Microfiller-inlaid flexible silicon dioxide nanofiber membrane and preparation method thereof

The preparation of flexible silica nanofiber membranes embedded with microfillers through electrospinning technology, solving the problems of insufficient thermal conduction, convection and radiation performance and poor flexibility and mechanical properties of silica fiber membranes under high temperature conditions in the prior art. , achieves low porosity, low thermal conductivity and high temperature stability, and is suitable for thermal insulation materials with complex usage conditions.

CN118910813AActive Publication Date: 2024-11-08ZHEJIANG SCI-TECH UNIV

Patent Information

Application Number
CN202411226415.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-08
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

The existing silica fiber membranes have insufficient resistance to thermal conduction, thermal convection and thermal radiation under high temperature conditions, and the flexibility and mechanical properties of the composite film materials are poor, which are prone to fall off, affecting the thermal insulation effect and safety.

Method used

Using electrostatic spinning technology to prepare flexible silica nanofiber films embedded in microfilters, and by uniformly dispersing inorganic microfilters and polymers in the spinning liquid, forming a composite of polymer/filter composite fibers and silica precursor hybrid fibers. Structure: After high-temperature calcination, the inorganic filler is embedded in the fiber pores to ensure the low porosity and low thermal conductivity of the fiber membrane.

Benefits of technology

It realizes the low heat convection and low heat transfer properties of the fiber membrane, maintains excellent flexibility and strength, avoids the fall of fillers, meets the requirements of high-temperature heat insulation and mechanical properties, and is suitable for complex use conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910813A_ABST
    Figure CN118910813A_ABST
Patent Text Reader

Abstract

The preparation method comprises the following steps: firstly, preparing a filler / organic polymer mixed solution and a silicon dioxide precursor solution, and carrying out multi-channel combined spinning by utilizing an electrostatic spinning technology; organic components in the polymer / filler composite fibers and the silicon dioxide precursor hybrid fibers are removed through high-temperature calcination, and the flexible fiber / filler composite membrane with the inorganic micron filler embedded between pores of the silicon dioxide nanofibers is obtained. The micron-sized filler in the composite fiber membrane covers pores among fibers in situ and can slightly slide in a local space, so that the composite membrane keeps the characteristics of flexibility and light weight of a silicon dioxide fiber membrane while greatly reducing air convection. The composite film has excellent heat insulation effect, flame resistance and high-temperature stability in high-speed air convection scenes such as high temperature, combustion, explosion and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of synthesis and preparation of inorganic composite ceramic fiber materials, and relates to a flexible silicon dioxide nanofiber membrane inlaid with micron fillers and a preparation method thereof. Technical Background

[0002] Silica has extremely low thermal conductivity and thermal expansion coefficient, while silica fiber membrane is a soft / flexible thermal insulation material with good thermal insulation performance and excellent high-temperature stability. It is widely used in battery insulation layer, aerospace body protection, building wall protection, solar collectors, industrial pipeline insulation and fireproof clothing. There are three ways of heat transfer: heat conduction, heat convection and heat radiation. Among them, heat conduction is the transfer from the higher temperature part of an object along the object to the lower temperature part, and silica material has an extremely low thermal conductivity to prevent the conduction of temperature between objects, greatly reducing heat transfer. However, under the complex conditions and extreme conditions of the use scenario, simple low thermal conductivity cannot meet the needs of industry and industry, and higher requirements are also placed on the performance of silica fiber membrane materials in resisting thermal convection and thermal radiation.

[0003] There are many pores in the fiber membrane, and the gas can transfer heat by convection through the pores, that is, there is still a problem of heat convection in the silica fiber membrane, which affects its thermal insulation effect. Chinese patent CN202211607713.5 discloses a method for preparing a high-strength and low-thermal conductivity ceramic aerogel material, and Chinese patent CN202210610438.6 discloses a method for preparing a fiber composite gel flexible membrane. These patents prepare silica fiber membranes by electrospinning technology, and then composite aerogel precursor liquid or coat silica sol on the fiber surface to make the fiber membrane have excellent heat resistance, but the use of impregnation or coating methods can easily make the composite fiber membrane brittle after aging, or only maintain a certain flexibility under very thin conditions; surface coating can easily cause stratification during use, fiber layer and aerogel layer breaking at different times, and other problems; the composite membrane material prepared by directly composite fiber membranes with aerogel particles has the problem of falling off and powdering during use, and the thermal insulation effect is poorly stable and has certain harm to the environment. After the nanofibers are impregnated with loads, the connection between the fibers becomes tight and fixed, which significantly deteriorates the softness of the material, seriously affecting its mechanical properties and its application range. More importantly, under high temperature conditions, the thermal radiation barrier effect of aerogel particles declines rapidly, and it is necessary to study new composite thermal insulation materials that are resistant to thermal conduction, thermal convection, and thermal radiation at the same time under high temperature conditions. Summary of the invention

