Carbon fiber substrate, prepreg, porous structure, method for producing said porous structure, preform, fiber-reinforced resin molded article, sandwich structure, and aircraft member

By using resin composition and binder resin in carbon fiber substrates, a nonwoven fabric structure is formed, which solves the heat resistance and forming processability of carbon fiber substrates in high-temperature and high-pressure processes, and realizes the dispersion of carbon fibers and the lightweight porous structure of carbon fibers Improvement of quantitative and mechanical properties.

CN118922597APending Publication Date: 2024-11-08TORAY INDUSTRIES INC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380029240.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-09
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing carbon fiber substrates have the challenges of coexisting formation processability and heat resistance in high-temperature and high-pressure processes, especially when using high-melting matrix resins, it is difficult to maintain the dispersed state of carbon fibers and the mechanical properties of the prepreg.

Method used

Using a carbon fiber substrate containing carbon fiber and a resin composition coated with carbon fiber surfaces, the dispersion and bonding effect of carbon fibers are ensured through the selection of specific resin compositions and adhesive resins, and a nonwoven fabric structure is formed to improve tensile strength and Heat resistance, and a porous structure is formed through the heating and expansion process.

Benefits of technology

The heat resistance and forming processability of the carbon fiber substrate under high temperature and high pressure conditions are improved, and the damage is prevented, and the dispersed state of carbon fiber is maintained, so as to obtain a prepreg and a porous structure with excellent heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922597A_ABST
    Figure CN118922597A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to obtain a carbon fiber substrate having both heat resistance and moldability at a high level, and to provide a highly heat-resistant prepreg or porous structure using the carbon fiber substrate. The present invention is a carbon fiber base material comprising carbon fibers (A) and a resin composition (B) that covers the surface of the carbon fibers (A), the carbon fibers (A) forming a non-woven fabric, and the tensile strength of the carbon fiber base material after heating at 300 DEG C for 5 minutes being at least 110% of the tensile strength before heating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a carbon fiber substrate and a prepreg. Background Art

[0002] Fiber-reinforced composite materials that use a reinforcing fiber substrate such as a carbon fiber substrate as a reinforcing material and are impregnated with a matrix resin in their pores are light in weight and have excellent mechanical properties such as strength or rigidity, so they are used in a variety of fields such as aviation / aerospace, automobiles, railway vehicles, ships, civil engineering, electronic equipment, industrial machinery, and sporting goods. In particular, the use of carbon fiber nonwoven fabrics for prepregs of carbon fiber substrates or porous structures formed by expanding them has the advantages of excellent mechanical properties and excellent processability for complex shapes such as thin walls or three-dimensional shapes. In addition, the use of nonwoven fabrics made by dispersing reinforcing fibers horizontally in single filaments and orienting the fibers isotropically for prepregs of reinforcing fiber substrates has the advantage of high design freedom of the stacked structure because the mechanical properties are isotropic, so there is no need to perform stacking to compensate for the low strength direction such as quasi-isotropic stacking. This prepreg can be used as a thin-walled single-layer body, or as a preformed body formed by freely stacking multiple prepregs for molding purposes, and can be formed into a non-voided fiber-reinforced resin molded body by heating and pressurizing, or formed into a voided body by heating and expansion, so it has the advantage of excellent processability for complex shapes such as thin walls or three-dimensional shapes. Patent document 1 shows a fiber-reinforced composite material having a carbon fiber substrate to which an adhesive is applied and a matrix resin impregnated therein.

[0003] On the other hand, when these uses are developed, the coexistence of molding processability and heat resistance is a continuous issue. In particular, the matrix resin required by the market is being promoted to have high heat resistance, and as a result, the impregnation process is becoming high temperature and high pressure, and there is a problem of developing a carbon fiber substrate that can withstand such a process and has excellent molding processability. In Patent Documents 2 and 3, as a carbon fiber for obtaining a fiber-reinforced resin with high heat resistance, a carbon fiber coated with polyetherimide as a sizing agent is disclosed.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Publication No. 2010 / 013645

[0007] Patent Document 2: Japanese Patent Publication No. 02-002990

[0008] Patent Document 3: Japanese Patent Publication No. 2014-500912 Summary of the invention

[0009] Problems to be solved by the invention

[0010] Patent Document 1 does not disclose a carbon fiber substrate that corresponds to a high temperature and high pressure process associated with the use of a high melting point matrix resin, and there is a problem of further improving heat resistance and molding processability. Patent Documents 2 and 3 are technologies related to sizing agents, which are not sufficient for impregnation or coating in reinforcing fibers in a non-woven fabric shape.

[0011] An object of the present invention is to provide a carbon fiber base material having both moldability and heat resistance.

[0012] Technical means of solving problems

[0013] The present invention is a carbon fiber substrate, comprising carbon fibers (A) and a resin composition (B) covering the surface of the carbon fibers (A), wherein the carbon fibers (A) form a nonwoven fabric, and the tensile strength of the carbon fiber substrate after heating at 300°C for 5 minutes is at least 110% of that before the heating.

[0014] The present invention is also a prepreg obtained by impregnating a base material derived from the carbon fiber base material of the present invention with a matrix resin (C) (first embodiment).

[0015] The present invention also provides a prepreg, which is obtained by impregnating a base material comprising carbon fibers (A) and an adhesive resin composition (D) with a matrix resin (C), wherein:

[0016] The carbon fiber (A) is discontinuous fiber and forms a non-woven fabric.

[0017] The glass transition temperature of the adhesive resin composition (D) is 120° C. or higher and 450° C. or lower.

[0018] The melting point of the matrix resin (C) is 250° C. or higher and 400° C. or lower.

[0019] The adhesive resin composition (D) is present at the interface between the carbon fiber (A) and the matrix resin (C).

[0020] The prepreg satisfies the following conditions (i) and (ii) (second aspect).

[0021] (i) The minimum value of tensile strength is 100 MPa or more.

[0022] (ii) The thickness deviation at 400° C. is 10% or less.

[0023] The present invention also provides a porous structure formed from the prepreg of the present invention.

[0024] In addition, the present invention is a method for producing a porous structure, which is a method for producing the porous structure of the present invention, and includes: a first step of melting and expanding the matrix resin (C); and a second step of solidifying the matrix resin (C).

[0025] The present invention also provides a preform including the prepreg of the present invention as a lamination unit.

[0026] The present invention is also a fiber-reinforced resin molded product obtained by heating and pressurizing the preform of the present invention.

[0027] The present invention is also a fiber-reinforced resin molded body formed by heating and expanding the preform of the present invention, and having voids.

[0028] The present invention is also a sandwich structure in which the fiber-reinforced resin molded body of the present invention is sandwiched as a core material between a pair of skin materials and integrated.

[0029] The present invention is also an aircraft component including the prepreg of the present invention, the porous structure of the present invention, the fiber-reinforced resin molded body of the present invention, or the sandwich structure of the present invention.

[0030] Effects of the Invention

[0031] The carbon fiber substrate of the present invention has excellent shapeability to flexibly follow the mold in the initial stage of fiber-reinforced resin molding. In addition, it is possible to prevent molding defects such as breakage under the high temperature and high pressure process of impregnating the matrix resin. Furthermore, the carbon fiber substrate of the present invention can maintain the dispersed state of the carbon fibers, and can easily obtain a prepreg or fiber-reinforced resin with excellent heat resistance, or a porous structure.

[0032] In addition, the prepreg of the present invention can achieve both heat resistance and isotropy of mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] [ Figure 1 ] Figure 1 The figure on the right is an enlarged view showing the state of the carbon fiber (A) and the resin composition (B) attached to the surface thereof.

[0034] [ Figure 2 ] Figure 2 This is a schematic diagram showing one embodiment of the prepreg of the present invention together with an enlarged view of its internal cross section.

[0035] [ Figure 3 ] Figure 3 This is a schematic diagram showing one embodiment of the porous structure of the present invention together with an enlarged image of its internal cross section.

[0036] [ Figure 4 ] Figure 4 This is a schematic diagram for explaining the pore diameter of a porous structure. DETAILED DESCRIPTION

[0037] In the present invention, the thickness direction of the prepreg is referred to as an out-of-plane direction, and the direction perpendicular to the out-of-plane direction is referred to as an in-plane direction.

[0038] [Carbon fiber substrate]

[0039] The carbon fiber substrate of the present invention comprises carbon fibers (A) and a resin composition (B) covering the surface of the carbon fibers (A).

[0040] Among the fibers known as reinforcing fibers, carbon fiber (A) also has excellent mechanical properties and lightness. As carbon fiber (A), polyacrylonitrile (PAN), rayon, and asphalt carbon fibers can be exemplified. From the perspective of mechanical properties and economic efficiency, PAN carbon fibers are preferred. Among PAN carbon fibers, from the perspective of mechanical properties of the obtained fiber-reinforced substrate, it is preferred to use carbon fibers with an elastic modulus of 200 GPa or more. In addition, from the perspective of cost, it is also preferred to use recycled carbon fibers.

[0041] The thermal mass reduction rate of carbon fiber (A) at 400°C is preferably 1% by mass or less. The thermal mass reduction rate is more preferably 0% by mass or more and 1% by mass or less. In the present invention, carbon fiber (A) is preferably a discontinuous fiber as described later, and a carbon fiber substrate is formed by bonding with a resin composition (B). If it is assumed that the heat resistance of carbon fiber (A) is low, the decomposition gas will cause the interface between carbon fiber (A) and resin composition (B) to peel off, and sometimes the bonding effect becomes insufficient. Therefore, it is preferred to set the thermal mass reduction rate of carbon fiber (A) to the range. The thermal mass reduction rate can be calculated by the following formula.

[0042] Thermal mass reduction rate (mass %) = [(M1-M2) / M1] × 100

[0043] Here, M1 is the mass (mg) of the sample after isothermally maintaining at 30°C for 10 minutes, and M2 is the mass (mg) of the sample when the temperature is subsequently increased at 10°C / min to 400°C.

[0044] The diameter of the carbon fiber (A) is preferably 1 μm to 20 μm, more preferably 3 μm to 10 μm, and further preferably 6 μm to 8 μm. By setting it within the above range, the dispersibility of the carbon fiber is excellent, and the high porosity and mechanical properties of the carbon fiber substrate can be effectively achieved. In addition, the mechanical properties of the prepreg obtained from the carbon fiber substrate can also be made better.

[0045] In the present invention, the carbon fiber (A) constituting the nonwoven fabric is preferably a discontinuous fiber, more preferably a number average fiber length of 0.1 mm to 100 mm, further preferably 1 mm to 20 mm, and particularly preferably 3 mm to 10 mm. By setting it to the above range, it is easy to expand the spacing between the fibers in the mesh structure of the nonwoven fabric, and it is easy to control the formation of pores. Regarding the number average fiber length of the carbon fiber (A), 400 carbon fibers (A) can be randomly selected, and the fiber lengths of these can be measured using an optical microscope, and the total fiber length can be divided by the number of measured fibers to calculate.

[0046] The carbon fiber (A) preferably contains 50% by mass or more of fibers having a fiber length of 2 mm or more and 10 mm or less, more preferably 3 mm or more and 8 mm or less, and more preferably 5 mm or more and 7 mm or less. The content is more preferably 80% by mass or more and 100% by mass or less, and more preferably 100% by mass. By setting the content in the above range, the carbon fibers (A) constituting the mesh of the nonwoven fabric are dispersed with each other, and the formation of pores or isotropic fiber orientation is easily controlled.

[0047] As a method for collecting samples in the method for measuring fiber length, there are, for example, the following methods: a dissolution method using an organic solvent; a melting method in which a resin component is heated and melted to produce a thin-walled sample for observation; or a method in which the resin component is removed by a burning method using an electric furnace and the remaining carbon fibers (A) are filtered and separated and then measured using an optical microscope.

[0048] The carbon fiber (A) forms a nonwoven fabric. This has the following advantages: compared with a fabric-shaped or one-direction oriented fiber substrate, a high porosity can be designed, thereby increasing the impregnation amount of the matrix resin (C) described later. In addition, by forming a nonwoven fabric with the carbon fiber (A), even if byproduct gases are generated during the reaction of the resin composition (B) described later, the byproduct gases can be easily discharged, and a hard carbon fiber substrate can be obtained. Figure 1 In the embodiment, carbon fibers (A) 1 are randomly dispersed as discontinuous fibers and are in the form of a nonwoven fabric having a network structure, thereby forming fine pores 3 between the fibers.

[0049] Generally speaking, the strength of a nonwoven fabric as a carbon fiber substrate is lower than that of a fabric or a fiber substrate oriented in one direction, and the risk of damage due to the inability to fully withstand the impregnation pressure during the melt impregnation of the matrix resin (C) increases. Therefore, in the present invention, carbon fibers with excellent mechanical properties are used. Carbon fibers (A) in the form of nonwoven fabrics can be manufactured by air-laid method, carding method, papermaking method, etc.

[0050] The mass ratio of the carbon fiber (A) in the carbon fiber substrate is preferably 90% or more and 97% or less. When the mass ratio is 90% or more, the strength of the carbon fiber substrate can be sufficient, and poor forming such as breakage can be effectively prevented during impregnation of the matrix resin (C). In addition, when the mass ratio is 97% or less, more preferably 96% or less, and further preferably 92% or less, the carbon fiber (A) can be prevented from agglomerating into a fiber bundle, thereby preventing insufficient dispersion of the carbon fiber (A) in the prepreg obtained from the carbon fiber substrate.

[0051] The resin composition (B) has the function of maintaining the non-woven fabric form by bonding the network structure of the carbon fibers (A) at their joints, or protecting the carbon fibers (A) from friction. Figure 1 In the figure on the right side of , the resin composition (B) 2 covers the surface of the carbon fiber (A), forming the carbon fiber (A) 4 covered with the resin composition (B). The carbon fiber substrate of the present invention bonded by the resin composition (B) can be prepreg while maintaining the network structure such as the fiber orientation or dispersion of the carbon fiber (A).

[0052] From the viewpoint of maintaining the network structure of the carbon fibers (A), the resin composition (B) preferably covers 50% to 100% of the surface area of ​​all the carbon fibers (A) constituting the carbon fiber substrate, more preferably 80% to 100%, and even more preferably 100%. In order to achieve the above state, it is preferred to go through a process of making the carbon fibers (A) into an aggregate such as a nonwoven fabric and impregnating it in the resin composition (B).

