Two-phase refractory high-entropy alloy strengthened through Laves phase precipitation in as-cast state and preparation method of two-phase refractory high-entropy alloy
By accurately controlling the components and processes in cast high-entropy alloys, the precipitation of Laves phase is achieved, the problems of material brittleness and performance deterioration are solved, the strength and plasticity are improved, and the preparation of a refractory high-entropy alloy with Laves phase precipitation strengthening is realized.
Patent Information
- Application Number
- CN202410966508.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
In cast high-entropy alloys, the precipitation of the Laves phase is prone to increase material brittleness and deterioration in performance, and existing research is relatively limited in this regard.
By precisely controlling the alloy composition and optimizing the smelting and cooling process, the precipitation of the Laves phase is achieved. The specific steps include weighing the raw materials according to a specific atomic percentage, and performing multiple smelting under the protection of argon gas after pretreatment to ensure the formation and distribution of the Laves phase.
The strength and plasticity of the material are improved, the compression strength of the room temperature is significantly improved, and the appropriate compression strain rate is maintained, realizing the preparation of a refractory high-entropy alloy with Laves phase precipitation strengthening.
Smart Images

Figure CN118910485A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a cast Laves phase precipitation strengthened dual-phase refractory high entropy alloy and a preparation method thereof. Background Art
[0002] High entropy alloys are a new type of alloy material composed of multiple metal elements with excellent mechanical properties, corrosion resistance and high temperature stability. In recent years, high entropy alloys have become a research hotspot in the field of materials science due to their complex chemical composition and unique microstructure. However, traditional high entropy alloys face some challenges in application, especially in improving their strength and high temperature performance, which still need further exploration and optimization. Refractory metals such as tungsten (W), molybdenum (Mo), tantalum (Ta) and niobium (Nb) have extremely high melting points and excellent mechanical properties. Combining these refractory metals with high entropy alloys can develop new materials with superior performance.
[0003] Laves phase is a common intermetallic compound with higher hardness and thermal stability than the matrix material. The introduction of Laves phase into alloy materials can significantly enhance the strength and creep resistance of the materials. However, in cast high-entropy alloys, the precipitation and distribution of Laves phase need to be precisely controlled to avoid increasing the brittleness of the material and deteriorating its performance. At present, most research focuses on the composition design and basic performance evaluation of traditional high-entropy alloys. Research on Laves phase precipitation strengthening of refractory high-entropy alloys in the cast state is still relatively limited. It is urgent to develop an effective preparation method to achieve the precipitation of Laves phase and the precipitation of the second phase, thereby improving the overall performance of the material. Summary of the invention
[0004] The purpose of the present invention is to solve the problem that the precipitation of Laves phase in refractory high entropy alloys easily leads to increased brittleness and performance degradation of the material. A two-phase refractory high entropy alloy strengthened by Laves phase precipitation in a cast state and a preparation method thereof are provided. By accurately controlling the alloy composition and optimizing the smelting and cooling processes, the precipitation of the Laves phase is successfully achieved, and the plasticity adaptation is ensured while the strength is improved.
[0005] The invention discloses a cast Laves phase precipitation strengthened dual-phase refractory high entropy alloy which consists of 27.78% to 32.25% of Ti, 13.89% to 16.13% of Zr, 13.89% to 16.13% of Nb, 13.89% to 16.13% of Hf, 13.89% to 16.13% of V and 3.23% to 16.66% of Al elements in atomic percentage, and the sum of the atomic percentages of the components is 100%.
[0006] A method for preparing a dual-phase refractory high entropy alloy strengthened by Laves phase precipitation in an as-cast state is carried out according to the following steps:
[0007] 1. Weigh the raw materials according to the atomic percentage;
[0008] 2. Pre-treat the raw materials and titanium block, then add the raw materials into the crucible of the smelting furnace in the order of Nb, Hf, V, Zr, Ti, and Al from bottom to top, then add 50-70g of titanium block into another crucible of the smelting furnace, then evacuate the smelting furnace and fill it with argon for protective smelting, first melt the titanium block, then melt the raw materials, and after cooling, obtain the button ingot sample;
[0009] 3. The alloy ingot is repeatedly melted for 7-10 times, and cooled to obtain a Laves phase precipitation strengthened dual-phase refractory high entropy alloy in the cast state.