[0004] The present invention provides a flexible silica nanofiber membrane inlaid with micron fillers and a preparation method thereof. The silica nanofiber membrane with a composite structure has the characteristics of low porosity, low thermal conductivity and thermal expansion coefficient, strong high temperature resistance, excellent flexibility, good mechanical properties, and outstanding material stability.

[0005] The present invention provides a method for preparing a flexible silica nanofiber membrane inlaid with micron fillers, and the specific steps are as follows:

[0006] The first step is to disperse the inorganic micron filler into the organic polymer solution to prepare a polymer / micron filler mixed solution as the spinning solution 1.

[0007] Step 2: subjecting the mixture of silicon source, solvent and catalyst to hydrolysis and condensation reaction under stirring to obtain silicon source hydrolyzate, and then adding the polymer solution, mixing and stirring evenly to prepare silicon dioxide precursor solution as spinning solution 2.

[0008] Step 3: Spinning solution 1 and spinning solution 2 are respectively poured into different syringes, and the two are electrospun according to the proportion and combination to prepare a composite fiber membrane hybrid fiber membrane in which polymer / filler composite fibers and polymer / silica precursor hybrid fibers are interlaced with each other. The organic components in the two fibers are removed by high-temperature calcination to obtain a flexible silica nanofiber membrane inlaid with micron fillers.

[0009] As the preferred technical solution:

[0010] In the first step, dispersion can be performed by ultrasound, stirring, etc., so that the filler is evenly dispersed in the organic polymer solution.

[0011] The inorganic micron filler is one or more of hollow silicon dioxide spheres, hollow glass microspheres, montmorillonite sheets, boron nitride nanosheets, graphene oxide nanosheets, and graphene nanosheets, and the filler size is 5um-100nm.

[0012] In the first step, the polymer / micron filler mixed solution has the characteristic of excellent compatibility, and excellent compatibility means that the filler does not undergo visible sedimentation when the polymer solution is left to stand for a long time.

[0013] The polymer in the first step and the polymer in the second step can be the same or different. The polymer is one or more of polyvinyl alcohol, polyvinyl butyral, and polyvinyl pyrrolidone.

[0014] In the second step, the silicon source is one or more of tetramethyl silicate, tetraethyl silicate, tetrapropyl silicate, tetrabutyl silicate, tetraphenyl silicate, silicon tetrachloride, and silicate; the solvent is one or more of deionized water, anhydrous ethanol, and N,N-dimethylformamide; and the catalyst is one or more of oxalic acid, phosphoric acid, hydrochloric acid, acetic acid, sulfuric acid, and nitric acid.

[0015] In the third step, the spinning solution 1 and the spinning solution 2 are extruded and spun simultaneously and received by the same receiving device, and the number of injectors and injection rates of the respective injectors are independent of each other.

[0016] In the third step, the ratio and combination of the spinning solution 1 and the spinning solution 2 are such that the mass ratio of the silica nanofibers to the micron filler in the final fiber membrane is 1:0.25-5. Electrospinning refers to the injection of a flow rate of 0.1-50 mL / h into the spinneret of the electrospinning equipment under the conditions of 15-35°C and a relative humidity of 20-70%, and the spinneret is connected to a high-voltage power supply of 10-100 kV for electrospinning. The distance between the receiving device and the spinneret is 3-70 cm.

[0017] In the third step, the polymer / filler composite fiber refers to the filler being wholly or partially bound inside the fiber, and the other part of the filler can be exposed outside the fiber; the polymer / silica precursor hybrid fiber refers to the silica and polymer components being uniformly distributed in the fiber; and the interpenetration refers to the polymer / filler composite fiber and the polymer / silica precursor hybrid fiber being randomly stacked and crossed in three-dimensional space.

[0018] In the third step, the high temperature calcination is carried out by heating the temperature to 200-800° C. at a heating rate of 0.1-10° C. / min and maintaining the highest temperature for 10-360 min.