[0053] As described in Examples below, the coverage of the resin composition (B) can be determined using the following formula from the surface oxygen concentration (O / C) obtained by X-ray photoelectron spectroscopy.

[0054] (Coverage rate of resin composition (B)) = {(O / C of carbon fiber (A)) - (O / C of carbon fiber substrate)} / {(O / C of carbon fiber (A)) - (O / C of resin composition (B))} × 100 (%).

[0055] The porosity of the carbon fiber substrate of the present invention is preferably 50% to 99%. The porosity of the carbon fiber substrate is more preferably 80% to 99%, and further preferably 90% to 99%. By setting the porosity to the above range, a large impregnation amount of the matrix resin (C) can be designed. In addition, the carbon fiber substrate of the present invention, which has excellent mechanical properties at high temperatures despite its high porosity, can prevent poor forming such as breakage of the carbon fiber substrate during the melt impregnation process of the matrix resin (C). The porosity of the carbon fiber substrate is the volume ratio of the pores in the carbon fiber substrate, which can be calculated by the following formula.

[0056] (Porosity of carbon fiber substrate) = {(Thickness of carbon fiber substrate [m]) - (Weight per unit area of ​​carbon fiber substrate [g / m 2 ]) / (density of the constituent components of the carbon fiber substrate [g / m 3 ])} / (thickness of carbon fiber substrate [m])×100[%].

[0057] The tensile strength of the carbon fiber substrate of the present invention after heat treatment at 300°C for 5 minutes is more than 110% of that before the heating. The tensile strength after the heat treatment is preferably more than 200% and less than 600% relative to the tensile strength before the heating, and more preferably more than 300% and less than 500%. As described later, the carbon fiber substrate of the present invention can be processed into a prepreg by melt impregnation of a matrix resin (C). In order to composite with the matrix resin (C), the heated and molten matrix resin (C) is impregnated into the pores of the carbon fiber substrate at high temperature and high pressure, but in the impregnation process, defects such as damage to the carbon fiber substrate sometimes occur. On the other hand, if a hard carbon fiber substrate is used before the impregnation process, elastic rebound or breakage sometimes occurs when following the shape of a mold, etc. Therefore, by setting the following characteristics, that is, the material is soft at the beginning of the impregnation process and has the shape-forming property of following the mold, etc., and at the same time, hardens in a manner that does not cause damage even under pressure during the impregnation process, even in the high-temperature and high-pressure impregnation process of the matrix resin (C), it is possible to prevent the occurrence of poor forming such as damage. The change in tensile strength before and after the heat treatment is measured for a certain direction of the carbon fiber substrate, and the tensile strength (Ta) measured at room temperature after heating at 300°C for 5 minutes and the tensile strength (Tao) of the carbon fiber substrate at room temperature that has not been subjected to the heat treatment in the same direction are respectively measured, and are obtained by the following formula.

[0058] The tensile strength after the heat treatment relative to the tensile strength before the heating (%) = (Ta / Tao)×100.

[0059] In addition, the tensile strength [N / cm] of the carbon fiber substrate in this specification is set to the following value: a test piece with a width of 50 mm and a length of 150 mm is cut out from the carbon fiber substrate, and a portion with a length of 50 mm is loaded at each end, and the remaining central portion with a length of 50 mm is subjected to a tensile test at room temperature at a test speed of 3 m / min, and the value is obtained by dividing the maximum point load obtained by the width of the test piece.

[0060] The carbon fiber substrate of the present invention is preferably excellent in isotropy during the impregnation of the matrix resin, that is, the strength of the carbon fiber substrate in a certain direction and the direction orthogonal thereto is close. In the case of large anisotropy, the risk of concentrated breakage in the direction of weak tensile strength increases when the matrix resin (C) is impregnated. As an indicator of such isotropy, it is preferred that the tensile strength ratio (Ta / Tb) after heat treatment is 0.6 to 1.7, and the tensile strength ratio (Ta / Tb) after heat treatment is obtained by dividing the Ta by the tensile strength (Tb) measured at room temperature after heat treatment at 300°C for 5 minutes in the orthogonal direction of the test direction. The tensile strength ratio (Ta / Tb) after heat treatment is more preferably 0.8 to 1.3, and further preferably 0.9 to 1.1. In addition, the absolute values ​​of Ta and Tb are preferably 25 N / cm or more and 100 N / cm or less, and more preferably 25 N / cm or more and 45 N / cm or less. By setting it as the said range, even when melt-impregnating a matrix resin (C) and impregnating it, a strong carbon fiber base material which does not generate|occur|produce damage can be obtained.

[0061] In addition, from the viewpoint of preventing breakage in the shaping process of following the mold, the carbon fiber substrate of the present invention is preferably excellent in isotropy before impregnation with the matrix resin. As the index, the tensile strength ratio (Tao / Tbo) before the heat treatment is preferably 0.6 to 1.7, and the tensile strength ratio (Tao / Tbo) before the heat treatment is obtained by dividing the tensile strength before the heat treatment, i.e., the Tao, by the tensile strength (Tbo) measured at room temperature in the orthogonal direction of the test direction. The tensile strength ratio (Tao / Tbo) before the heat treatment is more preferably 0.8 to 1.3, and further preferably 0.8 to 1.1. The absolute values ​​of Tao and Tbo are preferably 8 N / cm or more and 25 N / cm or less, and more preferably 8 N / cm or more and 15 N / cm or less. By setting it to the range, a carbon fiber substrate that is soft and has high mold followability is obtained.

[0062] In the present invention, the resin composition (B) is preferably a resin composition that undergoes a dehydration condensation reaction with a thermal mass reduction rate of 5% to 50% by mass represented by the following formula (1).

[0063] Thermal mass reduction rate (mass %) = [(W1-W2) / W1] × 100 (1)

[0064] Here, W1 is the sample mass (mg) after the temperature was raised from room temperature to 100°C at 10°C / min and then isothermally maintained for 30 minutes, and W2 is the sample mass (mg) when the temperature was further raised at 10°C / min to 250°C.

[0065] The resin composition (B) has the effect of hardening the carbon fiber substrate by a dehydration condensation reaction accompanied by heating. Moreover, by making the carbon fiber (A) into a non-woven fabric form, the byproduct gas generated by the dehydration condensation reaction of the resin composition (B) can be easily discharged. By setting the thermal mass reduction rate of the resin composition (B) to the range, in the impregnation of the matrix resin (C) into the carbon fiber substrate, the hardening of the resin composition (B) and the exhaust of the byproduct gas can be achieved in a balanced manner. The analysis of the mass of the gas generated during heating and its components can be performed by a thermogravimetric / mass spectrometer (Thermogravimetry-Mass Spectrometer, TG-MS). The thermal mass reduction rate of the dehydration condensation reaction of the resin composition (B) is more preferably 5% by mass to 30% by mass, and further preferably 5% by mass to 20% by mass.

[0066] When the resin composition (B) undergoes a dehydration condensation reaction, the byproduct gas generated contains water, and the byproduct gas is preferably 5% or more of water, more preferably 50% or more, and further preferably 100%. When a large amount of water is contained in the byproduct gas, it is possible to prevent overheating caused by pressurization during impregnation of the matrix resin (C) or to improve the releasability from the mold.

[0067] From the viewpoint of heat resistance of the obtained reaction product, the dehydration condensation reaction of the resin composition (B) as described above is more specifically preferably an imidization reaction, an oxazolization reaction or an imidization reaction. In the case of a thermal decomposition reaction such as oxidation or free radical cleavage accompanied by mass loss, the heat resistance or mechanical strength of the resin composition (B) is reduced, which may cause a molding defect such as damage to the carbon fiber substrate.

[0068] From this viewpoint, the resin composition (B) preferably comprises at least one selected from polyamic acid, polyamic acid salt, polyamic acid ester, polyhydroxyamide and polyaminoamide. Polyamic acid, polyamic acid salt and polyamic acid ester are precursors of polyimide resins by imidization reaction, polyhydroxyamide is a precursor of polybenzoxazole resin by oxazolidation reaction, and polyaminoamide is a precursor of polybenzimidazole resin by imidization reaction.

[0069] Polyamic acid can be synthesized by reacting tetracarboxylic dianhydride with an equimolar diamine compound. As a specific synthesis method, a method in which a diamine compound is dissolved in a solvent such as N-methyl-2-pyrrolidone (NMP), and tetracarboxylic dianhydride is added while stirring at room temperature, etc. can be cited. In the method, the carboxylic anhydride as the functional group of tetracarboxylic dianhydride and the amino group as the functional group of the diamine compound are subjected to an equimolar, i.e., 1 to 1, ring-opening addition polymerization reaction is performed, thereby high molecular weight, and a carboxyl group derived from carboxylic anhydride is generated as a byproduct. Polyamic acid salt is a salt obtained by neutralizing the byproduct carboxyl group using an alkaline compound. As the alkaline compound used for neutralization here, ammonia, monoalkylamine, dialkylamine, trialkylamine, tetraalkylammonium hydroxide, etc. can be cited.

[0070] Polyamic acid ester can be synthesized by reacting the by-produced carboxyl group with an alcohol in a polyamic acid to esterify the alcohol. Examples of the alcohol used here include methanol, ethanol, 1-propanol, and 2-propanol. Esterification is preferred because it can reduce the hydrolysis of the polyamic acid.

[0071] The polyamic acid, the polyamic acid salt, and the polyamic acid ester are cyclized by the imidization reaction in the molecule caused by heating, and are changed into polyimide while generating byproduct gas. The resin composition (B) may be a mixture of the polyamic acid, the polyamic acid salt, and the polyamic acid ester.

[0072] The resin composition (B) is preferably a polyamic acid salt from the viewpoint of having high water solubility and being usable as an aqueous solution with relatively low equipment load.

[0073] Examples of the tetracarboxylic dianhydride include 3,3',4,4'-biphenyltetracarboxylic dianhydride <s-BPDA (3,3',4,4'-biphenyl tetracarboxylic dianhydride)>, 2,3,3',4'-biphenyltetracarboxylic dianhydride <a-BPDA (2,3,3',4'-biphenyl tetracarboxylic dianhydride)>, 2,2',3,3'-biphenyltetracarboxylic dianhydride <i-BPDA (2,2',3,3'-biphenyl tetracarboxylic dianhydride)>, pyromellitic dianhydride <PMDA (pyromellitic anhydride)>, 3,3',4,4'-benzophenonetetracarboxylic dianhydride <BTDA (3,3',4,4'-benzophenone tetracarboxylic dianhydride)>, and 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride <BTDA (3,3',4,4'-dibenzophenone tetracarboxylic dianhydride). dianhydride)>, 4,4'-(4,4'-isopropylidene diphenyloxy)bis(phthalic anhydride), 4,4'-oxydiphthalic anhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride<NTDA(1,4,5,8-naphthalenetetracarboxylic dianhydride)>, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride<6FDA(2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride)>, etc. Among these, 4,4′-(4,4′-isopropylidenediphenoxy)bis(phthalic anhydride) is preferred from the viewpoint of the compatibility of the melt processability of the obtained polyamic acid and the heat resistance of the carbon fiber substrate and the adhesion to the matrix resin (C).

[0074] Examples of the diamine compound include phenylenediamines such as p-phenylenediamine <PPD (p-phenylenediamine)> and m-phenylenediamine <MPD (m-phenylenediamine)>; diaminobenzoic acids such as 3,5-diaminobenzoic acid; diaminodiphenyl ethers such as 4,4'-diaminodiphenyl ether <ODA (4,4'-diaminodiphenyl ether)>, 3,4'-diaminodiphenyl ether, and 3,3'-diaminodiphenyl ether; diaminodiphenylmethanes such as 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 3,3'-dichloro-4,4'-diaminodiphenylmethane, and 3,3'-dimethyl-4,4'-diaminodiphenylmethane; and diaminobenzophenones such as 4,4'-diaminobenzophenone. Among these, from the viewpoint of the coating property of the obtained polyamic acid and the balance between the heat resistance and the coating property on the carbon fiber (A), phenylenediamines are preferred, and meta-phenylenediamine is more preferred.

[0075] Polyhydroxyamide is a precursor of polybenzoxazole resin, and is a prepolymer having an amide bond formed by polycondensation of an aromatic diamine diol having an amino group and a hydroxyl group on adjacent carbon atoms in an aromatic ring with a dicarboxylic acid derivative such as an aromatic dicarboxylic acid, an aromatic dicarboxylic acid ester, an aromatic dicarboxylic acid dihalogen compound, and a heterocyclic dicarboxylic acid. As a specific synthesis method, a method of mixing an aromatic diamine diol and a dicarboxylic acid derivative in a solvent such as NMP at a molar ratio of 1 to 1 and stirring at 120°C for 12 hours can be cited. Polyhydroxyamide is subjected to a heat treatment at 200°C to 400°C, and the adjacent hydroxyl groups are condensed with the amide bond to form an oxazole ring, thereby reacting to form a polybenzoxazole resin having an oxazole ring and an aromatic ring in the molecule. Examples of the aromatic diamine diol include 3,3'-dihydroxybenzidine, 3,3'-diamino-4,4'-dihydroxybiphenyl, 4,6-diaminoresorcinol, 2,5-diaminohydroquinone, 4,4'-diamino-3,3'-dihydroxydiphenyl sulfone, 3,3'-diamino-4,4'-dihydroxydiphenyl sulfone, 4,4'-diamino-3,3'-dihydroxydiphenyl ether, 3,3'-diamino-4,4'-dihydroxydiphenyl ether, 4,4'-diamino-3,3'-dihydroxydiphenylmethane, 3,3'-diamino-4,4'-dihydroxydiphenylmethane, 2,2-bis(3-amino-4-hydroxyphenyl)-propane, 2,2-bis(3-amino-4-hydroxyphenyl)-hexafluoropropane, and hydrochlorides thereof. Examples of the dicarboxylic acid derivative include isophthalic acid and the like.