[0010] The present invention has the following gain effects:
[0011] 1. The present invention provides a novel Laves phase precipitation strengthened refractory high entropy alloy. The Ti, Zr, Nb, Hf, V, Al elements and their relative contents selected in the present invention are because these six elements can form a BCC phase and Laves phase two-phase refractory high entropy alloy. The atomic radius of Al in the present invention is 135pm, which is lower than the atomic radius of Ti, Zr, Nb, and Hf. The addition of Al element can increase the degree of lattice distortion, making the solid solution strengthening and fine grain strengthening effects of the alloy more significant, so as to improve the comprehensive mechanical properties of the alloy. In addition, the mixing enthalpy between Al element and Ti, Zr, Nb, Hf, and V elements is negative, which is easy to combine with other elements to form compounds to achieve second phase strengthening.
[0012] Second, the present invention first selects the matrix component Ti with a high Ti content 33.32 Zr 16.67 Nb 16.67 Hf 16.67 V 16.67 , the matrix has an excellent compressive strain rate, but a low compressive yield strength. Therefore, this invention changes the amount of Al element added to give full play to the best strengthening effect of Al element. When 16.66at.% Al element is added, the room temperature compressive strength of the alloy can be increased from 1008MPa to 1789.94MPa, which is 1.78 times higher than the original, and the compressive strain rate of 10.9% can be maintained.
[0013] 3. The alloy prepared by the method of the present invention is melted and solidified in a water-cooled copper crucible, which has low cost, simple process and easy implementation, does not require subsequent heat treatment and thermal deformation optimization, has a short preparation cycle, and the obtained structure after solidification is uniform and has a single solid solution structure.
[0014] The present invention strives to improve strength while ensuring plasticity adaptation, and proposes a Laves phase precipitation strengthened Ti with both strength and plasticity.a Zr b Nb c Hf d V e Al f The control method of refractory high entropy alloys. By changing the amount of Al added, it is beneficial to improve the mechanical properties, which provides new insights for the continued exploration of refractory high entropy alloy systems. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 XRD diagrams of the refractory high entropy alloys prepared in Examples 1 to 6 and Comparative Example 1;
[0016] Figure 2 This is a composition analysis diagram of the refractory high entropy alloy prepared in Example 2;
[0017] Figure 3 The SEM images of the refractory high entropy alloys prepared in Examples 1 to 6 and Comparative Example 1;
[0018] Figure 4 The Vickers hardness bar graph of the refractory high entropy alloys prepared in Examples 1 to 6 and Comparative Example 1;
[0019] Figure 5 The compressive stress-strain curves of the refractory high entropy alloys prepared in Examples 1 to 6 and Comparative Example 1 are shown. DETAILED DESCRIPTION
[0020] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.
[0021] Specific implementation method 1: In this implementation method, a cast Laves phase precipitation strengthened two-phase refractory high entropy alloy is composed of 27.78% to 32.25% Ti, 13.89% to 16.13% Zr, 13.89% to 16.13% Nb, 13.89% to 16.13% Hf, 13.89% to 16.13% V and 3.23% to 16.66% Al elements in atomic percentage, and the sum of the atomic percentages of each component is 100%.
[0022] Specific embodiment 2: This embodiment is different from the specific embodiment 1 in that the alloy is composed of 32.25% Ti, 16.13% Zr, 16.13% Nb, 16.13% Hf, 16.13% V and 3.23% Al in atomic percentage, expressed as Ti 32.25 Zr 16.13 Nb 16.13 Hf 16.13 V 16.13 Al 3.23 The rest is the same as the first specific implementation.
[0023] Specific embodiment 3: This embodiment is different from specific embodiment 1 or 2 in that the alloy is composed of 31.25% Ti, 15.625% Zr, 15.625% Nb, 15.625% Hf, 15.625% V and 6.25% Al in atomic percentage, expressed as Ti 31.25 Zr 15.625 Nb 15.625 Hf 15.625 V 15.625 Al 6.25 The rest is the same as the first or second embodiment.
[0024] Specific embodiment 4: This embodiment is different from the specific embodiments 1 to 3 in that the alloy is composed of 30.3% Ti, 15.15% Zr, 15.15% Nb, 15.15% Hf, 15.15% V and 9.1% Al in atomic percentage, expressed as Ti 30.3 Zr 15.15 Nb 15.15 Hf 15.15 V 15.15 Al 9.1 . The rest is the same as that of Specific Implementation Methods 1 to 3.
[0025] Specific embodiment 5: This embodiment is different from the specific embodiments 1 to 4 in that the alloy is composed of 29.41% Ti, 14.71% Zr, 14.71% Nb, 14.71% Hf, 14.71% V, and 11.75% Al in atomic percentage, expressed as Ti 29.41 Zr 14.71 Nb 14.71 Hf 14.71 V 14.71 Al 11.75 . The rest is the same as that of Specific Implementation Methods 1 to 4.
