the electron donating group, for example, a group having a methyl group bonded to the carbon atom at the α position of the amino group can be cited.
[0048] Unit B may not have an electron withdrawing group bonded to a cationic group. An electron withdrawing group may destabilize the cation of a cationic group. Examples of the electron withdrawing group include a carboxyl group.
[0049] As monomer B, for example, 1-aminoethyl acrylate, 1-aminopropyl acrylate, 1-aminoethyl methacrylate, 1-aminopropyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, tert-butylaminoethyl (meth)acrylate, dimethylaminoethyl methacrylate quaternary salt, 1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate, 2,2,6,6-tetramethyl-4-piperidinyl methacrylate, dimethylaminoethyl acrylate benzyl chloride quaternary salt, etc. From the viewpoint of further improving the dispersibility of the inorganic filler, monomer B is preferably selected from one or more of the group consisting of 1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate and 2,2,6,6-tetramethyl-4-piperidinyl methacrylate, and more preferably 1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate.
[0050] Unit C is a (meth) acrylic monomer that does not contain any of a cationic group and an anionic group. Unit C may have an amphiphilic group, a hydrophobic group, or a hydrophilic group in addition to a (meth) acryloyl group. As an amphiphilic group, for example, an oxyalkylene group can be mentioned. As a hydrophobic group, for example, a siloxane group and a hydrocarbon group can be mentioned. As a hydrophilic group, for example, a phosphate group can be mentioned. It should be noted that the so-called hydrocarbon group here does not include a methyl group constituting a methacryloyl group (hereinafter, the same applies to the hydrocarbon group in unit C).
[0051] From the viewpoint of affinity or compatibility between the copolymer and the resin when the resin composition further contains a resin, the unit C has one or more selected from the group consisting of an oxyalkylene group, a siloxane group, and a hydrocarbon group, and more preferably has one or more selected from the group consisting of a siloxane group and a hydrocarbon group.
[0052] Examples of the (meth)acrylic monomer having an oxyalkylene group include ethoxycarbonylmethyl (meth)acrylate, phenol ethylene oxide-modified (meth)acrylate, phenol (modified with 2 mol of ethylene oxide) (meth)acrylate, phenol (modified with 4 mol of ethylene oxide) (meth)acrylate, p-cumylphenol ethylene oxide-modified (meth)acrylate, nonylphenol ethylene oxide-modified (meth)acrylate, nonylphenol (modified with 4 mol of ethylene oxide) (meth)acrylate, nonylphenol (modified with 8 mol of ethylene oxide) (meth)acrylate, nonylphenol (modified with 2.5 mol of propylene oxide)acrylate, 2-ethylhexyl carbitol (meth)acrylate, ethylene oxide-modified phthalic acid (meth)acrylate, ethylene oxide-modified succinic acid (meth)acrylate, and tetrahydrofurfuryl (meth)acrylate.
[0053] Examples of (meth)acrylic monomers having a siloxane group include α-butyl-ω-(3-methacryloxypropyl) polydimethylsiloxane. Examples of (meth)acrylic monomers having a hydrocarbon group include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, phenyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, isobornyl (meth)acrylate, and methoxylated cyclodecatriene (meth)acrylate.
[0054] As a (meth)acrylic-based monomer which has a phosphate group, (meth)acryloyloxyethyl dialkyl phosphate is mentioned, for example.
[0055] Monomer C may be, in addition to the above-mentioned monomers, a (meth)acrylic monomer having a hydroxyl group. Examples of the (meth)acrylic monomer having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, and 3-chloro-2-hydroxypropyl (meth)acrylate.
[0056] Monomer C may be, for example, a (meth)acrylic monomer having an amide bond. Examples of the (meth)acrylic monomer having an amide bond include N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, diacetone(meth)acrylamide, and acryloylmorpholine.
