Preparation method of multifunctional finishing agent for brocade / spandex fabric
By synthesizing a multifunctional finishing agent with reaction of epoxy groups and amino groups, the problem of rough feel of Jinmin fabrics is solved, and the excellent moisture absorption and quick drying properties and smooth and fluffy feel of the fabrics are achieved, simplifying the preparation process and improving resistance Water-washing fastness, suitable for industrial production.
Patent Information
- Application Number
- CN202410890168.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-08
AI Technical Summary
The existing multi-functional finishing agent for bronchymime fabrics improves hydrophilicity and quick-drying properties, which leads to hard and rough feel, affecting the practicality of the fabric, and is difficult to prepare, high reaction temperature and affecting production efficiency.
Intermediate Y is synthesized by reaction of isopropyl alcohol, single-ended epoxy-capped silicone and double-ended amino polyethylene glycol, followed by substances such as acetone, polyethylene glycol, butanone oxime and hexamethylene diisocyanate. Carry out reactions, introduce silicone segments and chain extensions to regulate molecular weight, and form a multifunctional finishing agent with reaction of epoxy groups and amino groups. It is suitable for cross-linking reactions during high-temperature setting and improve film formation.
It realizes good moisture absorption, quick drying and smooth and fluffy feel of bronchiam fabrics, improves the versatility and water-resistant fastness of the fabrics, simplifies the preparation process, reduces energy consumption, and is suitable for industrial production.
Smart Images

Figure FT_1 
Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method of a multifunctional finishing agent for nylon-spandex fabrics, and in particular to a multifunctional finishing agent for nylon-spandex fabrics, which can greatly improve the hydrophilicity and quick-drying property of nylon-spandex fabrics and at the same time give the fabrics good smooth and fluffy hand feel. Background Art
[0002] With the continuous development of textile technology and the change of people's consumption concepts, there are higher requirements for the functionality, comfort, health, environmental protection and health care of fabrics. Nylon-spandex fabrics combine the advantages of nylon and spandex. Nylon provides strength and wear resistance, while spandex gives the fabric excellent elasticity. Therefore, nylon-spandex fabrics can well adapt to the needs of various parts of the body. This high elasticity makes nylon-spandex fabrics have unique advantages in clothing production, especially in sportswear that requires a high degree of fit and stretch. However, higher requirements are placed on the multifunctional performance of nylon-spandex fabrics.
[0003] As is known to all, hydrophilicity can be imparted to fabrics by copolymerization or co-spinning with hydrophilic components, graft polymerization, post-finishing processing, and changing the surface physical structure of the fiber. Among them, post-finishing processing is less difficult, more efficient, and more widely applicable. Currently, the multifunctional agents for nylon-spandex fabrics mostly rely on adipic acid, hexamethylenediamine, and long-chain polyethylene glycol as the main reactants. Using the principle of structural similarity, the amide segments in the molecular structure of the finishing agent can form eutectics with the fiber molecular chains under high-temperature setting conditions, and the polyethylene glycol segments can be embedded in the fabric surface, making the finished nylon-spandex fabric multifunctional. This type of multifunctional finishing agent can give nylon-spandex fabrics a certain degree of multifunctionality, but it is difficult to prepare, and the reaction temperature often needs to be above 180°C. At the same time, the molecular segments in this type of multifunctional agent form eutectics with the fiber molecular chains, which will cause the nylon-spandex fabric to feel hard and rough, affecting the practicality of nylon-spandex fabrics.
[0004] Therefore, it is an urgent need to develop a multifunctional finishing agent for nylon-spandex fabrics to improve the hydrophilicity and quick-drying properties of nylon-spandex fabrics and at the same time give them a smooth and fluffy feel. Summary of the invention
[0005] In view of the above technical problems existing in the multifunctional finishing of nylon-spandex fabrics, the present invention provides a method for preparing a multifunctional finishing agent for nylon-spandex fabrics.
[0006] To achieve the above object, the present invention prepares a multifunctional finishing agent for nylon-spandex fabric having the following general structural formula:
[0007] Among them, 52≤a≤84 and a is an integer; 32≤b≤72 and b is an integer; 32≤c≤72 and c is an integer; m, n>1, and are integers.