[0026] Specific embodiment 6: This embodiment is different from the specific embodiments 1 to 5 in that the alloy is composed of 28.57% Ti, 14.28% Zr, 14.28% Nb, 14.28% Hf, 14.28% V and 14.31% Al in atomic percentage, expressed as Ti 28.57 Zr 14.28 Nb 14.28 Hf 14.28 V 14.28 Al 14.31 . The rest is the same as the specific implementation modes 1 to 5.
[0027] Specific embodiment 7: This embodiment is different from the specific embodiments 1 to 6 in that the alloy is composed of 27.78% Ti, 13.89% Zr, 13.89% Nb, 13.89% Hf, 13.89% V and 16.66% Al in atomic percentage, expressed as Ti 27.78 Zr 13.89 Nb 13.89 Hf 13.89 V 13.89 Al 16.66 . The rest is the same as the specific implementation modes 1 to 6.
[0028] Specific embodiment 8: This embodiment is a method for preparing a dual-phase refractory high entropy alloy strengthened by Laves phase precipitation in a cast state, which is carried out according to the following steps:
[0029] 1. Weigh the raw materials according to the atomic percentage;
[0030] 2. Pre-treat the raw materials and titanium block, then add the raw materials into the crucible of the smelting furnace in the order of Nb, Hf, V, Zr, Ti, and Al from bottom to top, then add 50-70g of titanium block into another crucible of the smelting furnace, then evacuate the smelting furnace and fill it with argon for protective smelting, first melt the titanium block, then melt the raw materials, and after cooling, obtain the button ingot sample;
[0031] 3. The alloy ingot is repeatedly melted for 7-10 times, and cooled to obtain a Laves phase precipitation strengthened dual-phase refractory high entropy alloy in the cast state.
[0032] Specific embodiment 9: This embodiment is different from specific embodiment 8 or 9 in that the pretreatment in step 2 is grinding and polishing, cleaning and then drying. The rest is the same as specific embodiment 8 or 9.
[0033] Specific embodiment 10: This embodiment differs from the specific embodiments 8 to 9 in that: Step 2: vacuumize the furnace to a vacuum degree of 3×10 -3 Pa, and then high-purity argon gas is filled in as a protective gas to 0.05 MPa, and the current intensity during smelting is 300-600 A. The rest is the same as the eighth to ninth embodiments.
[0034] The following examples are used to verify the beneficial effects of the present invention:
[0035] Example 1: A Laves phase precipitation strengthened refractory high entropy alloy in the cast state, composed of 32.25% Ti, 16.13% Zr, 16.13% Nb, 16.13% Hf, 16.13% V and 3.23% Al in atomic percentage, denoted as Ti 32.25 Zr 16.13 Nb 16.13 Hf16.13 V 16.13 Al 3.23 ;
[0036] Its preparation method is as follows:
[0037] (1) Ti blocks, Zr blocks, Nb particles, Hf particles, V particles and Al particles are weighed according to the above atomic ratio to obtain raw materials; the purity of the raw materials is greater than 99.95%.
[0038] (2) Pre-treatment of the selected raw materials and metal titanium blocks by grinding and cleaning to remove oxides and impurities on the surface of the metal raw materials, and use 400-mesh SiC sandpaper to grind and remove the oxide scale; use acetone as a cleaning agent to perform an ultrasonic cleaning in an ultrasonic wave, the cleaning time is 8 minutes, the power of the ultrasonic wave is 100W, and the frequency is 25KHz; the raw materials and metal titanium blocks after acetone cleaning are then subjected to a second ultrasonic cleaning in an ultrasonic wave using anhydrous ethanol as a cleaning agent, the cleaning time is 5 minutes, the power of the ultrasonic wave is 120W, and the frequency is 35KHz, and then the surface of the sample is dried using a hair dryer;
[0039] (3) The processed raw materials are placed in the crucible of a non-consumable vacuum arc furnace in the order of Nb, Hf, V, Zr, Ti, and Al from bottom to top. At the same time, a titanium block is placed in another crucible of the non-consumable vacuum arc furnace and the furnace is evacuated to 3×10 -3 Pa, fill with protective high-purity argon gas to 0.05MPa, repeatedly evacuate, fill with argon gas, perform gas washing 3 times, and then start arc melting, first melt the metal titanium block, the melting current is 450A, the time is 3min, the residual oxygen in the arc furnace chamber is adsorbed during the melting process, and the oxidation behavior during the melting process is further reduced, and then the alloy ingot is melted, the melting current is 600A, the time is 5min, and the alloy ingot is obtained after cooling;
[0040] (4) The initially molten alloy ingot is turned over by the furnace's built-in manipulator, and then smelted again. The smelting is repeated 7 times. The alloy needs to be turned over each time to ensure the uniformity of the alloy composition. After multiple smeltings, Ti is cooled and obtained. 32.25 Zr 16.13 Nb 16.13 Hf 16.13 V 16.13 Al 3.23 Refractory high entropy alloys.
