Diaphragm

By using silver salt to modify the separator in lithium metal batteries, a high-ionic conductivity SEI protective layer is formed, which solves the safety problems caused by lithium dendrites, and improves the safety of the battery and the efficiency of the Coulomb.

CN118920012APending Publication Date: 2024-11-08DONGFENG MOTOR GRP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411180516.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The continuous growth of lithium dendrites in lithium metal batteries causes the diaphragm to be pierced, causing safety issues.

Method used

A separator including a base film and a silver salt coating is used, and the silver salt dissociates into silver ions and anions to form a high ionic conductivity and stable SEI protective layer to inhibit the growth of lithium dendrites.

Benefits of technology

The nucleation overpotential of the lithium deposition reaction is reduced by modifying the separator, and the lithium deposition is uniform, forming a continuous Li-Ag alloy and a high ionic conductivity SEI protective layer, which improves the safety of lithium metal batteries and the efficiency of Coulomb.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118920012A_ABST
    Figure CN118920012A_ABST
Patent Text Reader

Abstract

The invention relates to a diaphragm, which is applied to a lithium metal battery and comprises a base membrane and a coating attached to at least part of the surface of the base membrane, wherein the coating layer comprises the following paint components: silver salt; the silver salt can be dissociated into silver ions and anions, the anions can participate in the formation of a high-ionic-conductivity and stable SEI protective layer on the surface of a lithium metal electrode, and the mass fraction of the silver salt in the components of the coating is 80-95%. According to the invention, the modified diaphragm is modified by the silver salt, and Ag < + > can form a lithium-silver alloy on metal lithium, so that the nucleation overpotential of a lithium deposition reaction is reduced, and the deposition of lithium is uniform; anions can participate in forming a high-ionic-conductivity and stable SEI protection layer on the surface of the lithium metal negative electrode; as the dissociation of the silver salt is a continuous process, a lithium-silver alloy and a stable SEI protection layer with high ionic conductivity are always formed on the lithium metal negative electrode, so that the growth of lithium dendrites is inhibited, and finally, the safety of the lithium metal battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium metal batteries, and in particular to a diaphragm. Background Art

[0002] With the explosive growth in demand for portable electronic devices and new energy vehicles, the development of secondary lithium metal batteries with higher energy density is urgent. In the industrial pre-research project, in order to further improve the energy density of the battery, lithium metal batteries using metallic lithium as the negative electrode have attracted much attention. They have ultra-high theoretical specific capacity (3860mAh / g), extremely low standard redox potential (-3.04V) and extremely small density, and have excellent performance in solid-state batteries and new battery systems such as lithium-sulfur batteries / lithium-air batteries.

[0003] However, the development of lithium metal batteries also faces many challenges. The most critical problem is the continuous growth of lithium dendrites, which pierce the separator and cause battery safety problems. Summary of the invention

[0004] The present application provides a separator to solve the following technical problem: how to improve the safety of lithium metal batteries.

[0005] In a first aspect, the present application provides a diaphragm for use in a lithium metal battery, the diaphragm comprising a base film and a coating attached to at least a portion of the surface of the base film; wherein the coating component of the coating comprises: a silver salt; the silver salt can be dissociated into silver ions and anions, and the anions can participate in forming a high ionic conductivity and stable SEI protective layer on the electrode surface;

[0006] In the coating composition, the content of the silver salt is 80% to 95% by mass.

[0007] Optionally, the content of the silver salt is 87% to 92%.

[0008] Optionally, the silver salt includes at least one of the following: silver nitrate and silver fluoride.

[0009] Optionally, the coating composition further includes at least one of the following: a dispersant, a binder and conductive carbon black.

[0010] Optionally, the dispersant includes at least one of the following: carboxymethyl cellulose salt and polyacrylate.

[0011] Optionally, the carboxymethyl cellulose salt includes one of the following: lithium carboxymethyl cellulose, sodium carboxymethyl cellulose; and / or,

[0012] The polyacrylate comprises at least one of the following: polyacrylic acid and sodium polyacrylate.

[0013] Optionally, the binder includes at least one of the following: polyvinylidene fluoride, polyacrylic acid, and sodium alginate.

[0014] Optionally, the conductive carbon black includes at least one of the following: BP2000, Super P, Ketjen black, acetylene black, conductive graphite flakes, and carbon nanotubes.