[0019] In the third step, embedding means that the calcined inorganic filler is trapped in the pores between the silica fibers and cannot fall off, there is no hard sintering between the inorganic filler and the silica, and the inorganic filler can produce a small rotation and slip in the pores between the fibers.

[0020] The present invention uses electrospinning technology to prepare a flexible silica nanofiber membrane inlaid with micron fillers at one time. The inorganic fillers uniformly distributed in the obtained nanofiber membrane not only have high temperature resistance, but also the fillers and fibers are randomly stacked and crossed in three-dimensional space, so that the fiber membrane has low thermal convection and low heat transfer performance, while ensuring the excellent flexibility and strength of the fiber membrane. Compared with the existing aerogel attached to the surface of the fiber membrane or infiltrated into the pores of the fiber membrane, the composite nanofiber membrane of the present invention has a larger pore coverage, and the fiber cross-stacked structure has a stronger binding force on the filler, and the filler is not easy to fall off. At the same time, the inorganic filler can produce a small rotation and slip in the pores between the fibers, ensuring the softness and other excellent mechanical properties of the nanofiber membrane, which can be used as an ideal material for thermal insulation membranes.

[0021] The flexible silica nanofiber membrane inlaid with micron fillers and the preparation method thereof described in the present invention utilizes electrostatic spinning technology to prepare a composite structure in which fillers and fibers are randomly stacked and crossed in three-dimensional space, thereby overcoming the adverse effects of pore heat convection in the fiber membrane on the thermal insulation performance, as well as the disadvantages of the traditional thermal insulation hybrid membrane being hard in texture and the covering being easy to fall off. The preparation method of the present invention is simple, and the obtained nanofiber membrane has the advantages of low porosity, low thermal conductivity, high temperature resistance, combustion resistance, thermal dimensional stability, excellent mechanical properties, good softness, and material components not being easy to fall off. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the SEM image of the flexible silica nanofiber membrane inlaid with micron fillers in Example 1. DETAILED DESCRIPTION

[0023] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0024] Example 1

[0025] Step 1: Ultrasonically disperse 1 g of boron nitride nanosheets uniformly, then add them into a mixed solution of 5 g of 20 wt% polyvinyl pyrrolidone in N,N-dimethylformamide solution and 4 g of anhydrous ethanol, and stir them magnetically for 10 h to prepare a polyvinyl pyrrolidone / boron nitride nanosheet mixed solution with excellent compatibility as spinning solution 1.

[0026] Step 2: A mixture of 30 g tetraethyl silicate, 27 g N,N-dimethylformamide, 4.5 g deionized water and 0.3 g phosphoric acid was magnetically stirred for 10 h for hydrolysis and condensation reaction to obtain a silicon source hydrolyzate, and then 22 g of 20 wt% polyvinyl pyrrolidone solution was added and stirred for 10 h to mix evenly to prepare a silica precursor solution as spinning solution 2.

[0027] Step 3: Pour spinning solution 1 and spinning solution 2 into different syringes respectively, adjust the ratio and combination of the two for electrospinning, so that the mass ratio of silica nanofibers and boron nitride nanosheet fillers in the final fiber membrane is 1:1, and the two spinning solutions are extruded simultaneously and received by the same receiving device; the spinning temperature is 23°C, the relative humidity is 49%, the injection speed is 0.8mL / h, the spinning voltage is 22kV, and the receiving distance is 15cm. A hybrid fiber membrane in which polyvinyl pyrrolidone / boron nitride nanosheet composite fibers and polyvinyl alcohol / silica precursor hybrid fibers are interlaced with each other is prepared. By heating from room temperature to 600°C at a rate of 5°C / min and maintaining the highest temperature for 300 minutes, the organic components in the two fibers are removed to obtain a flexible fiber / filler composite membrane in which inorganic micron fillers are embedded between the pores of silica nanofibers. Its morphology is as follows Figure 1 As shown, from Figure 1 It can be seen that the boron nitride nanosheets are bound inside the silica fibers, and are randomly stacked and crossed with the silica fibers in three-dimensional space, while covering and blocking the pores where the fibers intersect, and the boron nitride nanosheets can produce a small rotation and slip in the pores between the fibers. The flexible silica nanofiber membrane inlaid with micronized boron nitride nanosheets does not burn under the outer flame of an alcohol lamp; calcination at 1000°C for 2h results in only 0.5% heat loss, and it is still flexible and can be folded 180°; the air permeability of the flexible silica nanofiber / boron nitride nanosheet composite membrane is 210 (KPa·s / m) / mm; the thermal insulation performance on a 600°C hot stage is: after standing for 5 minutes, the cold surface of the flexible silica nanofiber / boron nitride nanosheet composite membrane only heats up to 100°C, and the heating rate does not exceed 1°C / s, which meets the requirements for thermal insulation in the national standard GB38031-2020 "Safety Requirements for Electric Vehicle Batteries". Example 2