[0057] Monomer C may be, for example, a multifunctional (meth)acrylic monomer. Examples of the multifunctional (meth)acrylic monomer include 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, dicyclopentyl di(meth)acrylate, 2-ethyl-2-butyl-propylene glycol (meth)acrylate, neopentyl glycol-modified trimethylolpropane di(meth)acrylate, stearic acid-modified pentaerythritol di(meth)acrylate, 2-(1,2-cyclohexanedicarboxylic acid imide)ethyl (meth)acrylate, hexanediol di(meth)acrylate, and a multifunctional (meth)acrylate having a bisphenol structure.
[0058] The content of unit A is relative to the total of unit A, unit B and unit C (in other words, the total of all monomer units that copolymer has. The same below.) 100 mol %, can be more than 0.03 mol %, more than 0.1 mol %, more than 0.5 mol %, more than 1 mol %, more than 2 mol %, more than 3 mol %, more than 4 mol % or more than 5 mol %, can be less than 70 mol %, less than 60 mol %, less than 50 mol %, less than 40 mol %, less than 30 mol %, less than 20 mol %, less than 15 mol %, less than 10 mol % or less than 5 mol %.By making the content of unit A be more than 0.03 mol %, there is the tendency that the dispersibility of inorganic filler material further improves.By making the content of unit A be less than 70 mol %, there is the tendency that the viscosity of resin combination further reduces, the operability of resin combination further improves.
[0059] The content of unit B can be more than 0.02 mol %, more than 0.05 mol %, more than 0.07 mol % or more than 0.1 mol % relative to 100 mol % of total of unit A, unit B and unit C, and can be below 20 mol %, below 10 mol %, below 5 mol %, below 3 mol %, below 1 mol %, below 0.5 mol % or below 0.1 mol %.Be more than 0.02 mol % by making the content of unit B, thereby there is the tendency that the affinity of multipolymer and inorganic filler material becomes better.Be below 20 mol % by making the content of unit B, thereby there is the tendency that the viscosity of resin combination further reduces, the operability of resin combination further improves.
[0060] The content of unit C can be more than 10 mol %, more than 20 mol %, more than 30 mol %, more than 40 mol %, more than 50 mol %, more than 60 mol %, more than 70 mol %, more than 80 mol %, more than 90 mol %, more than 92 mol %, or more than 94 mol %, and can be below 99.8 mol %, below 99 mol %, below 98 mol %, below 97 mol %, below 96 mol %, or below 95 mol %.By making the content of unit C be more than 10 mol %, there is a tendency that the viscosity of resin combination further reduces and the operability of resin combination further improves.By making the content of unit C be below 99.8 mol %, there is a tendency that the affinity of copolymer and inorganic filler material becomes better.
[0061] The total of the content of unit A and unit B relative to the total 100 mol % of unit A, unit B and unit C can be more than 0.05 mol %, more than 0.2 mol %, more than 1 mol %, more than 2 mol %, more than 3 mol %, more than 4 mol % or more than 5 mol %, can be below 90 mol %, below 80 mol %, below 70 mol %, below 60 mol %, below 50 mol %, below 40 mol %, below 30 mol %, below 20 mol %, below 10 mol %, below 8 mol % or below 6 mol %.Be more than 0.05 mol % by making the total of the content of unit A and unit B, thereby there is the tendency that the dispersibility of inorganic filler further improves.Be below 90 mol % by making the total of the content of unit A and unit B, thereby there is the tendency that the operability of resin combination further improves.
[0062] The molar ratio of unit A to unit B (unit A / unit B) may be 0.01 or more, 0.9 or more, 1 or more, 5 or more, 10 or more, 20 or more, 30 or more, 40 or more, or 50 or more, and may be 200 or less, 150 or less, 100 or less, 90 or less, 80 or less, 70 or less, 60 or less, 50 or less, 40 or less, 30 or less, 20 or less, 15 or less, or 10 or less. By setting the molar ratio of unit A to unit B within the above range, the dispersibility of the inorganic filler tends to be further improved.