[0015] Optionally, in the coating composition, the content of the dispersant is 0.2% to 3%, the content of the binder is 1% to 10%, and the content of the conductive carbon black is 1% to 10% by mass.

[0016] Optionally, the material of the base film includes at least one of the following: polyolefin, polyethylene oxide, polyvinylidene fluoride, hexafluoropropylene copolymer, polyvinyl chloride, polytetrafluoroethylene, polyacrylonitrile, polymethyl methacrylate, polyimide, cellulose, and polyurethane.

[0017] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0018] The diaphragm provided in the embodiment of the present application is applied to lithium metal batteries, and the diaphragm includes a base film and a coating attached to at least part of the surface of the base film; wherein the coating component of the coating includes: silver salt; the silver salt can dissociate into silver ions and anions, and the anions can participate in the formation of a high ionic conductivity and stable SEI protective layer on the surface of the lithium metal electrode. In the coating component, the content of the silver salt is 80% to 95% by mass. The diaphragm is modified by using silver salt, and when the lithium metal battery containing the diaphragm is in operation, the silver salt can dissociate into Ag and N. + and anions; Ag + Bili + With higher redox potential, free Ag + It will be reduced by the metallic lithium at the negative terminal to form a lithium-silver alloy (Li-Ag alloy) thereon, which can reduce the nucleation overpotential of the lithium deposition reaction and uniformly deposit lithium; the anions can participate in the formation of a high ion conductivity and stable SEI protective layer on the surface of the lithium metal negative electrode; since the dissociation of the silver salt is a continuous process, a Li-Ag alloy and a high ion conductivity and stable SEI protective layer will always be formed on the lithium metal negative electrode, thereby inhibiting the growth of lithium dendrites, ultimately reflecting the improvement of the safety of lithium metal batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0020] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0021] Figure 1 A schematic flow chart of a method for preparing a diaphragm provided in an embodiment of the present application. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0023] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0024] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the specification of the present application, the terms "include", "comprise", etc. refer to "including but not limited to". In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" refers to one or more, and "multiple" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all represent: a, b, c, ab (i.e., a and b), ac, bc or abc, where a, b, c can be single or multiple, respectively.

[0025] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0026] At present, the development challenges of lithium metal batteries are that the uneven lithium flux and electrode exchange current density will lead to the growth of lithium dendrites, and the continuous growth of lithium dendrites will pierce the diaphragm, leading to battery safety issues. For this application scenario, in addition to conventional lithium metal / current collector modification and electrode interface modification, functional coating modification from the diaphragm end is a practical and effective solution. Therefore, the present application provides a diaphragm, which can be applied to lithium metal batteries, the diaphragm includes a base film and a coating attached to at least part of the surface of the base film; wherein the coating component of the coating includes: silver salt; the silver salt can dissociate into silver ions and anions, and the anions can participate in the formation of a high ionic conductivity and stable SEI protective layer on the electrode surface; in the coating component, the content of the silver salt is 80% to 95% by mass.

[0027] In some embodiments, the content of the silver salt is 87% to 92%.

[0028] In the embodiment of the present application, the diaphragm is modified by using a silver salt. When the lithium metal battery containing the diaphragm is working, the silver salt will dissociate into Ag + and anions; Ag + Bili + With higher redox potential, free Ag +It will be reduced by the metallic lithium at the negative terminal to form a lithium-silver alloy (Li-Ag alloy) thereon, which can reduce the nucleation overpotential of the lithium deposition reaction and uniformly deposit lithium; the anions can participate in the formation of a high ion conductivity and stable SEI protective layer on the surface of the lithium metal negative electrode; since the dissociation of the silver salt is a continuous process, a Li-Ag alloy and a high ion conductivity and stable SEI protective layer will always be formed on the lithium metal negative electrode, thereby inhibiting the growth of lithium dendrites, and ultimately reflecting the improvement of the safety of lithium metal batteries. In the above-mentioned coating components, the content of silver salt can be 80% to 95% by mass, thereby ensuring the role of silver salt in inhibiting the growth of lithium dendrites, while avoiding excessive silver salt content that damages the conductivity, mechanical properties and stability of the diaphragm. Exemplarily, the content of the above silver salt can be 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95% and the like; further, the content of the above silver salt can be 87%, 88%, 89%, 90%, 91%, 92% and the like.