[0028] Step 1: 1 g of hollow silica microspheres was evenly dispersed by ultrasonication for 30 min, then added into 7.3 g of 12.5 wt% polyvinyl alcohol aqueous solution, and magnetically stirred for 10 h to prepare a polyvinyl alcohol / hollow silica microsphere mixed solution with excellent compatibility as spinning solution 1.

[0029] Step 2: A mixture of 33 g tetraethyl silicate, 27.3 g water and 0.3 g phosphoric acid was magnetically stirred for 10 h for hydrolysis and condensation reaction to obtain a silicon source hydrolyzate, and then 24.1 g of a 12.5 wt% polyvinyl alcohol solution was added and stirred for 10 h to mix evenly to prepare a silica precursor solution as the spinning solution 2.

[0030] Step 3: Spinning solution 1 and spinning solution 2 are poured into different syringes respectively, and the ratio and combination of the two are adjusted for electrostatic spinning, so that the mass ratio of silica nanofibers to hollow silica microsphere fillers in the final fiber membrane is 1:1, and the two spinning solutions are extruded simultaneously and received by the same receiving device; the spinning temperature is 24°C, the relative humidity is 45%, the injection speed is 0.7mL / h, the spinning voltage is 20kV, and the receiving distance is 20cm. Prepare a hybrid fiber membrane in which polyvinyl alcohol / hollow silica microsphere composite fibers and polyvinyl alcohol / silica precursor hybrid fibers are interlaced with each other. By heating from room temperature to 700°C at a heating rate of 3°C / min and maintaining the highest temperature for 240min, the organic components in the two fibers are removed to obtain a flexible fiber / filler composite membrane in which an inorganic micron filler is embedded between the pores of silica nanofibers. The product obtained in this embodiment has a composite structure similar to that of Example 1 in which fillers and fibers are randomly stacked and crossed in three-dimensional space. The flexible silica nanofiber membrane inlaid with hollow silica microspheres does not burn under the outer flame of an alcohol lamp; after calcination at 1000°C for 2 hours, it only loses 0.4% of heat and is still flexible and foldable 180°; the air permeability of the flexible silica nanofiber / hollow silica microsphere composite membrane is 188 (KPa·s / m) / mm; the thermal insulation performance on a 600°C hot stage is: after standing for 5 minutes, the cold surface of the flexible silica nanofiber / hollow silica microsphere composite membrane only heats up to 113°C, and the heating rate does not exceed 1°C / s, which meets the requirements for thermal insulation in the national standard GB38031-2020 "Safety Requirements for Electric Vehicle Batteries".

[0031] Example 3

[0032] Step 1: 1 g of graphene oxide nanosheets was uniformly dispersed by ultrasonic treatment for 6 h, then added into 7.3 g of 12.5 wt% polyvinyl butyral solution in ethanol, and magnetically stirred for 10 h to prepare a polyvinyl butyral / graphene oxide nanosheet mixed solution with excellent compatibility as spinning solution 1.

[0033] Step 2: A mixture of 20 g tetraethyl silicate, 14 g water and 0.16 g oxalic acid was magnetically stirred for 10 h for hydrolysis and condensation reaction to obtain a silicon source hydrolyzate, and then 15 g of 12.5 wt% polyvinyl alcohol solution was added and stirred for 10 h to mix evenly to prepare a silica precursor solution as spinning solution 2.