[0041] Example 2: A Laves phase precipitation strengthened refractory high entropy alloy in the cast state, composed of 31.25% Ti, 15.625% Zr, 15.625% Nb, 15.625% Hf, 15.625% V and 6.25% Al in atomic percentage, denoted as Ti 31.25 Zr 15.625Nb 15.625 Hf 15.625 V 15.625 Al 6.25 ;
[0042] Its preparation method is as follows:
[0043] (1) Ti blocks, Zr blocks, Nb particles, Hf particles, V particles and Al particles are weighed according to the above atomic ratio to obtain raw materials; the purity of the raw materials is greater than 99.95%.
[0044] (2) Pre-treatment of the selected raw materials and metal titanium blocks by grinding and cleaning to remove oxides and impurities on the surface of the metal raw materials, and use 400-mesh SiC sandpaper to grind and remove the oxide scale; use acetone as a cleaning agent to perform an ultrasonic cleaning in an ultrasonic wave, the cleaning time is 8 minutes, the power of the ultrasonic wave is 100W, and the frequency is 25KHz; the raw materials and metal titanium blocks after acetone cleaning are then subjected to a second ultrasonic cleaning in an ultrasonic wave using anhydrous ethanol as a cleaning agent, the cleaning time is 5 minutes, the power of the ultrasonic wave is 120W, and the frequency is 35KHz, and then the surface of the sample is dried using a hair dryer;
[0045] (3) The processed raw materials are placed in the crucible of a non-consumable vacuum arc furnace in the order of Nb, Hf, V, Zr, Ti, and Al from bottom to top. At the same time, a titanium block is placed in another crucible of the non-consumable vacuum arc furnace and the furnace is evacuated to 3×10 - 3 Pa, fill with protective high-purity argon gas to 0.05MPa, repeatedly evacuate, fill with argon gas, perform gas washing 3 times, and then start arc melting, first melt the metal titanium block, the melting current is 450A, the time is 3min, the residual oxygen in the arc furnace chamber is adsorbed during the melting process, and the oxidation behavior during the melting process is further reduced, and then the alloy ingot is melted, the melting current is 600A, the time is 5min, and the alloy ingot is obtained after cooling;
[0046] (4) The initially molten alloy ingot is turned over by the furnace's built-in manipulator, and then smelted again. The smelting is repeated 7 times. The alloy needs to be turned over each time to ensure the uniformity of the alloy composition. After multiple smeltings, Ti is cooled and obtained. 31.25 Zr 15.625 Nb 15.625 Hf 15.625 V 15.625 Al 6.25 Refractory high entropy alloys.
[0047] Example 3: A Laves phase precipitation strengthened refractory high entropy alloy in the cast state, composed of 30.3% Ti, 15.15% Zr, 15.15% Nb, 15.15% Hf, 15.15% V and 9.1% Al in atomic percentage, denoted as Ti30.3 Zr 15.15 Nb 15.15 Hf 15.15 V 15.15 Al 9.1 ;
[0048] Its preparation method is as follows:
[0049] (1) Ti blocks, Zr blocks, Nb particles, Hf particles, V particles and Al particles are weighed according to the above atomic ratio to obtain raw materials; the purity of the raw materials is greater than 99.95%.
[0050] (2) Pre-treatment of the selected raw materials and metal titanium blocks by grinding and cleaning to remove oxides and impurities on the surface of the metal raw materials, and use 400-mesh SiC sandpaper to grind and remove the oxide scale; use acetone as a cleaning agent to perform an ultrasonic cleaning in an ultrasonic wave, the cleaning time is 8 minutes, the power of the ultrasonic wave is 100W, and the frequency is 25KHz; the raw materials and metal titanium blocks after acetone cleaning are then subjected to a second ultrasonic cleaning in an ultrasonic wave using anhydrous ethanol as a cleaning agent, the cleaning time is 5 minutes, the power of the ultrasonic wave is 120W, and the frequency is 35KHz, and then the surface of the sample is dried using a hair dryer;
[0051] (3) The processed raw materials are placed in the crucible of a non-consumable vacuum arc furnace in the order of Nb, Hf, V, Zr, Ti, and Al from bottom to top. At the same time, a titanium block is placed in another crucible of the non-consumable vacuum arc furnace and the furnace is evacuated to 3×10 - 3 Pa, fill with protective high-purity argon gas to 0.05MPa, repeatedly evacuate, fill with argon gas, perform gas washing 3 times, and then start arc melting, first melt the metal titanium block, the melting current is 450A, the time is 3min, the residual oxygen in the arc furnace chamber is adsorbed during the melting process, and the oxidation behavior during the melting process is further reduced, and then the alloy ingot is melted, the melting current is 600A, the time is 5min, and the alloy ingot is obtained after cooling;
[0052] (4) The initially molten alloy ingot is turned over by the furnace's built-in manipulator, and then smelted again. The smelting is repeated 7 times to ensure the uniformity of the alloy composition. After multiple smeltings, Ti is cooled and obtained. 30.3 Zr 15.15 Nb 15.15 Hf 15.15 V 15.15 Al 9.1 Refractory high entropy alloys.