[0029] In some embodiments, the silver salt comprises at least one of the following: silver nitrate, silver fluoride.

[0030] In the embodiment of the present application, the silver salt can be a combination of one or more of silver nitrate and silver fluoride. For example, the silver salt is silver nitrate. When the lithium metal battery using the silver nitrate modified diaphragm is working, the silver nitrate will dissociate into Ag in the electrolyte. + and NO3 - . Due to Ag + Bili + With higher redox potential, free Ag + It will be reduced by the metallic lithium at the negative terminal to form a lithium-silver alloy (Li-Ag alloy) on it, which can reduce the nucleation overpotential of the lithium deposition reaction and uniformly deposit lithium; NO3 dissociated from silver nitrate - It can participate in the formation of a highly ionic conductive and stable SEI protective layer on the surface of the lithium metal negative electrode. Since the dissociation of silver nitrate is a continuous process, a Li-Ag alloy and a highly ionic conductive and stable SEI protective layer will always be formed on the lithium metal negative electrode, thereby inhibiting the growth of lithium dendrites and improving the electrochemical and safety performance of lithium metal batteries. Similarly, the fluoride ions in silver fluoride can generate lithium fluoride on the surface of the lithium metal negative electrode, thereby participating in the formation of a highly ionic conductive and stable SEI protective layer.

[0031] In some embodiments, the coating composition further comprises at least one of the following: a dispersant, a binder, and conductive carbon black.

[0032] In an embodiment of the present application, the coating composition further includes an additive, which may be a combination of one or more of a dispersant, a binder, and conductive carbon black. Among them, the dispersant can enhance the affinity between the surface of the silver salt particles and the medium, and make the silver salt particles in the coating slurry easy to infiltrate and maintain a uniform dispersion state, thereby preventing the agglomeration of the silver salt particles. The binder can make the silver salt particles and the conductive carbon material particles adhere closely to the base film. The conductive carbon black can enhance the conductivity of the diaphragm. At the same time, the conductive carbon black can effectively improve the conductivity of the silver salt modified diaphragm, further improving the coulombic efficiency of the battery.

[0033] In some embodiments, the dispersant includes at least one of: a carboxymethyl cellulose salt and a polyacrylate salt.

[0034] In some embodiments, the carboxymethyl cellulose salt comprises one of the following: lithium carboxymethyl cellulose, sodium carboxymethyl cellulose; and / or,

[0035] The polyacrylate comprises at least one of the following: polyacrylic acid and sodium polyacrylate.

[0036] In the embodiments of the present application, the dispersant may be a combination of one or more of carboxymethyl cellulose salt and polyacrylic acid salt, and these dispersants may enhance the affinity between the surface of the silver salt particles and the remaining auxiliary medium, so that the silver salt particles can be easily wetted and uniformly dispersed in the coating slurry, thereby preventing the agglomeration of the silver salt particles, and ultimately maximizing the advantageous effects of the silver salt; wherein the carboxymethyl cellulose salt may be a combination of one or more of lithium carboxymethyl cellulose and sodium carboxymethyl cellulose, and the polyacrylic acid salt may be a combination of one or more of polyacrylic acid and sodium polyacrylate, and further, the dispersant may be sodium carboxymethyl cellulose (CMC).

[0037] In some embodiments, the binder includes at least one of the following: polyvinylidene fluoride (PVDF), polyacrylic acid (PAA), and sodium alginate (SA).

[0038] In an embodiment of the present application, the binder may be a combination of one or more of polyvinylidene fluoride (PVDF), polyacrylic acid (PAA), and sodium alginate (SA). These binders can make the silver salt particles and the conductive carbon material particles adhere tightly to the base film. Furthermore, the binder may be polyacrylic acid (PAA).

[0039] In some embodiments, the conductive carbon black includes at least one of the following: BP2000, Super P, Ketjen black, acetylene black, conductive graphite flakes, and carbon nanotubes.

[0040] In the embodiments of the present application, the conductive carbon black may be a combination of one or more of BP2000, Super P, Ketjen black, acetylene black, conductive graphite sheets, and carbon nanotubes. These conductive carbon blacks can enhance the conductivity of the diaphragm. Furthermore, the conductive carbon black may be BP2000.

[0041] In some embodiments, in the coating composition, by mass fraction, the content of the dispersant is 0.2% to 3%, the content of the binder is 1% to 10%, and the content of the conductive carbon black is 1% to 10%.