[0063] The weight average molecular weight of the copolymer can be 1,000 or more, 5,000 or more, 7,000 or more, 10,000 or more, 20,000 or more, 30,000 or more, 40,000 or more, or 50,000 or more, and can be 1,000,000 or less, 500,000 or less, 300,000 or less, 100,000 or less, 90,000 or less, 80,000 or less, 70,000 or less, or 60,000 or less. By making the weight average molecular weight of the copolymer 1,000 or more, even when the resin composition is kept for a long time under a high temperature environment, the dispersibility of the inorganic filler can be maintained, and the hardness of the resin composition can be suppressed. In addition, the shape retention of the resin composition is improved, and when applied to an inclined surface or a vertical surface, the offset and drooping of the resin composition are suppressed. By setting the weight average molecular weight of the copolymer to 1,000,000 or less, the viscosity of the resin composition tends to be further reduced and the handleability of the resin composition tends to be further improved. The weight average molecular weight of the copolymer is determined as a weight average molecular weight converted to standard polystyrene using GPC (gel permeation chromatography).
[0064] The copolymer can be obtained by polymerizing the monomer A, the monomer B, and the monomer C by a known polymerization method. Examples of the polymerization method include radical polymerization and anionic polymerization. The polymerization method is preferably radical polymerization.
[0065] The polymerization initiator used in the free radical polymerization may be a thermal polymerization initiator or a photopolymerization initiator. As the thermal polymerization initiator, for example, azo compounds such as azobisisobutyronitrile; and organic peroxides such as benzoyl peroxide, tert-butyl hydroperoxide, and di-tert-butyl peroxide may be mentioned. As the photopolymerization initiator, for example, benzoin derivatives may be mentioned. The polymerization initiator may also be a known polymerization initiator used in living free radical polymerization such as ATRP and RAFT.
[0066] The polymerization conditions can be appropriately adjusted according to the type of monomer, polymerization initiator, etc. When the copolymer is a random copolymer, each monomer can be pre-mixed and polymerized. When the copolymer is a block copolymer, each monomer can be added to the polymerization system in sequence.
[0067] The content of the copolymer is 0.01 to 10 parts by mass relative to 100 parts by mass of the inorganic filler. By making the content of the copolymer within this range, a resin composition capable of forming an insulating layer having excellent insulation reliability for DC high voltage application under high temperature and high humidity (85°C, 85%RH) conditions can be obtained. The content of the copolymer can be 0.05 parts by mass or more, 0.1 parts by mass or more, 0.5 parts by mass or more, 1 parts by mass or more, 2 parts by mass or more, 3 parts by mass or more, or 4 parts by mass or more relative to 100 parts by mass of the inorganic filler, and can be 9 parts by mass or less, 8 parts by mass or less, 7 parts by mass or less, 6 parts by mass or less, 5 parts by mass or less, or 4 parts by mass or less.
[0068] The content of the copolymer can be 0.1 mass % or more, 0.5 mass % or more, 1 mass % or more, 2 mass % or more, or 2.5 mass % or more, and can be 10 mass % or less, 8 mass % or less, 6 mass % or less, 5 mass % or less, 4 mass % or less, or 3 mass % or less, relative to the total mass of the resin composition.
[0069] Inorganic ion capture agents are inorganic materials that have the function of capturing at least one of cations and anions (having ion capture properties). In this specification, the so-called "ion capture properties" refer to: the property of adsorbing the ions of the capture object on the surface of the inorganic material; or the property of introducing the ions of the capture object into the structure of the inorganic material through ion exchange between the ions in the structure of the inorganic material and the ions of the capture object. As the ions of the capture object of the inorganic ion capture agent, cations such as Na ions, Cu ions, and Ag ions; and anions such as Cl ions and Br ions can be cited.
[0070] The inorganic ion capture agent includes both anion exchangers and cation exchangers, or includes zwitterion exchangers. Anion exchangers are inorganic materials that capture anions, cation exchangers are inorganic materials that capture cations, and zwitterion exchangers are inorganic materials that capture both anions and cations. The inorganic ion capture agent can be used alone or in the form of a combination of two or more, for example, the inorganic ion capture agent can include multiple anion exchangers, multiple cation exchangers, or multiple zwitterion exchangers.
[0071] The inorganic ion scavenger may include, for example, at least one selected from the group consisting of Al, Mg, Bi, Zr, Sb, Sn, Ti, and Zn, or may include at least one selected from the group consisting of Bi, Zr, and Sb. The inorganic ion scavenger may include, for example, an oxide, an oxychloride, and a hydrate thereof containing at least one of these metal elements. The inorganic ion scavenger may include two or more of these metal elements.