[0008] The preparation method of the multifunctional finishing agent having the above structural formula is as follows: Synthesis of intermediate Y According to the mass proportion, 20-25 parts of isopropanol are added to a reaction vessel equipped with a condensation reflux device, stirring is started, 80-100 parts of single-end epoxy-terminated silicone and 10-20 parts of double-terminated amino polyethylene glycol are added to the reaction vessel respectively, the temperature is raised to 60-65°C, and the temperature is kept for reaction for 5-6 hours. After the reaction is completed, the temperature is raised to 80-85°C, and the isopropanol is removed and recovered by vacuum distillation to obtain intermediate Y. The synthesis route is as follows: Among them, 52≤a≤84 and a is an integer; 32≤b≤72 and b is an integer.
[0009] Synthesis and preparation of finishing agents The mixture is prepared by mass proportioning, adding 30-50 parts of acetone to a reaction vessel equipped with a condensation reflux device, starting stirring, and sequentially adding 25-35 parts of intermediate Y, 10-20 parts of polyethylene glycol, 0.1-0.5 parts of butanone oxime and 1-5 parts of hexamethylene diisocyanate to the reaction vessel, heating to 80-85°C, adding 0.1-0.2 parts of dibutyltin dilaurate, and keeping the temperature for reaction for 2-3 hours. After the reaction is completed, adding 450-650 parts of water to the reaction vessel, stirring fully for 30-40 minutes, and removing and recovering acetone by vacuum distillation to obtain a multifunctional finishing agent for nylon-spandex fabrics. The synthesis route is as follows:
[0010] Among them, 32≤c≤72 and c is an integer; m, n>1, and are integers.
[0011] Due to the application of the above technical solution, the present invention has the following advantages: In order to make the finished nylon-spandex fabric have both good hygroscopicity and quick-drying properties and good smooth and fluffy feel, the present invention introduces silicone segments into the side chains of polyethylene glycol segments through the reaction of epoxy groups and amino groups; on the one hand, the ratio of polyethylene glycol to polyethylene glycol containing silicone side chains is regulated, and on the other hand, the molecular weight is regulated by regulating the chain extension of hexamethylene diisocyanate, so that the multifunctional finishing agent can achieve the best performance in terms of hygroscopicity, quick-drying and smooth and fluffy feel; similarly, the preparation method provided by the present invention can purposefully regulate the hygroscopicity, quick-drying properties and smooth and fluffy feel according to the needs of different nylon-spandex fabrics. The molecular structure of the finishing agent obtained by the present invention contains carbamate or substituted urea segments formed by hexamethylene diisocyanate and hydroxyl or secondary amine groups, which has a similar structure to nylon and spandex, and has a strong adsorption effect on nylon-spandex fabrics; at the same time, part of the isocyanate groups (-NCO) blocked by butanone oxime will be unblocked and re-crosslinked during the high-temperature setting process of 170°C, thereby enhancing the film-forming effect of the multifunctional finishing agent and greatly improving the washing fastness of the multifunctional finishing effect of nylon-spandex fabrics. The process of the present invention is relatively simple, the reaction raw materials are easy to obtain, the reaction process is easy to control, and the energy consumption is low, which is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS Attached Figure 1 This is an infrared spectrum of a multifunctional finishing agent for nylon-spandex fabrics in Example 1 of the present invention. DETAILED DESCRIPTION
[0012] The present invention will be further described below in conjunction with embodiments: Embodiment 1: Weigh 20 g of isopropanol and add it to a reaction container equipped with a condensation reflux device, start stirring, then weigh 80 g of single-end epoxy-terminated silicone (number average molecular weight of 4000) and 10 g of double-end amino polyethylene glycol (number average molecular weight of 1000) and add them to the reaction container respectively, raise the temperature to 65°C, keep the temperature for 6 hours, and after the reaction is completed, remove and recover the isopropanol by distillation under reduced pressure to obtain intermediate Y1; 30 g of acetone was weighed and added to a reaction vessel equipped with a condensing reflux device, and stirring was started. 25 g of intermediate Y1, 10 g of polyethylene glycol (number average molecular weight of 1000), 0.2 g of butanone oxime and 2.1 g of hexamethylene diisocyanate were weighed and added to the reaction vessel, the temperature was raised to 80°C, and 0.15 g of dibutyltin dilaurate was added. The temperature was kept for 3 hours. After the reaction was completed, 450 g of water was added to the reaction vessel, and the mixture was fully stirred for 30 min. Then, the vacuum degree was maintained at 0.09 atm, and the acetone was removed and recovered by reduced pressure distillation to obtain the product, which was a multifunctional finishing agent M1.