[0042] In the embodiment of the present application, in the above-mentioned coating components, the content of the above-mentioned dispersant can be 0.2% to 3%, the content of the above-mentioned binder can be 1% to 10%, and the content of the above-mentioned conductive carbon black can be 1% to 10%. The content of the coating components is reasonably designed to give play to the above-mentioned advantages of the dispersant, binder and conductive carbon, while avoiding excessive content thereof and destroying the conductivity, mechanical properties and stability of the diaphragm. Exemplarily, the content of the above-mentioned dispersant can be 0.2%, 0.5%, 1%, 2%, 3%, etc., the content of the above-mentioned binder can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc., and the content of the above-mentioned conductive carbon black is 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc.

[0043] In some embodiments, the material of the base film includes at least one of the following: polyolefin, polyethylene oxide, polyvinylidene fluoride, hexafluoropropylene copolymer, polyvinyl chloride, polytetrafluoroethylene, polyacrylonitrile, polymethyl methacrylate, polyimide, cellulose, and polyurethane.

[0044] In the embodiment of the present application, the material of the base film can be a combination of one or more of polyolefin, polyethylene oxide, polyvinylidene fluoride, hexafluoropropylene copolymer, polyvinyl chloride, polytetrafluoroethylene, polyacrylonitrile, polymethyl methacrylate, polyimide, cellulose, and polyurethane. Furthermore, polyethylene (PE) among polyolefins can be selected.

[0045] For the preparation method of the above-mentioned diaphragm, please refer to Figure 1The schematic flow diagram of a method for preparing a diaphragm provided in an embodiment of the present application is shown, comprising: S1, obtaining a coating containing a silver salt; S2, applying the coating to at least a portion of the surface of a base film to obtain a diaphragm. More specifically, S1 comprises: weighing the raw materials according to the above-mentioned mass fractions of the silver salt, dispersant, binder, and conductive carbon black, mixing the dispersant and the solvent evenly to obtain a dispersion, adding the dispersion to the silver salt powder material, and then adding the binder and conductive carbon black and stirring to obtain a coating slurry; S2 comprises: applying the coating slurry on one side / both sides of the base film using a micro-concave coater, the base film thickness is 9 to 11 μm, and the coating thickness is 2 to 3 μm. Among them, the solvent can be a combination of one or more of water, N-methylpyrrolidone (NMP), ethanol, and acetone to form a coatable slurry.

[0046] The diaphragm is used to prepare a lithium metal battery. In addition, the above-mentioned lithium metal battery includes: a positive electrode, a lithium metal negative electrode, an electrolyte and a diaphragm, and the diaphragm is the above-mentioned silver salt modified diaphragm. Furthermore, the positive electrode material includes a combination of one or more of lithium iron phosphate material, lithium iron manganese phosphate material, ternary positive electrode material, lithium manganese-rich based material and lithium nickel manganese oxide material; the electrolyte is composed of lithium salt and carbonate solvent. Since the lithium metal battery adopts part or all of the technical solutions of the above-mentioned embodiments, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be repeated here.

[0047] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0048] Example 1

[0049] A diaphragm comprises a base film and a coating attached to the surface of the base film; wherein the coating composition of the coating comprises: silver nitrate, dispersant CMC, and binder PAA; in the coating composition, by mass fraction, the content of silver nitrate is 95%, the content of CMC is 1%, and the content of PAA is 4%.

[0050] A preparation method of a diaphragm comprises: weighing raw materials according to a mass ratio of silver nitrate, CMC and PAA of 95:1:4, mixing CMC and deionized water evenly to obtain a dispersion, adding the dispersion to a silver nitrate powder material, and then adding PAA, stirring for 30 minutes to obtain a coating slurry; coating the coating slurry on both sides of a PE base film by using a micro-concave coater, the base film thickness is 9 μm, and the coating thickness is 2 μm.

[0051] Example 2

[0052] A diaphragm, comprising a base film and a coating attached to the surface of the base film; wherein the coating composition of the coating comprises: silver nitrate, dispersant CMC, binder PAA, conductive agent BP2000; in the coating composition, by mass fraction, the content of silver nitrate is 90%, the content of CMC is 1%, the content of PAA is 4%, and the content of conductive agent BP2000 is 5%.