[0072] As the anion exchanger, there can be mentioned an inorganic material containing at least one selected from the group consisting of Al, Mg, Bi, Zr, and Zn. As the anion exchanger, specifically, there can be mentioned IXE-500 (Bi system), IXE-530 (Bi system), IXE-550 (Bi system), IXE-700 (Mg, Al system), IXE-700F (Mg, Al system), IXE-770 (Mg, Al system), IXE-770D (Mg, Al system), IXE-702 (Al system), IXE-800 (Zr system), IXE-1000 (Zn system) (all manufactured by Toagosei Co., Ltd.), etc.
[0073] As the cation exchanger, there can be mentioned an inorganic material containing at least one selected from the group consisting of Zr, Sn, and Ti. Specific examples of the cation exchanger include IXE-100 (Zr series), IXE-200 (Sn series), IXE-300 (Sb series), IXE-400 (Ti series) (all manufactured by Toagosei Co., Ltd.), etc.
[0074] Examples of the zwitterionic ion exchanger include inorganic materials containing at least one selected from the group consisting of Al, Mg, Bi, Zr, and Sb. Specifically, examples of the zwitterionic ion exchanger include IXE-1320 (Mg, Al series), IXE-600 (Sb, Bi series), IXE-633 (Bi series), IXE-680 (Bi series), IXE-6107 (Zr, Bi series), IXE-6136 (Zr, Bi series), IXEPLAS-A1 (Zr, Mg, Al series), IXEPLAS-A2 (Zr, Mg, Al series), and IXEPLAS-B1 (Zr, Bi series) (all manufactured by Toagosei Co., Ltd.).
[0075] The average particle size of the inorganic ion scavenger can be 0.05 μm or more, 0.1 μm or more, 0.15 μm or more, 0.2 μm or more, 0.3 μm or more, 0.4 μm or more, or 0.5 μm or more, and can be 10 μm or less, 5 μm or less, 3 μm or less, 2 μm or less, 1.5 μm or less, or 1 μm or less. The average particle size of the inorganic ion scavenger can be 0.05 to 10 μm. The average particle size of the inorganic ion scavenger can be measured by laser diffraction and scattering method.
[0076] The content of at least one inorganic ion scavenger selected from the group consisting of Bi, Zr, and Sb can be 80 mass % or more, 90 mass % or more, or 95 mass % or more relative to the total mass of the inorganic ion scavenger. The content of at least one inorganic ion scavenger selected from the group consisting of Bi, Zr, and Sb can be substantially 100 mass % relative to the total mass of the inorganic ion scavenger.
[0077] The content of the inorganic ion scavenger is 0.1 to 50 parts by mass relative to 100 parts by mass of the total of the thermosetting resin and the copolymer. From the viewpoint of obtaining a resin composition capable of forming an insulating layer having a more excellent insulation reliability for the application of a DC high voltage under high temperature and high humidity (85°C, 85%RH) conditions, the content of the inorganic ion scavenger can be 0.3 parts by mass or more, 0.5 parts by mass or more, 1 part by mass or more, 2 parts by mass or more, 3 parts by mass or more, or 4 parts by mass or more relative to 100 parts by mass of the total of the thermosetting resin and the copolymer, and can be 40 parts by mass or less, 30 parts by mass or less, 20 parts by mass or less, 15 parts by mass or less, or 10 parts by mass or less.
[0078] When the inorganic ion scavenger contains both an anion exchanger and a cation exchanger, from the viewpoint of obtaining a resin composition capable of forming an insulating layer having better insulation reliability when a DC high voltage is applied under high temperature and high humidity (85°C, 85% RH) conditions, the mass ratio of the cation exchanger to the anion exchanger (the mass-based content of the cation exchanger / the mass-based content of the anion exchanger) can be 0.001 or more, 0.01 or more, 0.1 or more, or 1000 or less, 10 or less, or 5 or less.