[0076] Polyaminoamide is a precursor of polybenzimidazole resin, and is a prepolymer having an amide bond formed by polycondensation of a diamine component of an aromatic tetraamine compound with a dicarboxylic acid derivative such as an aromatic dicarboxylic acid, an aromatic dicarboxylic acid ester, an aromatic dicarboxylic acid dihalide, or a heterocyclic dicarboxylic acid. As a specific synthesis method, there can be cited a method in which an aromatic tetraamine compound and a dicarboxylic acid derivative are mixed in a solvent such as NMP at a molar ratio of 1:1, and stirred at 120°C for 12 hours. Polyaminoamide is subjected to a heat treatment at 200°C to 400°C, and adjacent amino groups are condensed with amide bonds to form an imidazole ring, thereby reacting to form a polybenzimidazole resin having an imidazole ring and an aromatic ring in the molecule. Aromatic tetraamine compounds include 3,3'-diaminobenzidine, 1,2,4,5-tetra-aminobenzene, 2,3,5,6-tetra-aminopyridine, 3,3',4,4'-tetra-aminodiphenyl sulfone, 3,3',4,4'-tetra-aminodiphenyl ether, 3,3',3,4'-tetra-aminodiphenylmethane, 3,3',4,4'-tetra-aminodiphenyldimethylmethane and their hydrochlorides. Dicarboxylic acid derivatives include isophthalic acid and the like. The polybenzimidazole resin obtained by imidazoleization of polyaminoamide has a glass transition temperature of 400° C. or more, and is preferred in terms of excellent heat resistance.

[0077] The resin composition (B) preferably comprises at least one selected from polyamic acid, polyamic acid salt, polyamic acid ester, polyhydroxyamide and polyaminoamide and comprises 50% by mass or more based on the total amount of these, more preferably comprising 80% by mass or more. It is further preferred that the resin composition (B) is only composed of at least one selected from polyamic acid, polyamic acid salt, polyamic acid ester, polyhydroxyamide and polyaminoamide. By setting the range, the resin composition (B) is in close contact with the carbon fiber (A), and a carbon fiber substrate with excellent heat resistance or mechanical strength can be obtained.

[0078] The resin composition (B) may contain other additives as appropriate according to the application, within the range not impairing the purpose of the present invention, for example, flame retardants, conductivity imparting agents, antioxidants, antibacterial agents, insect repellents, mold release agents, antistatic agents, plasticizers, lubricants, colorants, pigments, dyes, foaming agents, etc.

[0079] In the carbon fiber substrate of the present invention, the resin composition (B) is preferably 0.5 to 30 parts by mass relative to 100 parts by mass of carbon fiber (A). By having a resin composition (B) of 0.5 parts by mass or more, more preferably 1 part by mass or more, further preferably 3 parts by mass or more, further preferably 5 parts by mass or more, further preferably 8 parts by mass or more relative to 100 parts by mass of carbon fiber (A), the carbon fiber substrate has excellent handling properties and is not easily damaged during transportation. By having a resin composition (B) of 30 parts by mass or less, more preferably 15 parts by mass or less, further preferably 10 parts by mass or less relative to 100 parts by mass of carbon fiber (A), pores can be fully formed and impregnation of the matrix resin (C) can be easily performed.

[0080] The resin composition (B) preferably covers 50% or more of the surface area of ​​the carbon fibers (A). By making the coverage 50% or more, more preferably 80% or more, and even more preferably 100%, a firmly bonded interface between the carbon fibers (A) and the matrix resin (C) can be effectively formed in the prepreg of the present invention described later.

[0081] In order to form the coated state, it is preferred that the step of producing the carbon fiber base material include a step of impregnating the nonwoven fabric containing the carbon fibers (A) with the resin composition (B).

[0082] As described in Examples below, the coverage of the resin composition (B) can be determined using the following formula from the surface oxygen concentration (O / C) obtained by X-ray photoelectron spectroscopy.

[0083] (Coverage rate of resin composition (B)) (%) = {(O / C of carbon fiber (A)) - (O / C of carbon fiber substrate)} / {(O / C of carbon fiber (A)) - (O / C of resin composition (B))}×100.

[0084] By using the carbon fiber substrate of the present invention, poor forming such as breakage can be prevented during impregnation of the matrix resin (C), and a prepreg having an excellent expansion coefficient can be obtained. In particular, in the carbon fiber substrate of the present invention, even a highly heat-resistant matrix resin (C) that requires an impregnation process using high temperature and high pressure can be impregnated while poor forming such as breakage can be prevented. By the above effect, a porous structure having excellent heat resistance and being lightweight can be easily obtained by using a highly heat-resistant matrix resin (C).

[0085] [Prepreg]

[0086] The carbon fiber substrate of the present invention is suitable as a substrate of a prepreg. That is, the first embodiment of the prepreg of the present invention is obtained by impregnating a substrate derived from the carbon fiber substrate of the present invention with a matrix resin (C).

[0087] In addition, a second embodiment of the prepreg of the present invention is obtained by impregnating a base material including carbon fibers (A) and an adhesive resin composition (D) with a matrix resin (C).

[0088] The details of the carbon fibers (A) in the second embodiment are the same as those in the first embodiment, that is, the details of the carbon fibers (A) in the carbon fiber base material of the present invention.

[0089] The same also applies to the details of the matrix resin (C) in the first embodiment and the matrix resin (C) in the second embodiment.

[0090] The adhesive resin composition (D) in the second form is preferably derived from the resin composition described as the resin composition (B). The adhesive resin composition (B) or the adhesive resin composition derived from the resin composition (B) in the first form and the adhesive resin composition (D) in the second form are also combined and referred to as "adhesive resin composition". Hereinafter, unless the difference between the first form and the second form is particularly described, the two are assumed to be the same.

[0091] exist Figure 2 In the substrate including carbon fiber (A) 1 and the adhesive resin composition 2, fine pores are formed inside, and a prepreg is formed by impregnating the pores with a matrix resin (C) 5. In the prepreg, the carbon fiber (A) 1 is randomly dispersed and exists in the form of a non-woven fabric having a mesh structure, and the fine spaces between the fibers are filled with the matrix resin (C) 5. Moreover, the adhesive resin composition 2 exists at the interface between the carbon fiber (A) 1 and the matrix resin (C) 5.

[0092] The mass ratio of the carbon fiber (A) in the prepreg of the present invention is preferably 1% to 50%, more preferably 5% to 40%, and even more preferably 10% to 30%. If it is less than the above range, the reinforcing effect of the carbon fiber substrate on the prepreg may be insufficient. If it is greater than the above range, the carbon fiber substrate may be damaged during impregnation with the matrix resin (C).

[0093] As the resin contained in the adhesive resin composition, phenolic resin, urea-formaldehyde resin, melamine resin, polyimide resin, polybenzoxazole resin, polybenzimidazole resin, bismaleimide resin, benzoxazine resin, cyanate ester resin, etc. can be listed, and copolymers, modified substances, and resins blended with two or more of these can also be used. Among these, from the perspective of heat resistance, polyimide resin, polybenzoxazole resin and polybenzimidazole resin are preferably used. Furthermore, from the perspective of processability of carbon fiber substrates, polyimide resins are more preferably used, and in polyimide resins, polyetherimide resins having ether groups and imide groups are particularly preferably used.

[0094] In addition, the adhesive resin composition is preferably a composition comprising the following polymer or its derivative, that is, the polymer has at least one structure selected from an etherimide skeleton, a benzoxazole skeleton, a benzimidazole skeleton, a benzoxazine skeleton and a cyanate skeleton. By including the compound, the adhesive resin composition has excellent heat resistance, and then excellent adhesion to carbon fiber (A) or matrix resin (C). The etherimide skeleton means having an ether group and an imide group respectively. As a polymer or a derivative thereof having the skeleton, a polyetherimide resin can be cited. The benzoxazole skeleton is a structure in which an aromatic ring and an oxazole ring are bonded in a manner that shares one side. As a polymer or a derivative thereof having the skeleton, a polybenzoxazole resin can be cited. The benzimidazole skeleton is a structure in which an aromatic ring and an imidazole ring are bonded in a manner that shares one side. As a polymer or a derivative thereof having the skeleton, a polybenzimidazole resin can be cited. As a polymer or a derivative thereof having a benzoxazine skeleton, a benzoxazine resin can be cited. As a polymer or a derivative thereof having a cyanate skeleton, a cyanate resin can be cited. Furthermore, from the viewpoint of heat resistance and processability with respect to a carbon fiber substrate, the adhesive resin composition more preferably contains a polymer having an etherimide skeleton or a derivative thereof.

[0095] The glass transition temperature of the adhesive resin composition in the first form is preferably 120°C or more and 450°C or less. In addition, the glass transition temperature of the adhesive resin composition (D) in the second form is 120°C or more and 450°C or less. The glass transition temperature of the adhesive resin composition is more preferably 200°C or more and less than 400°C, and more preferably 200°C or more and 350°C or less. The adhesive resin composition has the function of maintaining the non-woven form by bonding the mesh structure of the carbon fiber (A) at its joints during the impregnation of the matrix resin (C), and exists at the interface between the carbon fiber (A) and the matrix resin (C) inside the obtained prepreg. By having the glass transition temperature of the adhesive resin composition within the range, the form of the carbon fiber substrate is maintained as a solid at the initial stage of the impregnation of the matrix resin (C), and then gradually softened, thereby dissolving with the matrix resin (C) in a molten state, and an interface in which the carbon fiber (A) and the matrix resin (C) are firmly and closely bonded can be formed.

[0096] The adhesive resin composition preferably has a thermal mass reduction rate of 5% by mass or less at 400°C. The adhesive resin composition has the function of maintaining the non-woven form by bonding the mesh structure of the carbon fiber (A) at its joints during the impregnation of the matrix resin (C), and is present at the interface between the carbon fiber (A) and the matrix resin (C) inside the obtained prepreg. The adhesive resin composition has a thermal mass reduction rate of 5% by mass or less at 400°C, preferably 0% by mass or more and 3% by mass or less, and has high heat resistance and is not easy to thermally decompose, which can prevent the decomposition gas from causing the interface between the carbon fiber (A) and the adhesive resin composition to peel off and reduce the bonding effect. The thermal mass reduction rate can be calculated by the following formula.

[0097] Thermal mass reduction rate (mass %) = [(M1-M2) / M1] × 100

[0098] Here, M1 is the mass (mg) of the sample after isothermally maintaining at 30°C for 10 minutes, and M2 is the mass (mg) of the sample when the temperature is subsequently increased at 10°C / min to 400°C.

[0099] The adhesive resin composition preferably covers 50% or more of the surface area of ​​the coated carbon fibers (A). When the coverage is 50% or more, more preferably 80% or more, and even more preferably 100%, a firmly bonded interface between the carbon fibers (A) and the matrix resin (C) can be effectively formed in the prepreg of the present invention described later.

[0100] In order to form the coated state, it is preferred that the step of producing the carbon fiber base material include a step of impregnating the nonwoven fabric containing the carbon fibers (A) with the resin composition (B).

[0101] As described in Examples below, the coverage of the binder resin composition can be determined using the following formula from the surface oxygen concentration (O / C) obtained by X-ray photoelectron spectroscopy.

[0102] (Coverage of adhesive resin composition) (%) = {(O / C of carbon fiber (A)) - (O / C of carbon fiber substrate)} / {(O / C of carbon fiber (A)) - (O / C of adhesive resin composition)}×100.

[0103] Generally, in prepregs, the processing temperature required for the binder resin having a high glass transition temperature is high, and therefore it is difficult to coat the surface of the reinforcing fiber with a high coverage rate. In the present invention, as a means to solve the above situation, the following method can be cited: the resin composition (B) is applied to the surface of the carbon fiber (A) as a precursor of the binder resin composition (D) and heated to react, thereby preparing the binder resin composition (D).

[0104] In addition, when using a polyimide resin or a polybenzoxazole resin or a polybenzimidazole resin as the adhesive resin composition (D), from the viewpoint of heat resistance and processability, the following method can also be preferably used: a resin composition (B) serving as a precursor thereof is applied to the carbon fiber (A), and then the carbon fiber (A) is subjected to a dehydration condensation reaction to thereby prepare the adhesive resin composition (D).

[0105] The matrix resin (C) is preferably a thermoplastic resin. Examples of the thermoplastic resin include polyester resins such as polyethylene terephthalate and polybutylene terephthalate, polyolefins such as polyethylene, polypropylene, polybutene, and modified polypropylene, polyamides such as polyoxymethylene, polyamide 6, and polyamide 66, polycarbonate, polymethyl methacrylate, polyvinyl chloride, polyarylene sulfide such as polyphenylene sulfide, polyphenylene ether, modified polyphenylene ether, polysulfone, modified polysulfone, polyethersulfone, polyketone, polyetherketone, polyetheretherketone, polyetherketoneketone, polyarylene etherketone, polyarylate, polyethernitrile, and phenoxy resins.

[0106] Furthermore, these thermoplastic resins may be copolymers or modified products, and / or resins obtained by blending two or more types of them.

[0107] Among these, in terms of the balance between moldability and heat resistance, the matrix resin (C) preferably contains at least one selected from the group consisting of polyetherketone, polyetheretherketone, polyetherketoneketone and polycarbonate as a main component, and more preferably contains at least one selected from the group consisting of polyetherketone, polyetheretherketone and polyetherketoneketone as a main component, and more preferably contains polyetherketoneketone as a main component. Here, the main component means that it accounts for 50% by mass or more of the constituent components, preferably 80% by mass or more and 100% by mass or less, and more preferably 100% by mass.

[0108] The melting point of the thermoplastic resin used as the matrix resin (C) in the first form is preferably 250°C or more and 400°C or less. The melting point of the thermoplastic resin used as the matrix resin (C) in the second form is 250°C or more and 400°C or less. By making the melting point of the thermoplastic resin 250°C or more, more preferably 280°C or more, and more preferably 300°C or more, the prepreg or the porous structure described later can be effectively made to have excellent heat resistance. In addition, by making the melting point of the thermoplastic resin 400°C or less, more preferably less than 400°C, more preferably 360°C or less, and more preferably 350°C or less, the prepreg can be effectively made to have excellent molding processability.

[0109] The glass transition temperature of the thermoplastic resin used as the matrix resin (C) is preferably 80°C or more and 250°C or less, more preferably 100°C or more and 230°C or less, and further preferably 140°C or more and 180°C or less. When the glass transition temperature is 80°C or more, preferably 100°C or more, more preferably 120°C or more, and further preferably 140°C or more, the heat resistance of the prepreg or the porous structure described later can be effectively improved. In addition, when the glass transition temperature is 250°C or less, preferably 230°C or less, more preferably 200°C or less, and further preferably 180°C or less, the compatibility with the adhesive resin composition is excellent, and the tensile strength of the obtained prepreg can be effectively improved.