[0053] Example 4: A Laves phase precipitation strengthened refractory high entropy alloy in the cast state, composed of 29.41% Ti, 14.71% Zr, 14.71% Nb, 14.71% Hf, 14.71% V and 11.75% Al in atomic percentage, denoted as Ti 29.41 Zr 14.71 Nb 14.71 Hf 14.71 V 14.71 Al 11.75 ;
[0054] Its preparation method is as follows:
[0055] (1) Ti blocks, Zr blocks, Nb particles, Hf particles, V particles and Al particles are weighed according to the above atomic ratio to obtain raw materials; the purity of the raw materials is greater than 99.95%.
[0056] (2) Pre-treatment of the selected raw materials and metal titanium blocks by grinding and cleaning to remove oxides and impurities on the surface of the metal raw materials, and use 400-mesh SiC sandpaper to grind and remove the oxide scale; use acetone as a cleaning agent to perform an ultrasonic cleaning in an ultrasonic wave, the cleaning time is 8 minutes, the power of the ultrasonic wave is 100W, and the frequency is 25KHz; the raw materials and metal titanium blocks after acetone cleaning are then subjected to a second ultrasonic cleaning in an ultrasonic wave using anhydrous ethanol as a cleaning agent, the cleaning time is 5 minutes, the power of the ultrasonic wave is 120W, and the frequency is 35KHz, and then the surface of the sample is dried using a hair dryer;
[0057] (3) The processed raw materials are placed in the crucible of a non-consumable vacuum arc furnace in the order of Nb, Hf, V, Zr, Ti, and Al from bottom to top. At the same time, a titanium block is placed in another crucible of the non-consumable vacuum arc furnace and the furnace is evacuated to 3×10 - 3 Pa, fill with protective high-purity argon gas to 0.05MPa, repeatedly evacuate, fill with argon gas, perform gas washing 3 times, and then start arc melting, first melt the metal titanium block, the melting current is 450A, the time is 3min, the residual oxygen in the arc furnace chamber is adsorbed during the melting process, and the oxidation behavior during the melting process is further reduced, and then the alloy ingot is melted, the melting current is 600A, the time is 5min, and the alloy ingot is obtained after cooling;
[0058] (4) The initially molten alloy ingot is turned over by the furnace's built-in manipulator, and then smelted again. The smelting is repeated 7 times to ensure the uniformity of the alloy composition. After multiple smeltings, Ti is cooled and obtained. 29.41 Zr 14.71 Nb 14.71 Hf 14.71 V 14.71 Al 11.75 Refractory high entropy alloys.
[0059] Example 5: A Laves phase precipitation strengthened refractory high entropy alloy in the cast state, composed of 28.57% Ti, 14.28% Zr, 14.28% Nb, 14.28% Hf, 14.28% V and 14.31% Al in atomic percentage, denoted as Ti 28.57 Zr 14.28 Nb 14.28 Hf 14.28 V 14.28 Al 14.31 ;
[0060] Its preparation method is as follows:
[0061] (1) Ti blocks, Zr blocks, Nb particles, Hf particles, V particles and Al particles are weighed according to the above atomic ratio to obtain raw materials; the purity of the raw materials is greater than 99.95%.