[0079] From the viewpoint of obtaining a resin composition capable of forming an insulating layer having better insulation reliability for application of a DC high voltage under high temperature and high humidity (85°C, 85% RH) conditions, the content of the inorganic ion scavenger can be 0.05% by mass or more, 0.1% by mass or more, 0.5% by mass or more, 1% by mass or more, 1.2% by mass or more, or 1.4% by mass or more, and can be 30% by mass or less, 20% by mass or less, 15% by mass or less, 10% by mass or less, 8% by mass or less, 6% by mass or less, or 4% by mass or less, relative to the total mass of the resin composition.
[0080] From the viewpoint of obtaining a resin composition capable of forming an insulating layer having better insulation reliability for DC high voltage application under high temperature and high humidity (85°C, 85% RH) conditions, the mass ratio of the inorganic ion scavenger to the copolymer (the content of the inorganic ion scavenger based on the mass basis / the content of the copolymer based on the mass basis) may be 0.005 or more, 0.01 or more, or 0.05 or more, and may be 1000 or less, 100 or less, or 50 or less. The mass ratio of the inorganic ion scavenger to the copolymer may be 25 or less, 10 or less, 5 or less, or 3 or less. The mass ratio of the inorganic ion scavenger to the copolymer may be 0.001 to 10000.
[0081] The resin composition may further contain a curing agent for curing the thermosetting resin. The curing agent is appropriately selected according to the type of the thermosetting resin. For example, as a curing agent in the case where the thermosetting resin is an epoxy resin, amine resins, anhydride resins, and phenolic resins can be cited. The curing agent can be used alone or in combination of two or more.
[0082] The content of the curing agent may be 1% by mass or more or 3% by mass or more, and may be 10% by mass or less or 5% by mass or less, based on the total mass of the resin composition.
[0083] The resin composition may further contain other components. Examples of other components include a curing accelerator, a coupling agent, a leveling agent, an antioxidant, a defoaming agent, a wetting agent, a dispersant, and a stabilizer.
[0084] The resin composition is obtained by mixing a thermosetting resin, an inorganic filler, a copolymer, and an inorganic ion scavenger (and a curing agent and other components as needed). The mixing can be carried out using, for example, a planetary mixer, a universal mixer, a kneader, a hybrid mixer, or the like.
[0085] The resin composition may have a peak in the range of 2θ=11 to 15° in X-ray diffraction measurement. The peak position in the X-ray diffraction measurement of the resin composition can be confirmed, for example, by preparing a cured product of the resin composition and subjecting the cured product to X-ray diffraction measurement. The resin composition may have a peak at a position of 2θ=11.5 to 14.5 or 11.8 to 14 in X-ray diffraction measurement.
[0086] The resin composition described above can be cured for example and used. That is, one embodiment of the present invention is a cured product (insulating resin cured product) of the above-mentioned resin composition. The cured product can be in a semi-cured state (B stage) or in a fully cured state (C stage).
[0087] The cured product can be obtained, for example, by heat treating the above-mentioned resin composition to cure it. The conditions of the heat treatment (heating temperature, heating time, etc.) can be appropriately set according to the types of resin and curing agent, the desired curing state, etc. The heat treatment can be carried out in one stage or in two stages.
[0088] The cured product may be, for example, in the form of a sheet. The cured product may be obtained, for example, by applying the resin composition to a substrate and heating (and pressurizing as required). The cured product may be a B-stage sheet in a semi-cured state or a C-stage sheet in a fully cured state.
[0089] The above-mentioned resin composition and its cured product can be suitably used to form an insulating layer of a metal-based substrate. That is, the above-mentioned resin composition and its cured product can also be referred to as a resin composition for a metal-based substrate and a cured product for a metal-based substrate, respectively.
[0090] Figure 1 Schematic cross-sectional view showing one embodiment of a laminate. Figure 1 As shown, a laminated body 10A according to one embodiment includes: a first metal layer 1A; an insulating layer (a cured product of the above-mentioned resin composition) 2 disposed on one surface of the first metal layer; and a second metal layer 3A disposed on the surface of the insulating layer 2 opposite to the first metal layer. In the laminated body 10A, the first metal layer 1A and the second metal layer 3A are separated by the insulating layer 2 and are electrically insulated from each other.