[0013] Embodiment 2: Weigh 20g of isopropanol and add it to a reaction container equipped with a condensation reflux device, start stirring, then weigh 80g of single-end epoxy-terminated silicone (number average molecular weight of 4000) and 15g of double-end amino polyethylene glycol (number average molecular weight of 1500) and add them to the reaction container respectively, raise the temperature to 65°C, keep the temperature for 6h, and after the reaction is completed, remove and recover the isopropanol by reduced pressure distillation to obtain intermediate Y2; 40 g of acetone was weighed and added to a reaction vessel equipped with a condensing reflux device, and stirring was started. 28 g of intermediate Y2, 15 g of polyethylene glycol (number average molecular weight of 1500), 0.3 g of butanone oxime and 2.2 g of hexamethylene diisocyanate were weighed and added to the reaction vessel. The temperature was raised to 85°C, and 0.15 g of dibutyltin dilaurate was added. The reaction was kept warm for 2 hours. After the reaction was completed, 540 g of water was added to the reaction vessel, and the mixture was fully stirred for 30 minutes. The acetone was then removed and recovered by distillation under reduced pressure to obtain the product, which was a multifunctional finishing agent M2.
[0014] Embodiment 3: Weigh 25 g of isopropanol and add it to a reaction container equipped with a condensation reflux device, start stirring, then weigh 100 g of single-end epoxy-terminated silicone (number average molecular weight of 5000) and 15 g of double-end amino polyethylene glycol (number average molecular weight of 1500) and add them to the reaction container respectively, raise the temperature to 65°C, keep the temperature for 6 hours, and after the reaction is completed, remove and recover the isopropanol by distillation under reduced pressure to obtain intermediate Y3; 50 g of acetone was weighed and added to a reaction vessel equipped with a condensing reflux device, and stirring was started. 32 g of intermediate Y3, 15 g of polyethylene glycol (number average molecular weight of 1500), 0.4 g of butanone oxime and 2.4 g of hexamethylene diisocyanate were weighed and added to the reaction vessel. The temperature was raised to 85°C, and 0.15 g of dibutyltin dilaurate was added. The reaction was kept warm for 3 hours. After the reaction was completed, 650 g of water was added to the reaction vessel, and the mixture was fully stirred for 30 minutes. The acetone was then removed and recovered by distillation under reduced pressure to obtain the product, which was a multifunctional finishing agent M3.
[0015] The attached figure is the infrared spectrum of the multifunctional finishing agent, at 3350cm -1 The absorption peak at 1720 cm is the stretching vibration peak of NH in the carbamate bond. -1 The strong absorption peak near 1535cm is the stretching vibration peak of C=O in the carbamate bond, while -1 The absorption peaks nearby belong to the carbamate bond NH and N-COOC. 1055 cm -1 The strong absorption peak near 960 cm -1 With 800 cm -1The absorption peak at 40° belongs to the vibration peak of Si-C. The group structure shown in the infrared spectrum is consistent with the design of the multifunctional finishing agent.
[0016] Performance Testing 1) Fabrics and auxiliaries Fabric: Black nylon-spandex blended woven fabric (spandex content 20%), weight 190~200 g / m 2 Auxiliary agent: Example 1: M1, Example 2: M2, Example 3: M3, Comparison sample 1: NL-622, Comparison sample 2: PM-226 2) Application process and testing Moisture absorption and quick-drying performance: Cut and weigh black nylon-spandex blended woven fabric, prepare dye liquor according to bath ratio of 1:10 and multifunctional agent dosage of 2g / L, heat to 80℃ in dyeing machine at a heating rate of 1℃ / min, keep warm for 30 minutes, dehydrate by centrifuge, set in heat setting machine (setting temperature 170℃, 60s), and then rehydrate in constant temperature and humidity room for 2h, and test and evaluate various multifunctional properties of fabric according to the test method of GB / T21655.1-2023 Evaluation of moisture absorption and quick-drying property of textiles Part 1: Single combination test method. The moisture absorption and quick-drying performance level of the product can be evaluated according to the following table.
