Alpha-Bi2O3 / alpha-Bi2O3 homojunction photocatalyst as well as preparation method and application thereof
By vertically growing α-Bi2O3 nanosheets on α-Bi2O3 nanorods, an α-Bi2O3 homojunction photocatalyst was prepared, which solved the problem that the properties and applications of this material were not studied in-depth in the prior art. , achieves efficient catalysis and stability, and has a wide range of applications for remediation of polluted water bodies.
Patent Information
- Application Number
- CN202411024761.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
At present, there is a lack of research and synthesis methods on α-Bi2O3/α-Bi2O3 homojunction photocatalyst, resulting in the failure to fully explore its properties and applications.
By mixing Bi2O3 nanorods with surfactant and adding acidic medium to react, an α-Bi2O3/α-Bi2O3 homojunction photocatalyst was prepared, where α-Bi2O3 nanosheets grew vertically on α-Bi2O3 nanorods, which improved Specific surface area and reaction sites to enhance photocatalytic activity.
The performance of efficient catalytic reduction of hexavalent chromium and degradation of bisphenol A of α-Bi2O3/α-Bi2O3 homojunction photocatalyst is achieved, and it has good photostability and reusability, with broad application prospects.
Smart Images

Figure CN118925709A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of photocatalyst and contaminated water restoration, and in particular to an α-Bi2O3 / α-Bi2O3 homojunction photocatalyst and a preparation method and application thereof. Background Art
[0002] In recent years, photocatalytic technology has been widely studied and applied in water decomposition, decomposition of organic pollutants, and reduction of carbon dioxide. Bi2O3 has a band gap of only 2.8eV and has excellent photocatalytic activity, becoming a research hotspot for photocatalytic materials in recent years. At present, there are many studies on Bi2O3 heterojunctions at home and abroad, and they all show excellent photocatalytic degradation of heavy metal ions and organic pollutants, and catalytic performance of organic small molecule reactions. Recently, α-Bi2O3 / β-Bi2O3 homojunctions have been reported in the literature. Since the two sides of the junction interface are the same material, the junction medium is connected by a strong chemical bond, which effectively reduces the junction interface energy barrier, is conducive to the rapid transfer of photogenerated electrons at the interface, and greatly improves the photocatalytic activity.
[0003] At present, there is no report on the synthesis of α-Bi2O3 / α-Bi2O3 homojunction. Therefore, the properties and synthesis methods of α-Bi2O3 / α-Bi2O3 homojunction need to be further studied. Summary of the invention
[0004] The purpose of the present invention is to provide an α-Bi2O3 / α-Bi2O3 homojunction photocatalyst and a preparation method and application thereof. The α-Bi2O3 nanosheets of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst grow vertically on α-Bi2O3 nanorods, providing a larger specific surface area and more reaction sites, thereby improving the photocatalytic activity. At the same time, the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst has good photostability and reusability and can be recycled. Moreover, the preparation method of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst is simple and convenient, low in cost, green and environmentally friendly, and has broad application prospects.
[0005] In order to achieve the above-mentioned object, in a first aspect, the present invention provides an α-Bi2O3 / α-Bi2O3 homojunction photocatalyst, wherein the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst comprises α-Bi2O3 nanorods and α-Bi2O3 nanosheets; wherein,
[0006] The α-Bi2O3 nanosheets grow vertically on the α-Bi2O3 nanorods.
[0007] In a second aspect, the present invention provides a method for preparing an α-Bi2O3 / α-Bi2O3 homojunction photocatalyst, characterized in that the preparation method comprises: mixing a precursor solution with a surfactant, adding an acidic medium for reaction;
[0008] Wherein, the precursor is Bi2O3 nanorods.
[0009] In a third aspect, the present invention provides an α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared by the preparation method described in the second aspect.
[0010] In a fourth aspect, the present invention provides an application of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst as described in the first aspect or the third aspect in the restoration of polluted water bodies.
[0011] In a fifth aspect, the present invention provides a method for reducing hexavalent chromium in polluted water, characterized in that the method comprises: mixing a photocatalyst with water containing hexavalent chromium, adjusting pH, adsorbing in the dark, and then irradiating with visible light;
[0012] Wherein, the photocatalyst is the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst described in the first aspect or the third aspect.