[0091] As the metal material constituting the first metal layer 1A, for example, aluminum, aluminum alloy, copper, copper alloy, iron, and stainless steel can be cited. The first metal layer 1A can be composed of one metal material, or can be composed of two or more metal materials. The first metal layer 1A can be a single-layer structure, or can be a multi-layer structure.
[0092] Examples of the metal material constituting the second metal layer 3A include copper, aluminum, and nickel. The second metal layer 3A may be composed of one metal material or two or more metal materials. The second metal layer 3A may be a single-layer structure or a multi-layer structure. Figure 1 In the embodiment, the second metal layer 3A is arranged on substantially the entire surface of the insulating layer 2 , but the second metal layer may be arranged only on a portion of the insulating layer 2 .
[0093] The thickness of the first metal layer 1A may be, for example, 0.5 mm or more and 3 mm or less. The thickness of the insulating layer 2 may be, for example, 50 μm or more and 300 μm or less. The thickness of the second metal layer 3A may be, for example, 5 μm or more and 1 mm or less.
[0094] Figure 2 Schematic cross-sectional view showing one embodiment of a circuit substrate. Figure 2 As shown, a circuit board 10B according to one embodiment includes: a metal layer 1B; an insulating layer (a cured product of the above-mentioned resin composition) 2 disposed on one surface of the metal layer 1B; and a metal circuit portion 3B disposed on the surface of the insulating layer 2 opposite to the metal layer 1B. In the circuit board 10B, the metal circuit portion 3B is, for example, a circuit processed (e.g., etched) into a predetermined pattern.
[0095] The metal material constituting the metal layer 1B may be the same as the metal material constituting the first metal layer 1A. The metal material constituting the metal circuit portion 3B may be the same as the metal material constituting the second metal layer 3A.
[0096] The thickness of the metal layer 1B may be, for example, 0.5 mm or more and 3 mm or less. The thickness of the insulating layer 2 may be, for example, 50 μm or more and 300 μm or less. The thickness of the metal circuit portion 3B may be, for example, 5 μm or more and 1 mm or less.
[0097] Example
[0098] Hereinafter, the present invention will be described in more detail using examples, but the present invention is not limited to these examples.
[0099] <Synthesis of copolymer>
[0100] The monomers used in the synthesis of the copolymers of the Examples are shown below.
[0101] ((Meth)acrylic monomer A having anionic group)
[0102] ·Acrylic acid (manufactured by Toagosei Co., Ltd.)
[0103] ((Meth)acrylic monomer B having a cationic group)
[0104] ·1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate ("ADEKA STAB LA-82" manufactured by ADEKA Co., Ltd.)
[0105] ((Meth)acrylic acid monomer C)
[0106] Benzyl methacrylate ("LIGHT ESTER BZ" manufactured by Kyoeisha Chemical Co., Ltd.)
[0107] First, 100 parts by mass of (meth)acrylic acid monomers containing 5 mol% of acrylic acid, 0.1 mol% of 1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate, and 94.9 mol% of benzyl methacrylate were added to an autoclave equipped with a stirrer. Next, 0.5 parts by mass of azobisisobutyronitrile (manufactured by Tokyo Chemical Industry Co., Ltd.) as an initiator (relative to 100 parts by mass of the total (meth)acrylic acid monomers) and 1000 parts by mass of a mixed solution of toluene (reagent special grade) and 2-propanol (reagent special grade) as a solvent (toluene:2-propanol=7:3 (volume ratio)) were added, and the inside of the autoclave was replaced with nitrogen. Then, the autoclave was heated at 65°C in an oil bath for 20 hours to perform free radical polymerization. After the polymerization was completed, deaeration was carried out at 120°C for 1 hour under reduced pressure to obtain a copolymer.
[0108] The polymerization rate with respect to 100% of the input amount of the monomers was analyzed by gas chromatography and the result was 98% or more. From this, it is estimated that the ratio of each monomer unit in the copolymer is about the same as the input ratio of the monomers.