[0110] The matrix resin (C) is also preferably a resin composition that contains other fillers or additives as appropriate according to the application within the range that does not impair the purpose of the present invention. Examples thereof include inorganic fillers, flame retardants, conductivity imparting agents, crystal nucleating agents, ultraviolet absorbers, antioxidants, vibration damping agents, antibacterial agents, insect repellents, deodorants, anti-coloring agents, heat stabilizers, mold release agents, antistatic agents, plasticizers, lubricants, colorants, pigments, dyes, foaming agents, foaming agents, coupling agents, etc.

[0111] The amount of the matrix resin (C) in the prepreg is preferably 5 to 1000 parts by mass relative to 100 parts by mass of carbon fiber (A), more preferably 50 to 700 parts by mass, and further preferably 100 to 500 parts by mass. If it is less than the range, the mechanical properties of the prepreg or the porous structure formed therefrom are sometimes insufficient. If it is greater than the range, the amount of the matrix resin (C) relative to the volume of the pores is large, and sometimes the carbon fiber substrate is damaged when the matrix resin (C) is melt-impregnated.

[0112] The minimum value of the tensile strength of the prepreg of the first form is preferably 100 MPa or more. The minimum value of the tensile strength of the prepreg of the second form is 100 MPa or more. The minimum value of the tensile strength of the prepreg is preferably 200 MPa or more, more preferably 240 MPa or more, and further preferably 260 MPa or more and 400 MPa or less.

[0113] In general, the tensile strength of the prepreg is strongly affected by the fiber orientation of the enclosed carbon fiber substrate. Even within the same plane of the prepreg, the tensile strength in the direction where the fiber orientation is biased and close to parallel carbon fibers is higher, and on the contrary, the tensile strength in the direction orthogonal to it is lower. Therefore, there is a situation where the tensile strength in a certain direction of the prepreg is high, but the tensile strength in the direction orthogonal to it is low. From this point of view, in order to obtain a prepreg with high mechanical properties in the in-plane direction, it is ideal to design the tensile strength based on the minimum value.

[0114] The minimum value of the tensile strength can be measured using a test piece cut out in four directions, 45°, 90°, and -45°, with any one direction in the in-plane direction of the prepreg as the reference 0°. The number of measurements for each direction is n=5, and the minimum value among all the measured values ​​(n=20) is set as the minimum value of the tensile strength.

[0115] The prepreg of the present invention preferably has a maximum value of tensile strength of 260 MPa or more, more preferably 260 MPa or more and 400 MPa or less.

[0116] Generally speaking, the more carbon fibers that are closer to parallel to the stretching direction in the fiber orientation of the enclosed carbon fiber substrate, the higher the tensile strength of the prepreg. By setting the maximum value of the tensile strength to the above range and designing it to the same degree as the minimum value of the tensile strength, a prepreg with more isotropic mechanical properties can be formed.

[0117] The maximum value of the tensile strength can be measured using a test piece cut out in four directions, 45°, 90°, and -45°, with any one direction in the in-plane direction of the prepreg as the reference 0°. The number of measurements for each direction is n=5, and the maximum value among all the measured values ​​(n=20) is set as the maximum value of the tensile strength.

[0118] The prepreg of the present invention preferably has a ratio of the maximum value of the tensile strength to the minimum value of the tensile strength of 1 to 3, more preferably 1 to 1.5, further preferably 1 to 1.2, and particularly preferably 1 to 1.1. By setting it within the above range, the mechanical properties in any direction in the in-plane direction of the prepreg are the same, and a prepreg with excellent mechanical properties can be made isotropically. The above value can be obtained by dividing the maximum value of the tensile strength of the prepreg by the minimum value of the tensile strength of the prepreg.

[0119] In addition, the prepreg of the present invention preferably has an average tensile strength of 100 MPa or more, more preferably 200 MPa or more, and further preferably 240 MPa or more, particularly preferably 260 MPa or more and 400 MPa or less. By setting the range, a prepreg having high mechanical properties isotropically can be obtained. Such average tensile strength can be measured using a test piece obtained by setting one direction in the in-plane direction of the prepreg as 0° as a reference and then cutting out a test piece in a total of four directions of 45°, 90°, and -45°. For each direction, the number of measurements is set to n=5, and the average value of all measured values ​​(n=20) is set to the average tensile strength.

[0120] In addition, from the perspective of obtaining a prepreg with isotropic mechanical properties, it is also preferred that the deviation of the tensile strength in the plane be set to 20% or less, and the deviation is more preferably 10% or less, and further preferably 5% or less. The deviation of the tensile strength is the coefficient of variation (CV) calculated by the following formula based on the average value and standard deviation of all measured values ​​(n = 20), and more specifically, it can be measured by the method described in the examples described later.

[0121] Deviation (%) of tensile strength=[(standard deviation of tensile strength) / (average value of tensile strength)]×100.

[0122] The prepreg of the present invention preferably has a thickness of 0.1 mm or more and 5 mm or less at 400°C, more preferably 0.1 mm or more and 2 mm or less, and further preferably 1 mm or more and 2 mm or less. The thickness at 400°C corresponds to the thickness of the prepreg after the prepreg is expanded by rebounding (spring back) through the enclosed carbon fiber substrate. The prepreg can be used for forming purposes corresponding to the desired thickness in a single layer or in multiple layers. By controlling the thickness of the prepreg when it is expanded within the range, it can be formed into a void body of various thicknesses, so it is preferred.

[0123] The thickness at 400° C. can be determined as an average value of the thickness of the prepreg heated on a hot plate at 400° C. for 5 minutes by non-contact measurement using a laser displacement meter.

[0124] The first form of the prepreg preferably has a thickness deviation of 10% or less at 400°C. The second form of the prepreg preferably has a thickness deviation of 10% or less at 400°C. The thickness deviation at 400°C is preferably 8% or less, more preferably 0% or more and 5% or less. When the prepreg of the present invention is heated to 400°C, the matrix resin (C) rebounds due to melting and expands in the void body. The expansion originates from the carbon fiber substrate enclosed in the prepreg, and the deviation of the thickness after expansion becomes an indicator of isotropy in the out-of-plane direction. That is, when the thickness of a certain part after expansion is large relative to the surrounding area, it can be said that the fiber orientation or fiber concentration of the enclosed carbon fiber substrate is different. In the case of a prepreg that is isotropic in the out-of-plane direction, the thickness after expansion is equal as a whole, resulting in a smaller thickness deviation.

[0125] In addition, the fiber-reinforced resin molded body or the void body described later is an integrated molded product formed by bonding the prepregs constituting the preform between layers. By making the prepregs expandable and having a small thickness deviation when expanded, the formation of gaps between layers is avoided, and a fiber-reinforced resin molded body or the void body with good adhesion can be obtained.

[0126] The thickness deviation at 400°C is the following CV value (coefficient of variation), that is, the thickness of the prepreg heated on a hot plate at 400°C for 5 minutes is measured non-contactly using a laser displacement meter. The CV value (coefficient of variation) can be calculated by the following formula based on the average value and standard deviation of the thickness. More specifically, it can be measured by the method described in the examples described later.

[0127] Deviation (%) of thickness at 400° C.=[(standard deviation of thickness at 400° C.) / (average value of thickness at 400° C.)]×100.

[0128] The prepreg of the present invention is heated to 400°C, and the matrix resin (C) having a melting point of 250°C or more and 400°C or less, preferably 280°C or more and 400°C or less, is melted to become an expanded state in which the rebound force formed by the carbon fiber substrate is released to the maximum extent. By setting it to such a state, the fiber orientation or the density of the carbon fiber substrate contained in the prepreg can be grasped. That is, the thickness of the state after expansion at 400°C becomes thinner with respect to the part where the fiber orientation of the carbon fiber (A) in the interior of the prepreg is biased and converged into a fiber bundle, or the part where the carbon fiber substrate is damaged and the concentration of the carbon fiber (A) becomes thinner. The distribution of such a part can be detected as a deviation of the thickness after expansion. The defects of such a carbon fiber substrate are easily generated during the impregnation of the matrix resin (C). As a method for confirming the defects after prepreg, the measurement of the deviation of the thickness at 400°C is effective.

[0129] In addition, defects in the carbon fiber substrate contained in the prepreg will affect the tensile strength of the prepreg. Therefore, for example, by making the thickness deviation at 400°C less than 10%, a prepreg with a high average tensile strength can be made, or a prepreg with isotropy, that is, a small ratio of the maximum value to the minimum value of the tensile strength and a high maximum value of the tensile strength can be made.

[0130] From the viewpoint of short impregnation distance and excellent productivity, the prepreg of the present invention is preferably manufactured by impregnating the matrix resin (C) in the out-of-plane direction. In the manufacturing method, first, the carbon fiber substrate repels the compression caused by the impregnation of the matrix resin (C). Under the repulsive force, the matrix resin (C) flows in the in-plane direction. When the resin flows, the force that stretches the carbon fiber substrate in the in-plane direction acts. When using an existing carbon fiber substrate, damage occurs due to the force in the in-plane direction, resulting in poor molding. By using the carbon fiber substrate of the present invention, such breakage can be prevented.

[0131] As a method for manufacturing the prepreg, a method that goes through the following steps can be cited: a heating impregnation step, in which the matrix resin (C) is plasticized by melting and impregnated into the pores of the carbon fiber substrate; and a cooling and solidification step, in which the impregnated matrix resin (C) is solidified. In the manufacturing method, as a method for compounding the matrix resin (C) with the carbon fiber substrate, a method of directly injecting the molten matrix resin (C) into the carbon fiber substrate can be cited; or a method of laminating a film-like, powder-like, or fibrous matrix resin (C) on the carbon fiber substrate, and then impregnating the matrix resin (C) by heating and melting. From the perspective of suppressing the uneven concentration of the prepreg or the bias of the fiber orientation and facilitating manufacturing, it is preferred to heat and pressurize the laminate of the film-like matrix resin (C) and the carbon fiber substrate.

[0132] The temperature in the heating impregnation step is preferably 250°C to 450°C, more preferably 280°C to 400°C, and further preferably 300°C to 400°C. The pressure in the heating impregnation step is preferably 0.5 MPa to 20 MPa, more preferably 5 MPa to 15 MPa. Even under the high temperature and high pressure conditions within the above range, the prepreg can be efficiently manufactured by using the carbon fiber substrate of the present invention.

[0133] The time in the heating and impregnation step is preferably 0.5 to 60 minutes, more preferably 5 to 30 minutes. The heating time in the above range is preferred because the carbon fiber substrate is hardened in parallel with the impregnation of the matrix resin (C), and strong adhesion can be achieved.

[0134] The temperature in the cooling and solidification process is preferably 20°C to 250°C, and more preferably 100°C to 200°C. The pressure in the cooling and solidification process is preferably 0.5MPa to 20MPa, and more preferably 5MPa to 15MPa. The time in the cooling and solidification process is preferably 0.5 minutes to 60 minutes, and more preferably 5 minutes to 30 minutes. By setting it in the above range, the prepreg can be manufactured efficiently.

[0135] As equipment for realizing the manufacturing method of the prepreg, a press molding machine or a double belt press machine can be preferably used. In the case of a batch method, the former is used, and an intermittent press system consisting of two or more machines for heating and cooling is arranged in parallel, so that productivity can be improved. In the case of a continuous method, the latter is used, and continuous processing can be easily performed, so continuous productivity is excellent.

[0136] The prepreg produced by the manufacturing method as exemplified above contains a carbon fiber substrate, which is in a state of accumulating repulsive force in the out-of-plane direction due to compression in the out-of-plane direction during impregnation with the matrix resin (C). Therefore, when the matrix resin (C) melts, the carbon fiber substrate releases the repulsive force, and a rebound phenomenon occurs in which the porosity is restored to its original state. That is, the prepreg has an out-of-plane expansion property, and can be formed into a porous structure.

[0137] The prepreg of the present invention preferably expands at an average expansion rate of 150% to 1,000% in the out-of-plane direction when the matrix resin (C) is melted, more preferably 200% to 800%, and still more preferably 450% to 700%. The above value is an expansion rate that can be calculated by (thickness of the porous structure after expansion [mm]) / (thickness of the prepreg before expansion [mm]) × 100 [%], and is the arithmetic mean value of 5 samples.

[0138] The prepreg of the present invention contains a carbon fiber substrate, which is in a state of accumulating repulsive force in the out-of-plane direction due to compression in the out-of-plane direction during impregnation with the matrix resin (C). Therefore, when the matrix resin (C) melts, the carbon fiber substrate releases the repulsive force and generates a rebound phenomenon to restore the original thickness. That is, this prepreg has an out-of-plane expansion property, and can be formed into a void body by sucking air during expansion.

[0139] [Porous structure]

[0140] The prepreg of the present invention can be formed into a porous structure by effectively utilizing its expansion property during heating. That is, the porous structure of the present invention is formed from the prepreg of the present invention.

[0141] exist Figure 3 In the embodiment, the carbon fiber substrate including carbon fiber (A) and the resin composition (B) covering the surface thereof expands in the out-of-plane direction due to its rebound force, and the pores generated by the volume expansion are generated as micropores inside the matrix resin (C). By setting the structure as described above, it is possible to achieve lightweight as a porous structure, and the reinforcement effect brought by the carbon fiber substrate can be exerted. In this way, by having a structure in which the pores in the porous structure are reinforced by the carbon fiber substrate, it is possible to simultaneously achieve lightweight brought by the increase in the amount of pores and the suppression of deformation of the pores, so that lightweight and mechanical properties can coexist at a high level.

[0142] The method for producing the porous structure preferably includes: a first step of melting and expanding the matrix resin (C); and a second step of curing the matrix resin (C).

[0143] The first step is a step of plasticizing the matrix resin (C) by melting it and selectively expanding it in an out-of-plane direction by utilizing the resilience of the carbon fiber base material.

[0144] In the first step, in order to melt and expand the matrix resin (C), the temperature at which the prepreg is heated is preferably 250°C to 450°C, and more preferably 300°C to 400°C. The pressure in the first step is preferably 0MPa to 5MPa, and more preferably 0.1MPa to 3MPa. The time spent in the first step is preferably 0.5 minutes to 60 minutes, and more preferably 5 minutes to 30 minutes. By setting the range, the prepreg is efficiently expanded, and a porous structure with excellent mechanical properties can be obtained.