[0062] (2) Pre-treatment of the selected raw materials and metal titanium blocks by grinding and cleaning to remove oxides and impurities on the surface of the metal raw materials, and use 400-mesh SiC sandpaper to grind and remove the oxide scale; use acetone as a cleaning agent to perform an ultrasonic cleaning in an ultrasonic wave, the cleaning time is 8 minutes, the power of the ultrasonic wave is 100W, and the frequency is 25KHz; the raw materials and metal titanium blocks after acetone cleaning are then subjected to a second ultrasonic cleaning in an ultrasonic wave using anhydrous ethanol as a cleaning agent, the cleaning time is 5 minutes, the power of the ultrasonic wave is 120W, and the frequency is 35KHz, and then the surface of the sample is dried using a hair dryer;
[0063] (3) The processed raw materials are placed in the crucible of a non-consumable vacuum arc furnace in the order of Nb, Hf, V, Zr, Ti, and Al from bottom to top. At the same time, a titanium block is placed in another crucible of the non-consumable vacuum arc furnace and the furnace is evacuated to 3×10 - 3 Pa, fill with protective high-purity argon gas to 0.05MPa, repeatedly evacuate, fill with argon gas, perform gas washing 3 times, and then start arc melting, first melt the metal titanium block, the melting current is 450A, the time is 3min, the residual oxygen in the arc furnace chamber is adsorbed during the melting process, and the oxidation behavior during the melting process is further reduced, and then the alloy ingot is melted, the melting current is 600A, the time is 5min, and the alloy ingot is obtained after cooling;
[0064] (4) The initially molten alloy ingot is turned over by the furnace's built-in manipulator, and then smelted again. The smelting is repeated 7 times to ensure the uniformity of the alloy composition. After multiple smeltings, Ti is cooled and obtained. 28.57 Zr 14.28 Nb 14.28 Hf 14.28 V 14.28 Al 14.31 Refractory high entropy alloys.
[0065] Example 6: A Laves phase precipitation strengthened refractory high entropy alloy in the cast state, composed of 27.78% Ti, 13.89% Zr, 13.89% Nb, 13.89% Hf, 13.89% V and 16.66% Al in atomic percentage, denoted as Ti 27.78 Zr 13.89 Nb 13.89 Hf 13.89 V 13.89 Al 16.66 ;
[0066] Its preparation method is as follows:
[0067] (1) Ti blocks, Zr blocks, Nb particles, Hf particles, V particles and Al particles are weighed according to the above atomic ratio to obtain raw materials; the purity of the raw materials is greater than 99.95%.
[0068] (2) Pre-treatment of the selected raw materials and metal titanium blocks by grinding and cleaning to remove oxides and impurities on the surface of the metal raw materials, and use 400-mesh SiC sandpaper to grind and remove the oxide scale; use acetone as a cleaning agent to perform an ultrasonic cleaning in an ultrasonic wave, the cleaning time is 8 minutes, the power of the ultrasonic wave is 100W, and the frequency is 25KHz; the raw materials and metal titanium blocks after acetone cleaning are then subjected to a second ultrasonic cleaning in an ultrasonic wave using anhydrous ethanol as a cleaning agent, the cleaning time is 5 minutes, the power of the ultrasonic wave is 120W, and the frequency is 35KHz, and then the surface of the sample is dried using a hair dryer;
[0069] (3) The processed raw materials are placed in the crucible of a non-consumable vacuum arc furnace in the order of Nb, Hf, V, Zr, Ti, and Al from bottom to top. At the same time, a titanium block is placed in another crucible of the non-consumable vacuum arc furnace and the furnace is evacuated to 3×10 - 3 Pa, fill with protective high-purity argon gas to 0.05MPa, repeatedly evacuate, fill with argon gas, perform gas washing 3 times, and then start arc melting, first melt the metal titanium block, the melting current is 450A, the time is 3min, the residual oxygen in the arc furnace chamber is adsorbed during the melting process, and the oxidation behavior during the melting process is further reduced, and then the alloy ingot is melted, the melting current is 600A, the time is 5min, and the alloy ingot is obtained after cooling;
[0070] (4) The initially molten alloy ingot is turned over by the furnace's built-in manipulator, and then smelted again. The smelting is repeated 7 times to ensure the uniformity of the alloy composition. After multiple smeltings, Ti is cooled and obtained. 27.78 Zr 13.89 Nb 13.89 Hf 13.89 V 13.89 Al 16.66Refractory high entropy alloys.
[0071] Comparative Example 1: This example is a refractory high entropy alloy, which is composed of 33.32% Ti, 16.67% Zr, 16.67% Nb, 16.67% Hf and 16.67% V in atomic percentage, represented by Ti 33.32 Zr 16.67 Nb 16.67 Hf 16.67 V 16.67 ;
[0072] Its preparation method is as follows:
[0073] (1) Weigh Ti blocks, Zr blocks, Nb particles, Hf particles and V particles according to the above atomic ratio to obtain raw materials; the purity of the raw materials is greater than 99.95%.