[0109] The weight average molecular weight of the obtained copolymer 1 was determined as a weight average molecular weight in terms of standard polystyrene by GPC (gel permeation chromatography). The measurement conditions were as follows.
[0110] High-efficiency GPC device: Tosoh Corporation's "HLC-8020"
[0111] Chromatographic columns: 1 "TSK guardcolumn MP (×L)" 6.0 mm ID × 4.0 cm manufactured by Tosoh Corporation, and 2 "TSK-GELMULTIPOREHXL-M" 7.8 mm ID × 30.0 cm manufactured by Tosoh Corporation (theoretical plate number is 16,000), a total of 3 columns (theoretical plate number as a whole is 32,000)
[0112] Developing solvent: tetrahydrofuran
[0113] Detector: RI (differential refractometer)
[0114] <Preparation of resin composition>
[0115] (Example 1)
[0116] 27.9 mass % of naphthalene epoxy resin HP-4032D (manufactured by DIC Corporation) as a thermosetting resin and 3.5 mass % of phenol Novolac resin VH-4150 (manufactured by DIC Corporation) as a curing agent were stirred at 170° C. to dissolve the curing agent in the thermosetting resin. A resin composition was prepared by using a planetary mixer to stir and mix a resin in which a curing agent was dissolved, 64.4 mass % (50 volume %) of a boron nitride filler (manufactured by Denka, with an average particle size of 40 μm and a thermal conductivity of 150 W / m·K) as an inorganic filler, 2.6 mass % (4 phf) of a copolymer, 1.4 mass % (4.5 phr) of an inorganic ion scavenger 1 (IXEPLAS-B1 (Zr, Bi series), with an average particle size of 0.4 μm, manufactured by Toagosei Co., Ltd.) as an inorganic ion scavenger, and 0.2 mass % of 1B2PZ (manufactured by Shikoku Chemicals Co., Ltd.) as a curing accelerator.
[0117] <Production of solidified body>
[0118] The obtained resin composition was applied onto a polyethylene terephthalate (PET) film having a thickness of 0.038 mm so as to have a thickness of 0.20 mm after curing, and dried by heating at 100° C. for 50 minutes to prepare a semi-cured body (B-stage state sheet).
[0119] <Manufacturing of Metal-Based Circuit Boards>
[0120] The prepared solidified body (sheet in the B stage state) was peeled off from the PET film and placed on the rough surface of a metal plate (copper plate with a thickness of 2.0 mm). The rough surface of a metal foil (copper foil with a thickness of 0.5 mm) was placed on the solidified body and heated and cured at 180°C for 410 minutes while applying a surface pressure of 10 MPa using a pressing machine.
[0121] Next, after masking a predetermined position with a resist, the copper foil was etched using a sulfuric acid-hydrogen peroxide mixed solution as an etching solution. The resist was removed, and the mixture was cleaned and dried to obtain a metal base circuit board having a circular electrode (copper foil) with a diameter of 20 mm.
[0122] (Example 2)
[0123] A resin composition, a cured product, and a metal base circuit board were prepared in the same manner as in Example 1 except that Inorganic Ion Scavenger 2 (IXE-600 (Sb, Bi system), average particle size 1.0 μm, manufactured by Toagosei Co., Ltd.) was used as the inorganic ion scavenger.
[0124] (Example 3)
[0125] A resin composition, a cured product, and a metal base circuit board were prepared in the same manner as in Example 1 except that Inorganic Ion Scavenger 3 (IXE-6107 (Zr, Bi system), average particle size 1.5 μm, manufactured by Toagosei Co., Ltd.) was used as the inorganic ion scavenger.
[0126] (Examples 4 to 9)
[0127] Except that the addition amount of the inorganic ion scavenger or the copolymer was changed as shown in Tables 1 and 2, a resin composition, a cured product, and a metal base circuit board were prepared in the same manner as in Example 1.
[0128] (Comparative Examples 1 to 4)
[0129] Except that the addition amount of the inorganic ion scavenger or the copolymer was changed as shown in Table 3, a resin composition, a cured product, and a metal base circuit board were prepared in the same manner as in Example 1.