[0034] Step 3: Spinning solution 1 and spinning solution 2 are poured into different syringes respectively, and the ratio and combination of the two are adjusted for electrostatic spinning, so that the mass ratio of silica nanofibers to graphene oxide nanosheet fillers in the final fiber membrane is 2:1, and the two spinning solutions are extruded simultaneously and received by the same receiving device; the spinning temperature is 24°C, the relative humidity is 40%, the injection speed is 0.7mL / h, the spinning voltage is 18kV, and the receiving distance is 10cm. A composite fiber membrane hybrid fiber membrane in which polyvinyl butyral / graphene oxide nanosheet composite fibers and polyvinyl alcohol / silicon dioxide precursor hybrid fibers are interlaced with each other is prepared. By heating from room temperature to 800°C high temperature calcination at a heating rate of 3°C / min, and maintaining the highest temperature for 150min, the organic components in the two fibers are removed to obtain a flexible fiber / filler composite membrane in which an inorganic micron filler is embedded between the pores of silica nanofibers. The product obtained in this embodiment has a composite structure similar to that of Example 1 in which fillers and fibers are randomly stacked and crossed in three-dimensional space. The flexible silica nanofiber membrane inlaid with micron-sized graphene oxide nanosheets does not burn under the outer flame of an alcohol lamp; after calcination at 1000°C for 2 hours, it only loses 0.5% of heat and is still flexible and can be folded 180°; the air permeability of the flexible silica nanofiber / graphene oxide nanosheet composite membrane is 200 (KPa·s / m) / mm; the thermal insulation performance on a 600°C hot stage is: after standing for 5 minutes, the cold surface of the flexible silica nanofiber / graphene oxide nanosheet composite membrane only heats up to 105°C, and the heating rate does not exceed 1°C / s, which meets the thermal insulation requirements of the national standard GB38031-2020 "Safety Requirements for Electric Vehicle Batteries".

[0035] Comparative Example 1

[0036] Step 1: A mixture of 33 g tetraethyl silicate, 27.3 g water and 0.195 ml phosphoric acid was magnetically stirred for 10 h for hydrolysis and condensation reaction to obtain a silicon source hydrolyzate, and then 24.1 g 12.5 wt% polyvinyl alcohol solution was added and stirred for 10 h to mix evenly to prepare a silica precursor solution as a spinning solution.

[0037] Step 2: Infuse the spinning solution into the syringe for electrospinning, with a spinning temperature of 24°C, a relative humidity of 45%, an injection speed of 0.7 mL / h, a spinning voltage of 20 kV, and a receiving distance of 20 cm. A fiber membrane composed of a composite fiber hybridized with a polyvinyl alcohol / silica precursor was prepared. The organic components in the fiber were removed by calcining at a temperature increase rate of 3°C / min from room temperature to 700°C, and the temperature was maintained at the highest temperature for 240 minutes to obtain a flexible silica nanofiber membrane without micron filler inlay. The flexible silica nanofiber membrane does not burn under the outer flame of an alcohol lamp; after calcination at 1000°C for 2 hours, it only loses 0.3% of heat and is still flexible and can be folded 180°; the thermal insulation performance on a 600°C hot stage is: after standing for 5 minutes, the cold surface of the flexible silica nanofiber membrane heats up to 300°C, and the heating rate exceeds 1°C / s, which does not meet the thermal insulation requirements of the national standard GB38031-2020 "Safety Requirements for Electric Vehicle Batteries".

[0038] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a flexible silica nanofiber membrane inlaid with micron fillers, It is characterized in that The steps include: The first step is to disperse the inorganic micron filler into the organic polymer solution to prepare a polymer / micron filler mixed solution as the spinning solution 1; Step 2: hydrolyze and condense the mixture of silicon source, solvent and catalyst under stirring to obtain silicon source hydrolyzate, then add the polymer solution, mix and stir evenly to prepare silicon dioxide precursor solution as spinning solution 2; Step 3: Pour spinning solution 1 and spinning solution 2 into different syringes respectively, and electrospin the two according to the proportion and combination to prepare a composite fiber membrane hybrid fiber membrane in which polymer / filler composite fibers and polymer / silica precursor hybrid fibers are interspersed with each other; remove the organic components in the two fibers by high-temperature calcination to obtain a flexible silica nanofiber membrane inlaid with micron fillers.

2. The method for preparing the flexible silica nanofiber membrane inlaid with micron fillers according to claim 1, It is characterized in that In the first step, the inorganic micron filler is one or more of hollow silica spheres, hollow glass microspheres, montmorillonite sheets, boron nitride nanosheets, graphene oxide nanosheets, and graphene nanosheets, and the mass percentage of the inorganic micron filler in the spinning solution 1 is 1-50wt%.