[0145] The second step is a step of fixing the carbon fiber base material in a resilient state by curing the matrix resin (C) to form a porous structure.

[0146] The temperature in the second step is preferably 20°C to 250°C, more preferably 100°C to 200°C. The pressure in the second step is preferably 0MPa to 5MPa, more preferably 0.1MPa to 3MPa. The time in the second step is preferably 0.5 minutes to 60 minutes, more preferably 1 minute to 30 minutes. By setting the expansion ratio to the above range, a porous structure with excellent mechanical properties can be obtained.

[0147] In addition, in the first process or the second process, it is preferred to adjust the thickness of the formed product. As a method for thickness control, from the perspective of ease of manufacturing, it is preferred to use a method of constraining the thickness using a metal plate or the like, a method of directly controlling the thickness by adjusting the applied pressure, etc. As equipment for implementing the method, a press molding machine or a double-belt press machine can be preferably used. In the case of a batch method, the former is used, and an intermittent pressing system consisting of two or more machines for heating and cooling is arranged in parallel, so that productivity can be improved. In the case of a continuous method, the latter is used, and continuous processing can be easily performed, so continuous productivity is excellent.

[0148] In the present invention, the porous structure has micropores with an average pore diameter of 500 μm or less. The average pore diameter is preferably 200 μm or less, more preferably 10 μm or more and 150 μm or less, and further preferably 30 μm or more and 100 μm or less. If it is less than the above range, the lightweight effect of the porous structure brought about by the expansion is sometimes insufficient, and if it is greater than the above range, the mechanical properties of the porous structure are sometimes reduced. The average pore diameter here is as follows: Figure 4As shown in the schematic diagram of the surface of the porous structure shown in FIG. 1 , the diameter 8 of the largest circle inscribed in the pores in the observation image is measured at 50 randomly selected positions. The surface observation of the porous structure can be performed, for example, by a scanning electron microscope (SEM).

[0149] The density of the porous structure of the present invention is preferably 0.01 g / cm 3 Above and 0.8g / cm 3 Below, more preferably 0.1 g / cm 3 Above and 0.5g / cm 3 Below, more preferably 0.2 g / cm 3 Above and 0.3g / cm 3 If the density is less than the above range, the reinforcing effect of the carbon fiber substrate as a porous structure may be insufficient, and if it is greater than the above range, the lightweight effect as a porous structure may be insufficient. The density [g / cm 3 ] is the sample mass of the porous structure [g] divided by the volume [cm 3 ] and can be calculated as the arithmetic mean of the results measured in 5 randomly selected samples.

[0150] The porous structure of the present invention preferably has a flexural strength when heated to 140°C of 80% or more, more preferably 90% or more and 100% or less of the flexural strength at 30°C. This value can be calculated as "retention rate of flexural strength when heated to 140°C" by the following formula.

[0151] (Retention rate of flexural strength when heated to 140°C) = (flexural strength at 140°C [MPa]) / (flexural strength at 30°C [MPa]) × 100 [%]

[0152] The bending strength was measured by a three-point bending test in accordance with Japanese Industrial Standards (JIS) K 7171 (2016), and was set as the arithmetic mean of 5 samples at each level. A constant temperature bath was used for temperature control at each level, and the test was performed at 30°C and 140°C respectively.

[0153] If the retention rate of the bending strength when heated to 140° C. is within the above range, a porous structure having excellent heat resistance and usable for structural material applications even in a high temperature environment such as 100° C. can be obtained, which is preferred.

[0154] The prepreg of the present invention can be used as a single layer or as a preformed body including the prepreg as a lamination unit. Since the mechanical properties of the prepreg of the present invention are isotropic, there is no need to perform lamination such as quasi-isotropic lamination to compensate for the direction of low strength, and the lamination structure has the advantage of high freedom of design. Therefore, the labor or time in the lamination process can be reduced, thereby reducing the economic burden.

[0155] [Preform]

[0156] The preform of the present invention comprises the prepreg of the present invention as a lamination unit. The number of lamination sheets in the preform is preferably 2 or more and 50 or less, more preferably 2 or more and 10 or less.

[0157] The preform may be formed into a "fiber-reinforced resin molded body having voids" (hereinafter, sometimes referred to as a "void body") or a "fiber-reinforced resin molded body not containing voids".

[0158] [Fiber-reinforced resin molded body]

[0159] The void body which is one form of the fiber-reinforced resin molded body of the present invention is formed by heating and expanding the preform of the present invention, that is, by welding the multi-layered prepregs constituting the preform of the present invention in an expanded state.

[0160] As a method for producing the void body, there can be cited a method comprising a step (1-A) of melting the matrix resin (C) and a step (2-A) of curing the matrix resin (C) while controlling the thickness of the molded product. The prepreg of the present invention or the preformed body thereof as a laminate has an out-of-plane expansion property, so by molding while controlling the thickness of the molded product, it can be molded into a fiber-reinforced resin molded body having voids inside.

[0161] The step (1-A) is a step of plasticizing the matrix resin (C) by melting it and selectively expanding it in the out-of-plane direction by utilizing the resilience of the carbon fiber base material.

[0162] The temperature of step (1-A) is preferably 250°C to 450°C, more preferably 280°C to 450°C, and further preferably 300°C to 400°C. The pressure in step (1-A) is preferably 0MPa to 5MPa, more preferably 0.1MPa to 3MPa. The time in step (1-A) is preferably 0.5 minutes to 60 minutes, more preferably 5 minutes to 30 minutes. By making the conditions of step (1-A) within the range, the prepreg constituting the preform can be efficiently expanded, thereby firmly bonding the layers of the prepregs to each other.

[0163] Step (2-A) is a step of fixing the carbon fiber base material in a resilient state by curing the matrix resin (C) to form a void body.

[0164] The temperature in step (2-A) is preferably 20°C to 280°C, more preferably 20°C to 250°C, further preferably 20°C to 200°C, and further preferably 20°C to 100°C. The pressure in step (2-A) is preferably 0 MPa to 3 MPa, more preferably 0 MPa to 1 MPa. The time in step (2-A) is preferably 0.5 minutes to 60 minutes, more preferably 5 minutes to 30 minutes. By setting the conditions of step (2-A) within the range, the expansion rate is controlled, and a void body with excellent mechanical properties and lightness can be obtained.

[0165] In step (2-A), the thickness of the formed product is controlled. From the perspective of manufacturing simplicity, a method of controlling the thickness using a metal plate or the like, or a method of directly controlling the thickness by adjusting the applied pressure is preferred.

[0166] As equipment for realizing the method for manufacturing the void body, a press forming machine can be preferably used. By setting an intermittent press system consisting of two or more machines for heating in step (1-A) and cooling in step (2-A) in parallel, productivity can be improved.

[0167] The void body of the present invention is preferably produced by expanding the preform used in the forming at an average expansion rate of 150% to 1,000% in the out-of-plane direction, more preferably 200% to 800%, and even more preferably 300% to 400%. The value is the expansion rate that can be calculated by (thickness of the void body [mm]) / (thickness of the preform body [mm])×100[%], and is the arithmetic mean value of 5 samples. By setting it to the above range, a void body with an excellent balance between lightness and mechanical properties can be obtained.

[0168] The density of the voids in the present invention is preferably 0.01 g / cm 3 Above and 0.8g / cm 3 Below, more preferably 0.1 g / cm 3 Above and 0.5g / cm 3 Below, more preferably 0.3 g / cm 3 Above and 0.5g / cm 3 By setting the density in the above range, a porous body having an excellent balance between lightness and mechanical properties can be obtained. The density [g / cm 3 ] is the sample mass of the void [g] divided by the volume [cm 3] and is calculated as the arithmetic mean of the results measured in 5 randomly selected samples.

[0169] The void-free fiber-reinforced resin molded body, which is one form of the fiber-reinforced resin molded body of the present invention, is formed by heating and pressurizing the preform of the present invention, that is, by welding the multi-layered prepregs constituting the preform of the present invention in a non-expanded state.

[0170] As a method for producing the fiber-reinforced resin molded body without voids, there can be cited a method comprising a step (1-B) of melting the matrix resin (C), and a step (2-B) of curing the matrix resin (C) while suppressing the rebound force of the prepreg. The prepreg of the present invention or the preformed body as a laminate thereof has an out-of-plane expansion property, but by molding under high pressure to suppress the rebound force, it can be formed into a fiber-reinforced resin molded body in a non-expanded state.

[0171] The step (1-B) is a step of plasticizing the matrix resin (C) by melting.

[0172] The temperature of step (1-B) is preferably 250°C to 450°C, more preferably 280°C to 450°C, and further preferably 300°C to 400°C. The pressure in step (1-B) is preferably 0MPa to 5MPa, more preferably 0.1MPa to 3MPa. The time in step (1-B) is preferably 0.5 minutes to 60 minutes, more preferably 5 minutes to 30 minutes. By setting the conditions of step (1-B) within the range, the layers of the prepregs constituting the preform can be firmly bonded to each other.

[0173] The step (2-B) is a step of curing the matrix resin (C) while suppressing the resilient force of the prepregs, thereby producing a fiber-reinforced resin molded body in which the stacked prepregs are integrated in a non-expanded state.

[0174] The temperature in step (2-B) is preferably 20°C to 280°C, more preferably 20°C to 250°C, further preferably 20°C to 200°C, and further preferably 20°C to 100°C. The pressure in step (2-B) is preferably 3MPa to 10MPa, more preferably 5MPa to 10MPa. The time in step (2-B) is preferably 0.5 minutes to 60 minutes, more preferably 5 minutes to 30 minutes. By setting the conditions of step (2-B) within the range, the expansion rate is controlled, and a fiber-reinforced resin molded body with excellent mechanical properties can be obtained.

[0175] As equipment for realizing the manufacturing method of the fiber-reinforced resin molded body, a press molding machine can be preferably used. By setting an intermittent press system consisting of two or more machines for heating in step (1-B) and cooling in step (2-B) in parallel, productivity can be improved.

[0176] The fiber-reinforced resin molded body containing no voids is preferably set to an average expansion rate in the out-of-plane direction of 90% to 150% relative to the preform used in molding, more preferably 100% to 120%, and even more preferably 100% to 105%. The value is an expansion rate that can be calculated by (thickness of the fiber-reinforced resin molded body [mm]) / (thickness of the preform [mm])×100[%], and is the arithmetic mean value of 5 samples. By setting it to the above range, a fiber-reinforced resin molded body with excellent mechanical properties can be obtained.

[0177] The density of the fiber-reinforced resin molded body without voids is preferably 0.8 g / cm 3 Above and 2.0g / cm 3 Below, more preferably 1.2 g / cm 3 Above and 1.5g / cm 3 By setting the density in the above range, a fiber-reinforced resin molded body having excellent mechanical properties can be obtained. The density [g / cm 3 ] is the sample mass [g] of the fiber-reinforced resin molded body divided by the volume [cm 3 ] and is calculated as the arithmetic mean of the results measured in 5 randomly selected samples.

[0178] The fiber-reinforced resin molded body of the present invention has excellent molding processability, and therefore is also preferably molded into a corrugated shape or a honeycomb shape. Here, the so-called corrugated shape refers to a shape of a corrugated plate with multiple curved surfaces or continuous bends. The so-called honeycomb shape refers to a structure in which a corrugated fiber-reinforced resin molded body is used as a chamber wall and multiple chamber walls are joined at the curved surface or curved convex portion, and is an aggregate of multiple hollow columnar chambers divided by chamber walls. The shape of the bottom surface of the hollow columnar chamber is preferably a triangle, a quadrangle, a hexagon, etc., and from the viewpoint of mechanical properties, a hexagon is more preferred.

[0179] [Sandwich structure]

[0180] The sandwich structure of the present invention is formed by sandwiching the fiber-reinforced resin molded body of the present invention as a core material between a pair of skin materials and integrating them. The fiber-reinforced resin molded body of the present invention has excellent heat resistance, so when used as a core material, deformation can be suppressed even in the heating and pressing process for joining the skin materials, and a sandwich structure with excellent dimensional accuracy can be obtained. In addition, the sandwich structure of the present invention has an excellent balance between lightness and mechanical properties. As skin materials, there are no particular restrictions, and examples include: prepreg or fiber-reinforced resin molded body, metal plate, resin plate, etc.

[0181] [Aircraft components]

[0182] The prepreg of the present invention, the porous structure or fiber-reinforced resin molded body using the prepreg, and the sandwich structure can be preferably used in aircraft components such as aircraft, artificial satellites, urban air mobility (UAM), and drones, automobile components, railway vehicle components, ship components, civil engineering components, electronic equipment frames, sporting goods, etc. In particular, the present invention can be preferably used in aircraft components that require both heat resistance and reliability.

[0183] Example

[0184] The materials used in Examples and Comparative Examples are as follows.

[0185] [PEKK]

[0186] A crystalline polyetherketoneketone containing polyetherketoneketone ("Kepstan" (registered trademark) 6003 manufactured by Arkema Co., Ltd.) having a melting point of 305° C. and a glass transition temperature of 157° C. as measured in accordance with JIS K7121 (2012) was used.

[0187] [PEEK]

[0188] A crystalline polyetheretherketone containing polyetheretherketone (“Victrex” (registered trademark) PEEK381G manufactured by Victrex Corporation) having a melting point of 334° C. and a glass transition temperature of 143° C. as measured in accordance with JIS K7121 (2012) was used.

[0189] [Carbon fiber nonwoven fabric]

[0190] (CF-1)

[0191] A carbon fiber bundle with a total of 12,000 single fibers was obtained by spinning, calcining, and surface oxidation of a copolymer mainly composed of polyacrylonitrile. The carbon fiber bundle had the following properties: a tensile elastic modulus of 220 GPa measured in accordance with JIS R7608 (2007) and a circular cross section with a single fiber diameter of 7 μm.