[0130] (Comparative Example 5)
[0131] A resin composition, a cured product, and a metal base circuit board were prepared in the same manner as in Example 1 except that Inorganic Ion Scavenger 4 (IXE-550 (Bi-based), average particle size 1.5 μm, manufactured by Toagosei Co., Ltd.) was used as the inorganic ion scavenger.
[0132] (Comparative Example 6)
[0133] A resin composition, a cured product, and a metal base circuit board were prepared in the same manner as in Example 1 except that Inorganic Ion Scavenger 5 (IXE-100 (Zr-based), average particle size 1.0 μm, manufactured by Toagosei Co., Ltd.) was used as the inorganic ion scavenger.
[0134] [Determination of XRD peaks]
[0135] The cured products prepared in the examples and comparative examples were subjected to X-ray diffraction measurement using an X-ray diffractometer "Rigaku MiniFlexII" manufactured by Rigaku Co., Ltd. The positions of XRD peaks detected in the range of 2θ=11 to 15° are shown in Tables 1 to 4.
[0136] [Reliability evaluation based on high temperature and high humidity bias test (THB)]
[0137] The obtained metal base substrate was subjected to a high temperature and high humidity bias test (THB), which measured the time until insulation breakdown under the test condition of applying a DC voltage of 2.0 kV between the metal foil and the metal plate at 85°C and 85% RH. The time until insulation breakdown was defined as the time from the start of voltage application until the leakage current value measured by a withstand voltage tester became 10 mA or more.
[0138] [Table 1]
[0139]
[0140] [Table 2]
[0141]
[0142] [Table 3]
[0143]
[0144] Description of Reference Numerals
[0145] 1A...first metal layer, 1B...metal layer, 2...insulating layer, 3A...second metal layer, 3B...metal circuit portion, 10A...laminated body, 10B...circuit board.
Claims
1. A resin composition comprising a thermosetting resin, an inorganic filler, a copolymer, and an inorganic ion scavenger, The copolymer comprises: a (meth)acrylic acid monomer unit A having an anionic group; a (meth)acrylic acid monomer unit B having a cationic group; and a (meth)acrylic acid monomer unit C other than the (meth)acrylic acid monomer unit A and the (meth)acrylic acid monomer unit B. The inorganic ion scavenger includes both an anion exchanger and a cation exchanger, or includes an amphoteric ion exchanger. The content of the inorganic ion scavenger is 0.1 to 50 parts by mass based on 100 parts by mass of the total of the thermosetting resin and the copolymer. The content of the copolymer is 0.01 to 10 parts by mass based on 100 parts by mass of the inorganic filler.
2. The resin composition according to claim 1, wherein The thermal conductivity of the inorganic filler material is greater than 20 W / m·K.
3. The resin composition according to claim 1 or 2, wherein The content of the inorganic filler is 30 to 70 volume % relative to the total volume of the resin composition.
4. The resin composition according to any one of claims 1 to 3, wherein The inorganic ion scavenger includes at least one selected from the group consisting of Bi, Zr, and Sb.
5. The resin composition according to any one of claims 1 to 4, wherein The average particle size of the inorganic ion scavenger is 0.05 to 10 μm.
6. The resin composition according to any one of claims 1 to 5, wherein The mass ratio of the inorganic ion scavenger to the copolymer is 0.001 to 10000. 7 . The resin composition according to claim 1 , which has a peak in the range of 2θ=11 to 15° in X-ray diffraction measurement.
8. The resin composition according to any one of claims 1 to 7, wherein The thermosetting resin is epoxy resin. 9 . An insulating resin cured product, which is a cured product of the resin composition according to claim 1 .
10. A laminate comprising: a first metal layer; an insulating layer disposed on one surface of the first metal layer; and a second metal layer disposed on a surface of the insulating layer opposite to the first metal layer, The insulating layer is the insulating resin cured body according to claim 9.
11. A circuit board comprising: a metal layer; an insulating layer disposed on one surface of the metal layer; and a metal circuit portion disposed on a surface of the insulating layer opposite to the metal layer, The insulating layer is the insulating resin cured body according to claim 9.