[0017]
[0018] The moisture absorption and quick-drying performance levels are divided into Level I, Level II and Level III: Level I means it has moisture absorption and quick-drying properties; Level II means it has good moisture absorption and quick-drying properties; Level III means it has excellent moisture absorption and quick-drying properties.
[0019] Fabric style performance: The finished fabric is stored in a constant temperature and humidity room for 12 hours, and a warp specimen is cut out with a size of 200mm×200mm. Each specimen and each index are measured three times to obtain the average value. The main records are friction characteristics such as the average coefficient of dynamic friction (MIU) and compression characteristics such as compression work (WC), which respectively show the smoothness and fluffiness of the fabric.
[0020] Performance Test Results 1. Water absorption test results
[0021] 2. Test results of drip diffusion time
[0022] 3. Drying rate test results
[0023] 4. Wicking height test results
[0024] In summary, it can be found that according to the test method of "GB / T 21655.1-2023 Evaluation of Moisture Absorption and Quick-drying of Textiles Part 1: Single Combination Test Method", the nylon-spandex fabrics finished in the embodiments all meet the Level III requirements, and various performance indicators are better than the nylon-spandex fabrics finished in the comparative example. It can be judged that this multifunctional finishing agent can give nylon-spandex fabrics excellent moisture absorption and quick-drying properties.
[0025] Fabric Style Performance Test Results Friction characteristics test results
[0026] The smaller the average coefficient of dynamic friction, the smoother the fabric surface feels. Obviously, the dynamic friction coefficient of the nylon-spandex fabric after finishing in the embodiment is much lower than that of the nylon-spandex fabric and the original fabric after finishing in the comparison example, indicating that the fabric surface feels smoother and better.
[0027] Compression characteristics test results
[0028] The greater the compression work ratio, the higher the compression work recovery rate, indicating that the fluffy feel of the fabric is better. Obviously, the compression work ratio of the nylon-spandex fabric after finishing in the embodiment is much higher than that of the nylon-spandex fabric after finishing in the comparison example, indicating that the fabric has a better fluffy feel.
[0029] In summary, the nylon-spandex fabrics finished in the examples all have lower average coefficient of dynamic friction and higher compression work ratio. It can be judged that this multifunctional finishing agent can give the nylon-spandex fabrics excellent smoothness and fluffy hand feel.
Claims
1. A method for preparing a multifunctional finishing agent for nylon-spandex fabrics, the preparation method comprising the following steps by weight: (1) Add 20-25 parts of isopropanol into a reaction vessel equipped with a condensing reflux device, start stirring, add 80-100 parts of single-end epoxy-terminated silicone and 10-20 parts of double-end amino polyethylene glycol into the reaction vessel respectively, raise the temperature to 60-65°C, keep the temperature for reaction for 5-6 hours, raise the temperature to 80-85°C after the reaction is completed, remove and recover the isopropanol by vacuum distillation, and obtain intermediate Y; (2) Add 30-50 parts of acetone into a reaction vessel equipped with a condensing reflux device, start stirring, and add 25-35 parts of intermediate Y, 10-20 parts of polyethylene glycol, 0.1-0.5 parts of butanone oxime and 1-5 parts of hexamethylene diisocyanate into the reaction vessel in sequence, raise the temperature to 80-85°C, add 0.1-0.2 parts of dibutyltin dilaurate, and keep the temperature to react for 2-3 hours. After the reaction is completed, add 450-650 parts of water into the reaction vessel, stir well for 30-40 minutes, remove and recover the acetone by vacuum distillation, and obtain a multifunctional finishing agent for nylon-spandex fabrics.
2. A method for preparing a multifunctional finishing agent for nylon-spandex fabric according to claim 1, characterized in that: The single-end epoxy-terminated silicone is one of single-end epoxy-terminated silicones having a number average molecular weight of 4000, 5000 and 6000; The double-terminated amino polyethylene glycol is a double-terminated amino polyethylene glycol with a number average molecular weight of about 1000, 1500 and 2000; The polyethylene glycol is one of polyethylene glycols having a number average molecular weight of 1000, 1500 and 2000.
Citation Information
Cited By
Breathable antibacterial fabric and preparation process thereof
CN119800718A
Air-permeable antibacterial fabric and preparation process thereof
CN119800718B