3. The method for preparing the flexible silica nanofiber membrane inlaid with micron fillers according to claim 1, It is characterized in that The polymer in the first step and the polymer in the second step can be the same or different in type. The polymer is one or more of polyvinyl alcohol, polyvinyl butyral, and polyvinyl pyrrolidone, and the mass percentage of the polymer in spinning solution 1 is 30-70wt%, and the mass percentage of the polymer in spinning solution 2 is 20-40wt%.

4. The method for preparing the flexible silica nanofiber membrane inlaid with micron fillers according to claim 1, It is characterized in that In the second step, the silicon source is one or more of tetramethyl silicate, tetraethyl silicate, tetrapropyl silicate, tetrabutyl silicate, tetraphenyl silicate, silicon tetrachloride, and silicate, and the mass percentage of the silicon source in the spinning solution 2 is 30-50wt%; the solvent is one or more of deionized water, anhydrous ethanol, and N,N-dimethylformamide, and the mass percentage of the solvent in the spinning solution 2 is 25-45wt%; the catalyst is one or more of oxalic acid, phosphoric acid, hydrochloric acid, acetic acid, sulfuric acid, and nitric acid, and the mass percentage of the catalyst in the spinning solution 2 is 0.1-1wt%.

5. The method for preparing the flexible silica nanofiber membrane inlaid with micron fillers according to claim 1, It is characterized in that In the third step, the spinning solution 1 and the spinning solution 2 are extruded and spun simultaneously and received by the same receiving device, and the number of injectors and the injection rate of each are independent of each other.

6. The method for preparing the flexible silica nanofiber membrane inlaid with micron fillers according to claim 1, It is characterized in that The ratio and combination of the spinning solution 1 and the spinning solution 2 in the third step are such that the mass ratio of the silica nanofibers to the micron filler in the final fiber membrane is 1:0.25-5. Electrospinning refers to the injection of a flow rate of 0.1-50 mL / h into the spinneret of the electrospinning equipment under the conditions of 15-35°C and a relative humidity of 20-70%, and the spinneret is connected to a high voltage power supply of 10-100 kV for electrospinning. The distance between the receiving device and the spinneret is 3-70 cm.

7. The method for preparing the flexible silica nanofiber membrane inlaid with micron fillers according to claim 1, It is characterized in that In the third step, the polymer / filler composite fiber refers to the filler being wholly or partially bound inside the fiber, and the other part of the filler can be exposed outside the fiber; the polymer / silica precursor hybrid fiber refers to the silica and polymer components being uniformly distributed in the fiber; the interpenetration refers to the polymer / filler composite fiber and the polymer / silica precursor hybrid fiber being randomly stacked and crossed in three-dimensional space.

8. The method for preparing the flexible silica nanofiber membrane inlaid with micron fillers according to claim 1, It is characterized in that In the third step, the high temperature calcination is carried out by heating the temperature to 200-800°C at a heating rate of 0.1-10°C / min and maintaining the highest temperature for 10-360 minutes.

9. The method for preparing the flexible silica nanofiber membrane inlaid with micron fillers according to claim 1, It is characterized in that In the third step, the embedding means that the calcined inorganic filler is trapped in the pores between the silica fibers and cannot fall off. There is no hard sintering between the inorganic filler and the silica, and the inorganic filler can produce a small rotation and slip in the pores between the fibers.

10. A flexible silica nanofiber membrane inlaid with micron fillers prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for preparing graphene / silica nanocomposite fiber through coaxial electrostatic spinning

    CN106637502A

  • Flexible high-strength silicon dioxide nanofiber membrane and preparation method thereof

    CN113944008A

  • Polyimide reinforced and toughened silicon dioxide nanofiber membrane and preparation method thereof

    CN114164666A

  • Inorganic nanoparticle-matrix material fibrous composite and method for producing the same

    JP2010229560A

  • Polymer composite membrane and preparation method thereof, GEL electrolyte and lithium ion battery having the same

    WO2016165633A1

Cited By

  • Device and method for preparing 1-10 [mu] m spherical core-shell structure metal powder

    CN119057071A

  • Hollow silicon dioxide microsphere modified heat insulation and noise reduction ceramic composite fiber and preparation method thereof

    CN119913747A

  • Light-shielding and heat-insulating film material for potassium chloride granular preparation and preparation method of light-shielding and heat-insulating film material

    CN120422522A

  • A light-proof and heat-insulating film material for a potassium chloride granule preparation and a method for preparing the same

    CN120422522B

  • A belt-shaped silica nanofiber membrane and a method for preparing the same

    CN122669549A