[0074] (2) Pre-treatment of the selected raw materials and metal titanium blocks by grinding and cleaning to remove oxides and impurities on the surface of the metal raw materials, and use 400-mesh SiC sandpaper to grind and remove the oxide scale; use acetone as a cleaning agent to perform an ultrasonic cleaning in an ultrasonic wave, the cleaning time is 8 minutes, the power of the ultrasonic wave is 100W, and the frequency is 25KHz; the raw materials and metal titanium blocks after acetone cleaning are then subjected to a second ultrasonic cleaning in an ultrasonic wave using anhydrous ethanol as a cleaning agent, the cleaning time is 5 minutes, the power of the ultrasonic wave is 120W, and the frequency is 35KHz, and then the surface of the sample is dried using a hair dryer;
[0075] (3) The processed raw materials are placed in the crucible of a non-consumable vacuum arc furnace in the order of Nb, Hf, V, Zr, and Ti from bottom to top. At the same time, a titanium block is placed in another crucible of the non-consumable vacuum arc furnace and the furnace is evacuated to 3×10 -3 Pa, fill with protective high-purity argon gas to 0.05MPa, repeatedly evacuate, fill with argon gas, perform gas washing 3 times, and then start arc melting, first melt the metal titanium block, the melting current is 450A, the time is 3min, the residual oxygen in the arc furnace chamber is adsorbed during the melting process, and the oxidation behavior during the melting process is further reduced, and then the alloy ingot is melted, the melting current is 600A, the time is 5min, and the alloy ingot is obtained after cooling;
[0076] (4) The initially molten alloy ingot is turned over by the furnace's built-in manipulator, and then smelted again. The smelting is repeated 7 times to ensure the uniformity of the alloy composition. After multiple smeltings, Ti is cooled and obtained. 33.32 Zr 16.67 Nb 16.67 Hf 16.67 V 16.67 Refractory high entropy alloys.
[0077] The XRD patterns of the refractory high entropy alloys of Examples 1 to 6 and Comparative Example 1 are as follows: Figure 1 As shown, the phase structure of the high entropy alloy is detected by X-ray diffractometer, the X-ray source is CuKα (λ=0.1542nm) ray, the scanning angle 2θ range is 20°-100°, and the scanning speed is 4° / min. Figure 1 It can be seen that the comparative example 1 contains only the BCC phase, and with the addition of the Al element, the Laves phase appears in Examples 1 to 6. With the gradual introduction of the Al element, the XRD diffraction peak moves to the right, and the Al atoms cause more serious lattice distortion to the matrix alloy. Figure 2 This is the composition analysis diagram of the refractory high entropy alloy prepared in Example 2. Figure 2 It can be seen from the component analysis results of Example 2 that a second phase, Laves phase, appears, which is consistent with the test results of XRD, and the Laves phase is enriched with V element.
[0078] The scanning electron microscope organization diagrams of the refractory high entropy alloys prepared in Examples 1 to 6 and Comparative Example 1 are as follows: Figure 2 As shown in the figure, it can be seen that its microstructure is a typical dendrite and interdendritic structure.
[0079] The Vickers hardness results of the refractory high entropy alloys prepared in Examples 1 to 6 and Comparative Example 1 are as follows: Figure 3 As shown in the figure, it can be seen that with the addition of Al element, the total Vickers hardness continues to increase, from 317.29 HV in comparative example 1 to 533.73 HV in example 6, which is 1.68 times the original. The increase in Vickers hardness of examples 1 to 6 is mainly due to solid solution strengthening, second phase strengthening and grain refinement strengthening.
[0080] Table 1 Compressive yield strength and compressive strain of different Al contents
[0081]
[0082] The compressive stress-strain curves of the refractory high entropy alloys prepared in Examples 1 to 6 and Comparative Example 1 are as follows: Figure 4As shown. The room temperature compressive stress-strain curve of the alloy and Table 1 show that with the addition of Al element, the room temperature compressive strength of the alloy increases from 1008MPa to 1789.94MPa, which is 1.78 times the original. Among them, the compressive strains of Example 1, Example 2, Example 3 and Comparative Example 1 are all above 50%, and the compressive strains of Example 4, Example 5 and Example 6 are continuously decreasing. This is because with the addition of Al element, the hard strengthening phase Laves phase continues to increase, so that the yield strength of the alloy is improved, while the compressive strain is reduced. When 16.66at.% of Al element is added, the room temperature compressive strength of the alloy can be increased to 1789.94MPa, and the compression strain rate of 10.9% can be maintained.
Claims
1. A dual-phase refractory high entropy alloy strengthened by Laves phase precipitation in the as-cast state, Features The alloy consists of 27.78% to 32.25% Ti, 13.89% to 16.13% Zr, 13.89% to 16.13% Nb, 13.89% to 16.13% Hf, 13.89% to 16.13% V and 3.23% to 16.66% Al elements in atomic percentage, and the sum of the atomic percentages of the components is 100%.