[0192] The carbon fiber bundle is cut into 6 mm long using a cartridge cutter to obtain chopped carbon fibers. A dispersion containing water and a surfactant (manufactured by Nacalai Tesque (stock), polyoxyethylene lauryl ether (trade name)) with a concentration of 0.1% by mass is prepared, and a carbon fiber nonwoven fabric is prepared using the dispersion and chopped carbon fibers. The manufacturing device includes a cylindrical container with a diameter of 1000 mm having an opening and closing cock at the bottom of the container as a dispersion tank, and a linear conveying portion (inclination angle 30°) connecting the dispersion tank and the papermaking tank. A stirrer is attached to the opening on the upper surface of the dispersion tank, and chopped carbon fibers and a dispersion (dispersion medium) can be added from the opening. The papermaking tank includes a mesh conveyor having a papermaking surface with a width of 500 mm at the bottom, and a conveyor capable of transporting a carbon fiber nonwoven fabric (papermaking substrate) is connected to the mesh conveyor. Papermaking is performed by setting the carbon fiber concentration in the dispersion to 0.05% by mass. In addition, the papermaking conditions were adjusted so that the carbon fibers were dispersed in a monofilamentous state and dispersed isotropically in the in-plane direction. The papermaking substrate was dried in a drying oven at 200°C for 30 minutes to form a paper having a thickness of 1.68 mm and a unit area weight of 100 g / m 2 The carbon fiber nonwoven fabric CF-1. The thermal mass reduction rate of CF-1 is 0 mass %.

[0193] (CF-2)

[0194] Carbon fiber nonwoven fabric CF-2 was obtained in the same manner as CF-1 except that the length of the cut using the box cutter was changed to 3 mm. The weight per unit area of ​​CF-2 was 100 g / m 2 , thickness is 0.85 mm, and thermal mass reduction rate is 0 mass %.

[0195] [Polyamic acid salt (PAMC)]

[0196] The following polyamic acid salt is prepared: 4,4'-(4,4'-isopropylidene diphenyloxy)bis(phthalic anhydride) as tetracarboxylic dianhydride is reacted with m-phenylenediamine as a diamine compound at a molar ratio of 1:1 to obtain a polyamic acid, and the polyamic acid is further neutralized with N,N-dimethyl-2-aminoethanol as a trialkylamine to obtain a polyamic acid salt. The compound is diluted with purified water to prepare an aqueous solution with a concentration of 10% by mass for use.

[0197] [Polyvinyl alcohol (PVA (polyvinylalcohol))]

[0198] Polyvinyl alcohol (Polyvinyl alcohol 500 manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., completely saponified type) was used. The compound was diluted with purified water to prepare an aqueous solution having a concentration of 10% by mass.

[0199] [Polyaminoamide (PAA (polyamine amide))]

[0200] Polyaminoamide was synthesized by reacting 3,3'-diaminobenzidine as an aromatic tetraamine compound and isophthalic acid as a dicarboxylic acid derivative at a molar ratio of 1:1. The polyaminoamide reaction was carried out in an NMP solvent and used as an NMP solution having a concentration of 10% by mass.

[0201] The evaluation methods of the structures, physical properties, etc. in each example / comparative example are as follows.

[0202] [Porosity of carbon fiber substrate]

[0203] The porosity of the carbon fiber substrate is the volume ratio of the pores in the carbon fiber substrate, and is calculated using the thickness and weight per unit area of ​​the carbon fiber substrate and the density of its constituent components using the following formula. The density here can be calculated according to JIS K0061 (2001).

[0204] (Porosity of carbon fiber substrate) = {(Thickness of carbon fiber substrate [m]) - (Weight per unit area of ​​carbon fiber substrate [g / m 2 ]) / (density of the constituent components of the carbon fiber substrate [g / m 3 ])} / (thickness of carbon fiber substrate [m])×100[%].

[0205] [Coverage of resin composition (B)]

[0206] The coverage of the carbon fiber substrate with the resin composition (B) can be determined using the following formula from the surface oxygen concentration (O / C) obtained by X-ray photoelectron spectroscopy.

[0207] The coverage rate (%) of the resin composition (B) = {(O / C of carbon fiber (A)) - (O / C of carbon fiber substrate)} / {(O / C of carbon fiber (A)) - (O / C of resin composition (B))}×100.

[0208] In the samples here, in addition to the carbon fiber substrate, samples of carbon fiber (A) alone before coating with the resin composition (B) and samples obtained by forming a 0.1 mm thick film with the resin composition (B) alone were used.

[0209] The surface oxygen concentration (O / C) of each sample was determined according to the following procedure. First, the sample was cut into pieces with a width of 20 mm and a length of 20 mm and placed on a sample support. 1,2 As an X-ray source, the sample chamber was kept at 1×10 -8 Torr, measured at a photoelectron escape angle of 45°. As a correction value for the peak generated by charging during measurement, C 1s The binding energy value of the main peak (peak top) of is consistent with 284.6 eV. The number of carbon atoms is based on the C obtained by drawing a straight line baseline in the range of 282 eV to 296 eV. 1s The number of oxygen atoms is calculated based on the peak area of ​​O. 1s The surface oxygen concentration (O / C) was determined as the value obtained by dividing the number of oxygen atoms by the number of carbon atoms, that is, the atomic ratio. As an X-ray photoelectron spectrometer, PHI Quantera II manufactured by ULVAC-PHI (Co., Ltd.) was used.

[0210] [Tensile strength of carbon fiber substrate]

[0211] A test piece with a width of 50 mm and a length of 150 mm was cut out from the carbon fiber substrate, and a portion of 50 mm in length was carried at each end, and the remaining portion of 50 mm in length in the middle was subjected to a tensile test at room temperature at a test speed of 3 m / min. The tensile strength [N / cm] was obtained by dividing the maximum point load obtained by the width of the test piece, and the arithmetic mean of 5 samples at each level was used. In addition, the tensile test of the carbon fiber substrate was carried out for the level of heating treatment at 300°C for 5 minutes and the level without the heating treatment. Specifically, as the tensile strength in a certain direction of the carbon fiber substrate, the tensile strength (Ta) of the level subjected to the heating treatment and the tensile strength (Tao) of the level not subjected to the heating treatment were calculated. Furthermore, as the tensile strength in a direction orthogonal to the certain direction, the tensile strength (Tb) of the level subjected to the heating treatment and the tensile strength (Tbo) of the level not subjected to the heating treatment were calculated. The change in tensile strength before and after the heating treatment is calculated based on the Ta and Tao and by the following formula.

[0212] (Strength after heating relative to tensile strength before heating) = Ta / Tao×100[%]

[0213] The tensile strength ratio after the heat treatment (Ta / Tb) was calculated as a value obtained by dividing the Ta by the Tb, and the tensile strength ratio before the heat treatment (Tao / Tbo) was calculated as a value obtained by dividing the Tao by the Tbo.

[0214] [Thermogravimetric / mass analysis (TG-MS)]

[0215] The mass of the gas generated during heating and its components were analyzed using a thermogravimetric / mass spectrometer (TG-MS). The thermal mass reduction rate of the resin composition (B) was determined by the following formula (1) using thermogravimetric analysis (TG).

[0216] Thermal mass reduction rate (mass %) = [(W1-W2) / W1] × 100 (1)

[0217] Here, W1 is the sample mass (mg) after the temperature was raised from room temperature to 100°C at 10°C / min and then isothermally maintained for 30 minutes, and W2 is the sample mass (mg) when the temperature was further raised at 10°C / min to 250°C.

[0218] The generated gas was analyzed by mass spectrometry (MS) using GC / MSQP2010 (manufactured by Shimadzu Corporation). Whether it was a dehydration condensation reaction or a thermal decomposition reaction other than this was determined based on the presence or absence of water in the generated gas.

[0219] [Number average fiber length of carbon fiber (A)]

[0220] 400 carbon fibers were randomly extracted from the carbon fiber nonwoven fabric as the carbon fibers (A), and their lengths were measured using an optical microscope. The number average fiber length (Ln) was calculated using the following formula.

[0221] Number average fiber length (Ln) = (ΣLi) / Nf

[0222] Li: measured fiber length (i = 1, 2, 3, ..., n)

[0223] Nf: The total number of fibers whose length was measured.

[0224] [Average expansion ratio of prepreg in out-of-plane direction]

[0225] The out-of-plane expansion coefficient of the prepreg is determined by the following formula from the thickness of the prepreg and the thickness of the porous structure obtained by expanding the prepreg by heating it at a temperature equal to the melting point of the matrix resin (C) plus 20° C. for 5 minutes.

[0226] Expansion ratio of the prepreg in the out-of-plane direction (%)=[thickness of the porous structure (mm) / thickness of the prepreg (mm)]×100.

[0227] The average expansion coefficient in the out-of-plane direction of the prepreg is determined as the arithmetic mean of the expansion coefficients in the out-of-plane direction of the prepreg measured at five randomly selected locations.

[0228] [Density of prepreg or porous structure]

[0229] Density of prepreg or porous structure (g / cm 3 ) is the mass of the sample (g) divided by the volume (cm 3 ) and is calculated as the arithmetic mean of the results measured in five randomly selected samples.

[0230] [Average pore diameter of prepreg or porous structure]

[0231] The average pore diameter is Figure 4 As shown in the schematic diagram of the surface of the porous structure shown in FIG. 1 , it is measured based on the diameter of the largest circle inscribed in the pores. The surface of the prepreg or porous structure is observed using a scanning electron microscope (SEM), the largest circle inscribed in the pores is depicted in the observed image, and the diameter length of the circle is calculated as the pore diameter. The arithmetic mean of the lengths obtained by measuring the values ​​at 50 randomly selected locations is calculated, i.e., the average pore diameter.

[0232] [Flexural Strength of Porous Structure]

[0233] The bending strength is measured by a three-point bending test according to JIS K7171 (2016) using an "Instron" (registered trademark) 5565 universal material testing machine (manufactured by Instron Japan) as a testing machine. The ambient temperature during the measurement is adjusted by a thermostatic bath, and the bending strength is measured under various temperature environments of 30°C and 140°C. The bending strength uses the arithmetic mean of 5 samples at each level. Furthermore, the retention rate of the bending strength when heated to 140°C is calculated by the following formula.

[0234] (Retention rate of flexural strength when heated to 140°C)=(flexural strength at 140°C [MPa]) / (flexural strength at 30°C [MPa])×100[%].

[0235] [Tensile strength of prepreg]

[0236] The tensile strength of the prepreg is measured by a tensile test according to the International Standardization Organization (ISO) 527-3 method (1995) using an "Instron" (registered trademark) 5565 universal material testing machine (manufactured by Instron Japan) as a testing machine. For the test piece, an arbitrary direction is set as the 0° direction, and a test piece is cut out in four directions, namely, the 45° direction, the 90° direction, and the -45° direction. For each direction, the number of measurements is set to n=5, and for all the measured values ​​(n=20), the maximum and minimum values, and the average value of these, i.e., the average tensile strength, are respectively obtained. The standard deviation is then obtained, and the CV value (coefficient of variation) that can be calculated by the following formula is set as the deviation of the tensile strength.

[0237] Deviation of tensile strength (%) = [(standard deviation of tensile strength) / (average value of tensile strength)] × 100

[0238] Furthermore, the ratio of the maximum value of the tensile strength to the minimum value was determined by dividing the maximum value of the tensile strength by the minimum value of the tensile strength.

[0239] [Prepreg thickness at 400°C and its variation]

[0240] A hot plate including a laser displacement meter and capable of measuring thickness in a non-contact manner is used. The prepreg is placed on a hot plate, heated to 400°C, and the thickness of the prepreg after being kept for 5 minutes is read. The thickness of the prepreg is read at 20 randomly selected locations, and the average value is set as the thickness at 400°C. The standard deviation is then calculated, and the CV value (coefficient of variation) that can be calculated by the following formula is set as the thickness deviation at 400°C.

[0241] Deviation (%) of thickness at 400° C.=[(standard deviation of thickness at 400° C.) / (average value of thickness at 400° C.)]×100.

[0242] [Coverage of the Adhesive Resin Composition (D)]

[0243] The coverage of the carbon fiber substrate with the binder resin composition (D) can be determined using the following formula from the surface oxygen concentration (O / C) obtained by X-ray photoelectron spectroscopy.

[0244] The coverage rate (%) of the adhesive resin composition (D) = {(O / C of carbon fiber (A)) - (O / C of carbon fiber substrate)} / {(O / C of carbon fiber (A)) - (O / C of adhesive resin composition (D))}×100.

[0245] In the samples here, in addition to using a carbon fiber substrate, samples were also used in which a carbon fiber (A) monomer was used before applying an adhesive resin composition (D), and a precursor of the adhesive resin composition (D) was used as a monomer and heated under the same conditions as when making the carbon fiber substrate to form a 0.1 mm thick film.

[0246] The surface oxygen concentration (O / C) of each sample was determined in the same manner as in the above-mentioned "coverage rate of the resin composition (B)".

[0247] [Thermal mass reduction rate]

[0248] Thermogravimetric analysis (TG) was used to determine the thermal mass reduction rate of the carbon fibers (A) and the binder resin composition (D) according to the following formula.

[0249] Thermal mass reduction rate (mass %) = (M1-M2) / M1×100

[0250] Here, M1 is the mass (mg) of the sample after isothermally maintaining at 30°C for 10 minutes, and M2 is the mass (mg) of the sample when the temperature is subsequently increased at 10°C / min to 400°C.

[0251] The carbon fiber (A) sample used was the carbon fiber (A) before the adhesive resin composition (D) was applied. The sample of the adhesive resin composition (D) was evaluated by heating the precursor of the adhesive resin composition (D) alone under the same conditions as when the carbon fiber substrate was prepared.

[0252] [Glass Transition Temperature of Binder Resin Composition (D)]

[0253] The glass transition temperature of the adhesive resin composition (D) was measured using differential scanning calorimetry (DSC) in accordance with JIS K7121 (2012). The sample of the adhesive resin composition (D) was evaluated by heating the precursor of the adhesive resin composition (D) alone under the same conditions as when the carbon fiber substrate was prepared.

[0254] [Fiber length of carbon fiber (A)]

[0255] 400 carbon fibers (A) were randomly selected from the carbon fiber substrate, and their lengths were measured using an optical microscope. The number average fiber length (Ln) was calculated using the following formula.

[0256] Number average fiber length (Ln) = (ΣLi) / Nf

[0257] Li: measured fiber length (i = 1, 2, 3, ..., n)

[0258] Nf: The total number of fibers whose length was measured.