[0053] A preparation method of a diaphragm comprises: weighing raw materials according to a mass ratio of silver nitrate, CMC, PAA and BP2000 of 90:1:4:5, mixing CMC and deionized water to obtain a dispersion, adding the dispersion to silver nitrate powder material and BP2000, and then adding PAA, stirring for 30 minutes to obtain a coating slurry; coating the coating slurry on both sides of a PE base film by using a micro-concave coater, the base film thickness is 9 μm, and the coating thickness is 2 μm.

[0054] Example 3

[0055] A diaphragm, comprising a base film and a coating attached to the surface of the base film; wherein the coating composition of the coating comprises: silver nitrate, dispersant CMC, binder PAA, conductive agent BP2000; in the coating composition, by mass fraction, the content of silver nitrate is 80%, the content of CMC is 3%, the content of PAA is 7%, and the content of conductive agent BP2000 is 10%.

[0056] A preparation method of a diaphragm comprises: weighing raw materials according to a mass ratio of silver nitrate, CMC, PAA and BP2000 of 80:3:7:10, mixing CMC with deionized water to obtain a dispersion, adding the dispersion to silver nitrate powder material and BP2000, then adding PAA, and stirring for 30 minutes to obtain a coating slurry; coating the coating slurry on both sides of a PE base film by using a micro-concave coater, the base film thickness is 9 μm, and the coating thickness is 2 μm.

[0057] Example 4

[0058] A diaphragm comprises a base film and a coating attached to the surface of the base film; wherein the coating composition of the coating comprises: silver fluoride, dispersant CMC, and binder PAA; in the coating composition, by mass fraction, the content of silver fluoride is 95%, the content of CMC is 1%, and the content of PAA is 4%.

[0059] A preparation method of a diaphragm comprises: weighing raw materials according to a mass ratio of silver fluoride, CMC and PAA of 95:1:4, mixing CMC and deionized water to obtain a dispersion, adding the dispersion to a silver fluoride powder material, then adding PAA, and stirring for 30 minutes to obtain a coating slurry; coating the coating slurry on both sides of a PE base film by using a micro-concave coater, the base film thickness is 9 μm, and the coating thickness is 2 μm.

[0060] Example 5

[0061] A diaphragm, comprising a base film and a coating attached to the surface of the base film; wherein the coating composition of the coating comprises: silver fluoride, dispersant CMC, binder PAA, conductive agent BP2000; in the coating composition, by mass fraction, the content of silver fluoride is 90%, the content of CMC is 1%, the content of PAA is 4%, and the content of conductive agent BP2000 is 5%.

[0062] A preparation method of a diaphragm comprises: weighing raw materials according to a mass ratio of silver fluoride, CMC, PAA and BP2000 of 90:1:4:5, uniformly mixing CMC with deionized water to obtain a dispersion, adding the dispersion to silver fluoride powder material and BP2000, then adding PAA, and stirring for 30 minutes to obtain a coating slurry; coating the coating slurry on both sides of a PE base film by using a micro-concave coater, the base film thickness is 9 μm, and the coating thickness is 2 μm.

[0063] Comparative Example 1

[0064] A commercial PVDF separator.

[0065] The diaphragms obtained in Examples 1 to 5 and Comparative Example 1 were respectively applied to a lithium metal battery, the lithium metal battery comprising: a positive electrode, a lithium metal negative electrode, an electrolyte and a diaphragm, the specific components of the electrolyte comprising: lithium hexafluorophosphate, ethylene carbonate (EC), ethyl methyl carbonate (EMC), fluoroethylene carbonate (FEC) and vinylene carbonate (VC). A Li||Li symmetric cell (CR2032 button cell) was assembled in a glove box filled with argon.

[0066] Performance Test:

[0067] The batteries obtained in Examples 1 to 5 and Comparative Example 1 were subjected to charge and discharge tests at a current density of 1 mA / cm 2 The number of cycles is 200, and all the metallic lithium at the negative electrode is removed at the 201st cycle, and the average coulombic efficiency is calculated based on this. Please refer to the charge and discharge test results of the battery shown in Table 1.