2. A dual-phase refractory high entropy alloy strengthened by Laves phase precipitation in the as-cast state according to claim 1, It is characterized in that The alloy consists of 32.25% Ti, 16.13% Zr, 16.13% Nb, 16.13% Hf, 16.13% V and 3.23% Al in atomic percentage, and is represented by Ti 32.25 Zr 16.13 Nb 16.13 Hf 16.13 V 16.13 Al 3.23 .
3. A dual-phase refractory high entropy alloy strengthened by Laves phase precipitation in the as-cast state according to claim 1, It is characterized in that The alloy consists of 31.25% Ti, 15.625% Zr, 15.625% Nb, 15.625% Hf, 15.625% V and 6.25% Al in atomic percentage, and is represented by Ti 31.25 Zr 15.625 Nb 15.625 Hf 15.625 V 15.625 Al 6.25 .
4. The as-cast Laves phase precipitation-strengthened dual-phase refractory high entropy alloy according to claim 1, It is characterized in that The alloy consists of 30.3% Ti, 15.15% Zr, 15.15% Nb, 15.15% Hf, 15.15% V and 9.1% Al in atomic percentage, and is represented by Ti 30.3 Zr 15.15 Nb 15.15 Hf 15.15 V 15.15 Al 9.1 .
5. The cast Laves phase precipitation strengthened dual-phase refractory high entropy alloy according to claim 1, It is characterized in that The alloy is composed of 29.41% Ti, 14.71% Zr, 14.71% Nb, 14.71% Hf, 14.71% V, and 11.75% Al in atomic percentage, and is represented by Ti 29.41 Zr 14.71 Nb 14.71 Hf 14.71 V 14.71 Al 11.75 .
6. The as-cast Laves phase precipitation-strengthened dual-phase refractory high entropy alloy according to claim 1, It is characterized in that The alloy consists of 28.57% Ti, 14.28% Zr, 14.28% Nb, 14.28% Hf, 14.28% V and 14.31% Al in atomic percentage, and is represented by Ti 28.57 Zr 14.28 Nb 14.28 Hf 14.28 V 14.28 Al 14.31 .
7. The as-cast Laves phase precipitation-strengthened dual-phase refractory high entropy alloy according to claim 1, It is characterized in that The alloy consists of 27.78% Ti, 13.89% Zr, 13.89% Nb, 13.89% Hf, 13.89% V and 16.66% Al in atomic percentage, and is represented by Ti 27.78 Zr 13.89 Nb 13.89 Hf 13.89 V 13.89 Al 16.66 .
8. A method for preparing a cast Laves phase precipitation strengthened dual-phase refractory high entropy alloy as claimed in claim 1, It is characterized in that The preparation method is carried out according to the following steps:
1. Weigh the raw materials according to the atomic percentage; 2. Pre-treat the raw materials and titanium block, then add the raw materials into the crucible of the smelting furnace in the order of Nb, Hf, V, Zr, Ti, and Al from bottom to top, then add 50-70g of titanium block into another crucible of the smelting furnace, then evacuate the smelting furnace and fill it with argon for protective smelting, first melt the titanium block, then melt the raw materials, and after cooling, obtain the button ingot sample; 3. The alloy ingot is repeatedly melted for 7-10 times, and cooled to obtain a Laves phase precipitation strengthened dual-phase refractory high entropy alloy in the cast state.
9. The method for preparing a cast Laves phase precipitation strengthened dual-phase refractory high entropy alloy according to claim 8, It is characterized in that The pretreatment in step 2 is grinding and polishing, cleaning and then drying.
10. The method for preparing a cast Laves phase precipitation strengthened dual-phase refractory high entropy alloy according to claim 8, It is characterized in that Step 2: Vacuum the furnace to a vacuum degree of 3×10 -3 Pa, and then high-purity argon gas is filled in as protective gas to 0.05MPa. The current intensity during smelting is 300-600A.
Citation Information
Patent Citations
AlxCrFeNiCuVTi high-entropy alloy material and preparation method thereof
CN103194656A
Method for enhancing wear resistance of refractory high-entropy alloy
CN113151725A
Multi-element refractory high-entropy alloy and preparation method thereof
CN113373366A
High-entropy alloy with excellent mechanical property and oxidation resistance at high temperature and preparation method
CN114752792A
Method for regulating and controlling obdurability and failure mode of TiZrHfNbTa system refractory high-entropy alloy
CN115572881A
Cited By
Nb-Si-based high-entropy alloy and preparation method and application thereof
CN121161120A