[0259] [Mass Ratio of Carbon Fiber (A) in Carbon Fiber Base Material]

[0260] The mass ratio of the carbon fibers (A) in the carbon fiber substrate is determined by the following formula from the mass of the carbon fiber substrate and the mass of the carbon fibers (A) before application of the precursor of the binder resin composition.

[0261] Mass ratio (%) of carbon fibers (A) in the carbon fiber base material=(mass (g) of carbon fibers (A)) / (mass (g) of carbon fiber base material)×100.

[0262] [Mass Ratio of Carbon Fiber (A) in Prepreg]

[0263] The mass ratio of the carbon fibers (A) in the prepreg is determined by the following formula from the mass of the prepreg and the mass of the carbon fibers (A) used therein.

[0264] Mass ratio (%) of carbon fibers (A) in the prepreg=(mass (g) of carbon fibers (A)) / (mass (g) of prepreg)×100.

[0265] [Expansion rate of fiber-reinforced resin molded body or void body]

[0266] The expansion coefficient of the fiber-reinforced resin molded body or the void body is determined by the following formula based on the thickness of the preform used for molding and the thickness of the fiber-reinforced resin molded body or the void body obtained by molding the preform.

[0267] (Expansion ratio) = (thickness of fiber-reinforced resin molded body or void body [mm]) / (thickness of preform [mm]) × 100 [%]

[0268] The thickness of the fiber-reinforced resin molded body or the void body and the thickness of the preform were each determined as the average value of thicknesses measured at five randomly selected locations.

[0269] [Density of fiber-reinforced resin molded body or void body]

[0270] Density of fiber-reinforced resin molded body or void body [g / cm 3 ] is the mass of the sample [g] divided by the volume [cm 3 ] and is calculated as the average value of the results measured in 5 randomly selected samples.

[0271] Hereinafter, the carbon fiber base material, the prepreg, and the porous structure produced in the examples and comparative examples of the present invention will be described.

[0272] [Example 1]

[0273] (Carbon fiber (A))

[0274] As the carbon fiber (A), carbon fiber obtained by cutting a carbon fiber nonwoven fabric CF-1 into a size of 300 mm×300 mm was used.

[0275] (Resin composition (B))

[0276] PAMC was used as the resin composition (B), and was diluted to prepare an aqueous solution of 1% by mass.

[0277] (Carbon fiber substrate)

[0278] The carbon fiber nonwoven fabric was immersed in the aqueous solution. Then, the carbon fiber nonwoven fabric was taken out and heated and dried at 100° C. for 1 hour to prepare a carbon fiber substrate.

[0279] The difference between the mass of the obtained carbon fiber substrate and the mass of the used carbon fiber (A) is the amount of the resin composition (B) attached, and the amount of the resin composition (B) is 5 parts by mass relative to 100 parts by mass of the carbon fiber (A). In addition, the coverage of the resin composition (B) is 100%. The results of each evaluation are shown in Table 1.

[0280] [Example 2]

[0281] The resin composition (B) was diluted again to a concentration of 3% by mass, and the amount of the resin composition (B) deposited was 10 parts by mass. A carbon fiber substrate was obtained in the same manner as in Example 1 except for the above.

[0282] The coverage of the resin composition (B) in the carbon fiber substrate was 100%. Table 1 shows the results of each evaluation.

[0283] [Comparative Example 1]

[0284] A carbon fiber substrate was obtained in the same manner as in Example 1 except that PVA was used as the resin composition (B). The coverage of the sample with PVA was 100%. Table 1 shows the results of each evaluation.

[0285] [Comparative Example 2]

[0286] The carbon fiber nonwoven fabric CF-1 was used for evaluation as it was without using the resin composition (B). Table 1 shows the results of each evaluation.

[0287] [Example 3]

[0288] (Carbon fiber (A))

[0289] The same cut carbon fiber nonwoven fabric CF-1 as the carbon fiber nonwoven fabric CF-1 used in Example 1 was used.

[0290] (Resin composition (B))

[0291] PAA was used as the resin composition (B), and was diluted to 1% by mass in an N-methyl-2-pyrrolidone (NMP) solution.

[0292] (Carbon fiber substrate)

[0293] The carbon fiber nonwoven fabric is immersed in the NMP solution. The carbon fiber nonwoven fabric is then taken out from the NMP solution and then immersed in water, thereby precipitating the resin composition (B) on the surface of the carbon fiber (A). The carbon fiber nonwoven fabric is then taken out from the water and heated and dried at 100° C. for 1 hour to prepare a carbon fiber substrate.

[0294] The amount of the resin composition (B) attached was 5 parts by mass relative to 100 parts by mass of the carbon fibers (A). The coverage of the resin composition (B) was 100%. Table 1 shows the results of each evaluation.

[0295] [Table 1]

[0296]

[0297] [Example 1-2]

[0298] (Carbon fiber substrate)

[0299] As the carbon fiber substrate, the carbon fiber substrate obtained in Example 1 was used.

[0300] (Matrix resin (C))

[0301] As the matrix resin (C), two sheets of PEKK having a unit area weight of 150 g / m 2 300mm×300mm resin film.

[0302] (Prepreg)

[0303] The carbon fiber substrate and the resin film are stacked in the order of resin film / carbon fiber substrate / resin film. Furthermore, the laminate is clamped by a flat-plate mold (tooling plate) made of 400mm×400mm stainless steel (SUS), thereby heating and pressing the laminate while conveying the laminate. The pressing process is first carried out by heating at a temperature of 350°C and a pressure of 10MPa for 10 minutes. Then, it is cooled and solidified at a temperature of 150°C and a pressure of 10MPa for 10 minutes to produce a prepreg with a thickness of 0.28mm.

[0304] Regarding the appearance of the obtained prepreg, no damage was found in the carbon fiber base material, and no molding failure was confirmed.

[0305] [Example 2-2]

[0306] A prepreg was prepared in the same manner as in Example 1-2 except that the carbon fiber substrate obtained in Example 2 was used as the carbon fiber substrate. In terms of the appearance of the obtained prepreg, no damage was found in the carbon fiber substrate and no molding failure was confirmed. The results of each evaluation are shown in Table 2.

[0307] [Comparative Example 1-2]

[0308] A prepreg was prepared in the same manner as in Example 1-2 except that the carbon fiber base material obtained in Comparative Example 1 was used as the carbon fiber base material.

[0309] In the obtained prepreg, molding defects due to damage of the carbon fiber substrate were found at some locations. Table 2 shows the results of various evaluations performed by selecting locations with less damage.

[0310] [Comparative Example 2-2]

[0311] A prepreg was prepared in the same manner as in Example 1-2 except that the carbon fiber nonwoven fabric CF-1 evaluated in Comparative Example 2 was used as the carbon fiber substrate. However, the carbon fiber substrate was damaged and shattered during press molding, and a prepreg could not be obtained. The results are shown in Table 2.

[0312] [Example 3-2]

[0313] A prepreg was prepared in the same manner as in Example 1-2 except that the carbon fiber base material obtained in Example 3 was used as the carbon fiber base material.

[0314] Regarding the appearance of the obtained prepreg, no damage was found in the carbon fiber base material, and no molding failure was confirmed.

[0315] [Table 2]

[0316]

[0317] [Examples 1-3]

[0318] (Prepreg)

[0319] As the prepreg, the prepreg obtained in Example 1-2 was used.

[0320] (Porous structure)

[0321] The prepreg of 300mm×300mm and 0.28mm thickness was stacked in four sheets and clamped between a 400mm×400mm SUS flat-plate mold (tooling plate) together with a 4mm thick SUS spacer, thereby performing heating and pressurization while controlling the expansion ratio. In the pressing process, first, heating was performed at a temperature of 350°C and a pressure of 1MPa for 10 minutes, and then, cooling and curing were performed at a temperature of 150°C and a pressure of 1MPa for 10 minutes. The expansion ratio was controlled to 360%, and the thickness of the obtained porous structure was 4mm. The results of each evaluation are shown in Table 3.

[0322] [Comparative Examples 1-3]

[0323] The porous structure was produced in the same manner as in Example 1-3 except that the prepreg obtained in Comparative Example 1-2 was used as the prepreg.

[0324] [Example 3-3]

[0325] A porous structure was produced in the same manner as in Example 1-3 except that the prepreg obtained in Example 3-2 was used as the prepreg.

[0326] [Examples 1-4]

[0327] (Prepreg)

[0328] As the prepreg, the prepreg obtained in Example 1-2 was used.

[0329] (Porous structure)

[0330] The prepreg of 300mm×300mm and 0.28mm thickness is stacked in three sheets and clamped between a 400mm×400mm SUS-made flat-plate mold (tooling plate) together with a 4mm thick SUS spacer, thereby heating and pressing while controlling the expansion ratio. In the pressing process, first heat at a temperature of 350°C and a pressure of 1MPa for 10 minutes, and then cool and solidify at a temperature of 150°C and a pressure of 1MPa for 10 minutes. The expansion ratio is controlled to 480%, and the thickness of the obtained porous structure is 4mm. The results of each evaluation are shown in Table 3.

[0331] [Comparative Examples 1-4]

[0332] A porous structure was produced in the same manner as in Example 1-4 except that the prepreg obtained in Comparative Example 1-2 was used as the prepreg. However, the expansion ratio in the out-of-plane direction was insufficient, and the target porous structure of 4 mm thickness could not be obtained. The results of each evaluation are shown in Table 3.

[0333] [Examples 3-4]

[0334] A porous structure was produced in the same manner as in Example 1-4 except that the prepreg obtained in Example 3-2 was used as the prepreg.

[0335] [Table 3]

[0336]

[0337] [Example 4]

[0338] (Carbon fiber (A))

[0339] The same cut carbon fiber nonwoven fabric CF-1 as the carbon fiber nonwoven fabric CF-1 used in Example 1 was used.

[0340] (Resin composition (B))

[0341] As a solution of the resin composition (B) which is a precursor of the binder resin composition (D), a 1 mass % aqueous solution of PAMC similar to the solution used in Example 1 was used.

[0342] (Carbon fiber substrate)

[0343] The carbon fiber nonwoven fabric is immersed in the aqueous solution. Then, the carbon fiber nonwoven fabric is taken out and heated and dried at 200°C for 1 hour to imidize the PAMC to obtain a carbon fiber substrate in which the polyetherimide resin as the adhesive resin composition (D) is attached to the carbon fiber (A). The fiber length of the reinforcing fiber (A) is 6 mm, and the coverage of the adhesive resin composition (D) is 100%. The glass transition temperature of the adhesive resin composition (D) is 220°C, and the thermal mass reduction rate at 400°C is 1% by mass.

[0344] (Matrix resin (C))

[0345] As the matrix resin (C), two sheets of PEKK having a unit area weight of 150 g / m 2 300mm×300mm resin film.

[0346] (Prepreg)

[0347] The carbon fiber substrate and the resin film are stacked in the order of resin film / carbon fiber substrate / resin film. Furthermore, the laminate is clamped by a 400mm×400mm SUS-made flat-plate mold (tooling plate), thereby heating and pressing while conveying the laminate. In the pressing process, first, heating is performed at a temperature of 350°C and a pressure of 10MPa for 10 minutes, and then cooling and curing is performed at a temperature of 30°C and a pressure of 10MPa for 10 minutes, thereby producing a prepreg with a thickness of 0.28mm. The results of each evaluation are shown in Table 4.

[0348] [Example 5]

[0349] A prepreg was obtained in the same manner as in Example 4 except that the concentration of the PAMC aqueous solution was set to 3% by mass. The fiber length of the carbon fiber (A) was 6 mm, and the coverage of the adhesive resin composition (D) was 100%. The glass transition temperature of the adhesive resin composition (D) was 220°C, and the thermal mass reduction rate at 400°C was 1% by mass. The thickness of the prepreg was 0.28 mm. The results of each evaluation are shown in Table 4.

[0350] [Example 6]

[0351] A prepreg was obtained in the same manner as in Example 4 except that CF-2 was used as the carbon fiber (A). The fiber length of the carbon fiber (A) was 3 mm, and the coverage of the adhesive resin composition (D) was 100%. The glass transition temperature of the adhesive resin composition (D) was 220° C., and the thermal mass reduction rate at 400° C. was 1% by mass. The thickness of the prepreg was 0.28 mm. The results of each evaluation are shown in Table 4.

[0352] [Example 7]

[0353] A prepreg was obtained in the same manner as in Example 4 except that PEEK was used as the matrix resin (C). The fiber length of the carbon fiber (A) was 6 mm, and the coverage of the adhesive resin composition (D) was 100%. The glass transition temperature of the adhesive resin composition (D) was 220° C., and the thermal mass reduction rate at 400° C. was 1% by mass. The thickness of the prepreg was 0.28 mm. The results of each evaluation are shown in Table 4.

[0354] [Example 8]

[0355] (Carbon fiber (A))

[0356] The same cut carbon fiber nonwoven fabric CF-1 as the carbon fiber nonwoven fabric CF-1 used in Example 1 was used.

[0357] (Resin composition (B))

[0358] PAA was used as the resin composition (B) which was a precursor of the binder resin composition (D), and was diluted to prepare a 1 mass % NMP solution.

[0359] (Carbon fiber substrate)

[0360] The carbon fiber nonwoven fabric is immersed in the NMP solution. Then, the carbon fiber nonwoven fabric is taken out and heated and dried at 200°C for 1 hour to imidazole the PAA, thereby obtaining a carbon fiber substrate in which the polybenzimidazole resin as the adhesive resin composition (D) is attached to the carbon fiber (A). The coverage of the adhesive resin composition (D) is 100%. The glass transition temperature of the adhesive resin composition (D) is 425°C, and the thermal mass reduction rate at 400°C is 1% by mass.

[0361] (Matrix resin (C))

[0362] As the matrix resin (C), two sheets of PEKK having a unit area weight of 150 g / m 2 300mm×300mm resin film.

[0363] (Prepreg)

[0364] The carbon fiber substrate and the resin film are stacked in the order of resin film / carbon fiber substrate / resin film. Furthermore, the laminate is clamped by a 400mm×400mm SUS-made flat-plate mold (tooling plate), thereby heating and pressing while conveying the laminate. In the pressing process, first, heating is performed at a temperature of 350°C and a pressure of 10MPa for 10 minutes, and then cooling and curing is performed at a temperature of 30°C and a pressure of 10MPa for 10 minutes, thereby producing a prepreg with a thickness of 0.28mm. The results of each evaluation are shown in Table 4.