[0068] Table 1 Battery charge and discharge test results

[0069] Group First week coulomb efficiency 200-week average coulomb efficiency Example 1 99.7% 96.6% Example 2 99.8% 99.4% Example 3 99.7% 98.5% Example 4 99.7% 95.4% Example 5 99.8% 99.1% Comparative Example 1 99.6% 88.2%

[0070] It can be seen from Table 1 that the average coulombic efficiency of the battery assembled using the silver salt modified diaphragm is significantly improved compared with the ordinary commercial diaphragm, which indicates that the growth of lithium dendrites is inhibited, the formation of dead lithium is reduced, and the safety performance of the battery is improved; through the analysis of Examples 1 and 2, as well as Examples 4 and 5, adding conductive carbon black to the diaphragm coating can effectively improve the conductivity of the silver salt modified diaphragm and further improve the coulombic efficiency.

[0071] One or more technical solutions in the embodiments of the present application also have at least the following technical effects or advantages:

[0072] (1) The present invention uses a silver salt to modify the preparation of the modified diaphragm, and the dissociated Ag + A lithium-silver alloy (Li-Ag alloy) can be formed on metallic lithium, thereby reducing the nucleation overpotential of the lithium deposition reaction and making the lithium deposition uniform; the anions dissociated from the silver salt can participate in forming a high ion conductivity and stable SEI protective layer on the surface of the lithium metal negative electrode; since the dissociation of the silver salt is a continuous process, a Li-Ag alloy and a high ion conductivity and stable SEI protective layer will always be formed on the lithium metal negative electrode, thereby inhibiting the growth of lithium dendrites, and ultimately reflecting the improvement of the safety of lithium metal batteries;

[0073] (2) The present embodiment of the present invention can effectively improve the conductivity of the silver salt modified diaphragm by adding conductive carbon black to the diaphragm coating, thereby further improving the coulombic efficiency;

[0074] (3) The diaphragm provided in the embodiments of the present application is used to prepare lithium metal batteries, which effectively improves the safety performance and cycle life of lithium metal batteries;

[0075] (4) The preparation process of the diaphragm provided in the embodiments of the present application is simple, matches existing process equipment, is suitable for large-scale production, and is highly economical.

[0076] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A diaphragm, characterized in that: Applied to lithium metal batteries, the diaphragm includes a base film and a coating attached to at least a portion of the surface of the base film; wherein the coating composition of the coating includes: a silver salt; the silver salt can be dissociated into silver ions and anions, and the anions can participate in forming a high ion conductivity and stable SEI protective layer on the surface of the lithium metal electrode; In the coating composition, the content of the silver salt is 80% to 95% by mass.

2. The diaphragm according to claim 1, characterized in that The content of the silver salt is 87% to 92%.

3. The diaphragm according to claim 1, characterized in that The silver salt includes at least one of the following: silver nitrate and silver fluoride.

4. The diaphragm according to claim 1, characterized in that The coating composition further includes at least one of the following: a dispersant, a binder and conductive carbon black.

5. The diaphragm according to claim 4, characterized in that The dispersant includes at least one of the following: carboxymethyl cellulose salt and polyacrylate.

6. The diaphragm according to claim 5, characterized in that The carboxymethyl cellulose salt includes one of the following: lithium carboxymethyl cellulose, sodium carboxymethyl cellulose; and / or, The polyacrylate comprises at least one of the following: polyacrylic acid and sodium polyacrylate.

7. The diaphragm according to claim 4, characterized in that The binder includes at least one of the following: polyvinylidene fluoride, polyacrylic acid, and sodium alginate.

8. The diaphragm according to claim 4, characterized in that The conductive carbon black includes at least one of the following: BP2000, Super P, Ketjen black, acetylene black, conductive graphite flakes, and carbon nanotubes.

9. The diaphragm according to any one of claims 4 to 8, characterized in that: In the coating composition, the content of the dispersant is 0.2% to 3% by mass, the content of the binder is 1% to 10% by mass, and the content of the conductive carbon black is 1% to 10% by mass.

10. The diaphragm according to claim 1, characterized in that The material of the base film includes at least one of the following: polyolefin, polyethylene oxide, polyvinylidene fluoride, hexafluoropropylene copolymer, polyvinyl chloride, polytetrafluoroethylene, polyacrylonitrile, polymethyl methacrylate, polyimide, cellulose, and polyurethane.

Citation Information

Patent Citations

  • Fluorine-containing diaphragm, negative electrode interface modification material, method for performing interface modification on negative electrode material and battery

    CN114883749A