[0365] [Example 9]

[0366] A prepreg was obtained in the same manner as in Example 8 except that PEEK was used as the matrix resin (C). The fiber length of the carbon fiber (A) was 6 mm, and the coverage of the adhesive resin composition (D) was 100%. The glass transition temperature of the adhesive resin composition (D) was 425° C., and the thermal mass reduction rate at 400° C. was 1% by mass. The thickness of the prepreg was 0.28 mm. The results of each evaluation are shown in Table 4.

[0367] [Comparative Example 3]

[0368] A prepreg was obtained in the same manner as in Example 4 except that PVA was used as the resin composition (B). The coverage of the adhesive resin composition (D) was 100%. The glass transition temperature of the adhesive resin composition (D) was 60° C., and the thermal mass reduction rate at 400° C. was 60% by mass. The thickness of the prepreg was 0.28 mm. The results of each evaluation are shown in Table 4.

[0369] [Comparative Example 4]

[0370] A prepreg was obtained in the same manner as in Comparative Example 3 except that CF-2 was used as the carbon fiber (A). The fiber length of the carbon fiber (A) was 3 mm, and the coverage of the adhesive resin composition (D) was 100%. The glass transition temperature of the adhesive resin composition (D) was 60° C., and the thermal mass reduction rate at 400° C. was 60% by mass. The thickness of the prepreg was 0.28 mm. The results of each evaluation are shown in Table 4.

[0371] [Comparative Example 5]

[0372] A prepreg was obtained in the same manner as in Comparative Example 3 except that PEEK was used as the matrix resin (C). The fiber length of the carbon fiber (A) was 6 mm, and the coverage of the adhesive resin composition (D) was 100%. The glass transition temperature of the adhesive resin composition (D) was 60° C., and the thermal mass reduction rate at 400° C. was 60% by mass. The thickness of the prepreg was 0.28 mm. The results of each evaluation are shown in Table 4.

[0373] [Table 4]

[0374]

[0375] [Example 10]

[0376] (Prepreg)

[0377] As the prepreg, the prepreg obtained in Example 4 was used.

[0378] (Preform)

[0379] Four of the above-mentioned prepregs having a size of 300 mm×300 mm and a thickness of 0.28 mm were stacked to prepare a preform.

[0380] (Fiber-reinforced resin molded body)

[0381] The preform was clamped between 400mm×400mm SUS flat-plate molds (tooling plates) and heated and pressed. In the pressing process, it was first heated at a temperature of 350°C and a pressure of 3MPa for 10 minutes, and then cooled and solidified at a temperature of 30°C and a pressure of 5MPa for 10 minutes. The obtained fiber-reinforced resin molded body had a thickness of 1.12mm, an expansion rate of 100%, and a density of 1.4g / cm 3 , and it is a molded product without gaps.

[0382] [Example 11]

[0383] (Prepreg)

[0384] As the prepreg, the prepreg obtained in Example 4 was used.

[0385] (Preform)

[0386] Four of the above-mentioned prepregs having a size of 300 mm×300 mm and a thickness of 0.28 mm were stacked to prepare a preform.

[0387] (Fiber-reinforced resin molded body)

[0388] The preform is clamped together with a 4mm thick SUS spacer between a 400mm×400mm SUS flat-plate mold (tooling plate), thereby performing heating and pressurization while controlling the expansion rate. In the pressing process, first, it is heated at a temperature of 350°C and a pressure of 3MPa for 10 minutes, and then cooled and solidified at a temperature of 30°C and a pressure of 1MPa for 10 minutes to obtain a fiber-reinforced resin molded body (void body) with voids. The obtained void body has a thickness of 4mm, an expansion rate of 360%, and a density of 0.4g / cm 3 The bending strength at 30°C was 53 MPa, and the bending strength at 140°C was 48 MPa. The retention rate of the bending strength when heated to 140°C was 91%.

[0389] [Example 12]

[0390] A void body was formed in the same manner as in Example 11 except that the prepreg obtained in Example 8 was used as the prepreg. The obtained void body had a thickness of 4 mm, an expansion ratio of 360%, and a density of 0.4 g / cm 3 The bending strength at 30°C was 53 MPa, the bending strength at 140°C was 50 MPa, and the retention rate of the bending strength when heated to 140°C was 94%.

[0391] [Comparative Example 6]

[0392] A void body was formed in the same manner as in Example 11 except that the prepreg obtained in Comparative Example 3 was used as the prepreg. The obtained void body had a thickness of 4 mm, an expansion ratio of 360%, and a density of 0.4 g / cm 3 The bending strength at 30°C was 47 MPa, the bending strength at 140°C was 32 MPa, and the retention rate of the bending strength when heated to 140°C was 68%.

[0393] [Example 13]

[0394] (Prepreg)

[0395] As the prepreg, the prepreg obtained in Example 1-2 was used.

[0396] (Preform)

[0397] Two sheets of the above-mentioned prepreg having a length of 300 mm×a width of 300 mm and a thickness of 0.28 mm were stacked to prepare a preform.

[0398] (Fiber-reinforced resin molded body)

[0399] The preform is clamped between a pair of molds with concave and convex shapes, and heated and pressed while controlling the expansion rate. In the pressing process, it is first heated at a temperature of 350°C and a pressure of 3MPa for 10 minutes, and then cooled and solidified at a temperature of 30°C and a pressure of 1MPa for 10 minutes. The obtained fiber-reinforced resin molded body has a thickness of 2mm, an expansion rate of 360%, and a density of 0.4g / cm 3 Furthermore, the obtained fiber-reinforced resin molded body is formed into a corrugated shape by transferring the concavo-convex shape of the mold, and when observed from one of the surfaces, it is a corrugated plate shape in which the fiber-reinforced resin molded body, which is 10 mm long in the length direction, is repeatedly bent in the order of bending angles of 120° / 120° / 240° / 240°.

[0400] [Example 14]

[0401] The corrugated fiber-reinforced resin molded body obtained in Example 13 was cut into strips with a width of 10 mm. The convex parts of the adjacent cut pieces were stacked so that the convex parts were facing each other. The epoxy resin adhesive (120° C. curing type) was applied to the joint surfaces of the convex parts, and the convex parts were heated and pressurized at a temperature of 120° C. and a pressure of 0.1 MPa for 1 hour to obtain a fiber-reinforced resin molded body with a honeycomb structure in which hollow columnar chambers in the shape of regular hexagonal prisms with a side of 10 mm were arranged.

[0402] [Example 15]

[0403] (core material)

[0404] The honeycomb-shaped fiber-reinforced resin molded body obtained in Example 14 was used as a core material.

[0405] (Surface material)

[0406] Two sheets of the prepreg obtained in Example 1-2 were used as a pair of surface materials.

[0407] (Sandwich structure)

[0408] Epoxy resin adhesive (120°C curing type) was applied to the facing surfaces of the two skin materials. The core material was sandwiched between the skin materials and heated and pressed at 120°C and 0.1 MPa for 1 hour to integrate them into a sandwich structure.

[0409] [Explanation of Symbols]

[0410] 1: Carbon fiber (A)

[0411] 2: Resin composition (B) or adhesive resin composition

[0412] 3: Porosity

[0413] 4: Carbon fiber (A) coated with a resin composition (B) or an adhesive resin composition

[0414] 5: Matrix resin (C)

[0415] 6: In-plane direction

[0416] 7: Out-of-plane direction

[0417] 8: Pore diameter (diameter of the inscribed circle of the pore)

Claims

1. A carbon fiber substrate comprising carbon fibers (A) and a resin composition (B) coating the surface of the carbon fibers (A), Carbon fiber (A) forms a non-woven fabric. The tensile strength of the carbon fiber substrate after being heated at 300° C. for 5 minutes is 110% or more of that before the heating.

2. The carbon fiber substrate according to claim 1, wherein The resin composition (B) contains at least one selected from the group consisting of polyamic acid, polyamic acid salt, polyamic acid ester, polyhydroxyamide, and polyaminoamide.

3. The carbon fiber substrate according to claim 1 or 2, wherein The resin composition (B) can undergo a dehydration condensation reaction, wherein the thermal mass reduction rate defined by the following formula (1) in the reaction is 5% by mass to 50% by mass, Thermal mass reduction rate (mass %) = [(W1-W2) / W1] × 100 (1) Here, W1 is the sample mass (mg) after the temperature was raised from room temperature to 100°C at 10°C / min and then isothermally maintained for 30 minutes, and W2 is the sample mass (mg) when the temperature was further raised at 10°C / min to 250°C.

4. The carbon fiber substrate according to any one of claims 1 to 3, wherein The tensile strength ratio (Ta / Tb) obtained by dividing the tensile strength in any direction (Ta) of the carbon fiber substrate measured at room temperature after heating at 300°C for 5 minutes by the tensile strength in the orthogonal direction (Tb) is 0.6 to 1.

7.

5. The carbon fiber substrate according to any one of claims 1 to 4, wherein The number average fiber length of the carbon fibers (A) is 0.1 mm to 100 mm.

6. The carbon fiber substrate according to any one of claims 1 to 5, wherein The resin composition (B) is contained in an amount of 0.5 to 30 parts by mass based on 100 parts by mass of the carbon fibers (A).

7. The carbon fiber substrate according to any one of claims 1 to 6, wherein The mass ratio of the carbon fibers (A) in the carbon fiber substrate is 90% or more and 97% or less.

8. A prepreg, wherein the carbon fiber substrate according to any one of claims 1 to 7, or a substrate derived therefrom, is impregnated with a matrix resin (C).

9. The prepreg according to claim 8, wherein the base material comprising the carbon fiber (A) and the adhesive resin composition is impregnated with the matrix resin (C), The adhesive resin composition is the resin composition (B) or is derived from the resin composition (B), The adhesive resin composition has a glass transition temperature of 120° C. or higher and 450° C. or lower. The melting point of the matrix resin (C) is 250° C. or higher and 400° C. or lower. The adhesive resin composition is present at the interface between the carbon fiber (A) and the matrix resin (C), The prepreg satisfies the following conditions (i) and (ii): (i) The minimum tensile strength is 100 MPa or more; (ii) The thickness deviation at 400° C. is 10% or less.

10. A prepreg, comprising a substrate comprising carbon fibers (A) and an adhesive resin composition (D) impregnated with a matrix resin (C), wherein: The carbon fiber (A) is discontinuous fiber and forms a non-woven fabric. The glass transition temperature of the adhesive resin composition (D) is 120° C. or higher and 450° C. or lower. The melting point of the matrix resin (C) is 250° C. or higher and 400° C. or lower. The adhesive resin composition (D) is present at the interface between the carbon fiber (A) and the matrix resin (C). The prepreg satisfies the following conditions (i) and (ii): (i) The minimum tensile strength is 100 MPa or more; (ii) The thickness deviation at 400° C. is 10% or less.

11. The prepreg according to claim 10, wherein The adhesive resin composition (D) is a composition containing a polymer having at least one structure selected from the group consisting of an etherimide skeleton, a benzoxazole skeleton, a benzimidazole skeleton, a benzoxazine skeleton, and a cyanate skeleton, or a derivative thereof.

12. The prepreg according to claim 10 or 11, wherein The adhesive resin composition (D) comprises at least one resin selected from phenolic resin, urea-formaldehyde resin, melamine resin, polyimide resin, polybenzoxazole resin, polybenzimidazole resin, bismaleimide resin, benzoxazine resin, and cyanate resin.

13. The prepreg according to any one of claims 10 to 12, wherein The adhesive resin composition (D) has a thermal mass reduction rate at 400° C. of 5% by mass or less.

14. The prepreg according to any one of claims 8 to 13, wherein The matrix resin (C) contains at least one selected from polyetherketone, polyetheretherketone, and polyetherketoneketone as a main component.

15. The prepreg according to any one of claims 8 to 14, wherein The amount of the matrix resin (C) is 5 to 1,000 parts by mass based on 100 parts by mass of the carbon fibers (A).

16. The prepreg according to any one of claims 8 to 15, wherein The carbon fibers (A) contain 50% by mass or more of fibers having a fiber length of 2 mm to 10 mm.

17. The prepreg according to any one of claims 8 to 16, wherein The thickness at 400° C. is 0.1 mm or more and 5 mm or less.

18. The prepreg according to any one of claims 8 to 17, wherein The variation in tensile strength within the plane is 20% or less.

19. The prepreg according to any one of claims 8 to 18, wherein The maximum value of tensile strength is 260 MPa or more.

20. The prepreg according to any one of claims 8 to 19, wherein The ratio of the maximum value of the tensile strength to the minimum value of the tensile strength is 1-3.

21. The prepreg according to any one of claims 8 to 20, wherein The mass ratio of the carbon fibers (A) in the prepreg is 1% to 50%.

22. The prepreg according to any one of claims 8 to 21, wherein When the matrix resin (C) is melted, it expands at an average expansion rate of 150% to 1,000% in the out-of-plane direction.

23. A porous structure formed from the prepreg according to any one of claims 8 to 22.

24. The porous structure according to claim 23, wherein The bending strength when heated to 140°C is 80% or more of the bending strength at 30°C.

25. A method for producing a porous structure, which is a method for producing the porous structure according to claim 23 or 24, comprising: In the first step, the matrix resin (C) is melted and expanded; and a second step of curing the matrix resin (C).

26. A preform comprising the prepreg according to any one of claims 8 to 22 as a lamination unit.

27. A fiber-reinforced resin molded body obtained by heating and pressurizing the preform according to claim 26.

28. A fiber-reinforced resin molded body formed by heating and expanding the preform according to claim 26, and having voids.

29. The fiber-reinforced resin molded product according to claim 27 or 28, which has a corrugated shape or a honeycomb shape.

30. A sandwich structure, comprising the fiber-reinforced resin molded body according to any one of claims 27 to 29 as a core material, sandwiched between a pair of surface materials, and integrated.

31. An aircraft component comprising the prepreg according to any one of claims 8 to 22, the porous structure according to claim 23 or 24, the fiber-reinforced resin molded body according to any one of claims 27 to 29, or the sandwich structure according to claim 30.

Citation Information

Cited By

  • Carbon fiber substrate, prepreg, porous structure, method for manufacturing same, preform, fiber-reinforced resin molded body, sandwich structure, and aircraft member

    EP4502268A4