[0013] In a sixth aspect, the present invention provides a method for degrading bisphenol A in polluted water, characterized in that the method comprises: mixing a photocatalyst with water containing bisphenol A, adjusting the pH, adsorbing in the dark, and then irradiating with visible light;
[0014] Wherein, the photocatalyst is the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst described in the first aspect or the third aspect.
[0015] In the above technical scheme, the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst of the present invention includes α-Bi2O3 nanorods and α-Bi2O3 nanosheets; wherein the α-Bi2O3 nanosheets grow vertically on the α-Bi2O3 nanorods, and the special homogeneous structure provides a larger specific surface area and more reaction sites, thereby improving the photocatalytic activity.
[0016] At the same time, the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst of the present invention is prepared by mixing porous α-Bi2O3 nanorods as a precursor with a surfactant at room temperature (15-30°C), adding an acidic medium, and synthesizing the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst by simple stirring. The steps are simple, the reaction conditions are mild, the cost is low, and it is green and environmentally friendly.
[0017] Furthermore, the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst of the present invention has excellent photocatalytic performance in catalytic reduction of hexavalent chromium [Cr(VI)] and degradation of bisphenol A (BPA), and has good photostability and reusability, and has broad application prospects.
[0018] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:
[0020] Figure 1 X-ray diffraction (XRD) spectra of the Bi2O3 nanorods prepared in Preparation Example 1, the α-Bi2O3 / α-Bi2O3 homojunction photocatalysts prepared in Examples 1-3, and the Bi2O3 nanosheets prepared in Comparative Example 1;
[0021] Figure 2 a is a scanning electron microscope analysis (SEM) image of the Bi2O3 nanorods prepared in Preparation Example 1, b is a SEM image of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 2, c is a SEM image of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1, d is a SEM image of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 3, and e is a SEM image of the Bi2O3 nanosheets prepared in Comparative Example 1;
[0022] Figure 3 a is a SEM image of the product obtained in Comparative Example 2, and b is a SEM image of the product obtained in Comparative Example 3;
[0023] Figure 4 a is a transmission electron microscope (TEM) image of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1, and b is a high-resolution transmission electron microscope (HRTEM) image of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1;
[0024] Figure 5 a is the UV-visible diffuse reflectance spectrum of the Bi2O3 nanorods prepared in Preparation Example 1 and the Bi2O3 nanosheets prepared in Comparative Example 1, and b is the energy band diagram of the Bi2O3 nanorods prepared in Preparation Example 1 and the Bi2O3 nanosheets prepared in Comparative Example 1;
[0025] Figure 6Wherein a is the degradation curve of α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 for Cr(VI) (50 mg / L), b is the degradation curve of α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 for Cr(VI) (50 mg / L) at different pH values, c is the degradation curve of α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 with different dosages for Cr(VI) (50 mg / L), d is the degradation curve of α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 for Cr(VI) solutions of different concentrations;
[0026] Figure 7 a is the degradation curve of α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 for Cr(VI) (50 mg / L) under different cycle numbers, b is the SEM image of α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 after reducing Cr(VI) (50 mg / L) under light, c is the XRD image of α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 after reducing Cr(VI) (50 mg / L) under light, d is the X-ray photoelectron spectrum (XPS) of Cr 2p after α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 after reducing Cr(VI) (50 mg / L) under light;
[0027] Figure 8 The degradation curve of bisphenol A (BPA) (20 mg / L) of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1;
[0028] Fig. 9 a is a three-dimensional morphology image of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1, b is a Kelvin probe microscope (KPFM) image of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 collected from Bi2O3 nanosheets (left) to Bi2O3 nanorods (right), c is a surface potential map of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 under illumination, and d is a profile of the potential line corresponding to the surface potential map;
[0029] Fig.10 a is the degradation curve of α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 to Cr(VI) (50 mg / L) in the presence of different scavengers, b is the degradation curve of α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 to BPA (20 mg / L) in the presence of different scavengers, c is the degradation curve of DMPO-·O2- d is the electron spin resonance spectrum (EPR) of DMPO-·OH of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 under dark and light irradiation;
[0030] Fig.11 In the figure, a is the energy band diagram of Bi2O3 nanorods and Bi2O3 nanosheets, and b is the photocatalytic mechanism diagram of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1. DETAILED DESCRIPTION
[0031] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0032] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0033] In a first aspect, the present invention provides an α-Bi2O3 / α-Bi2O3 homojunction photocatalyst, wherein the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst comprises α-Bi2O3 nanorods and α-Bi2O3 nanosheets; wherein,
[0034] The α-Bi2O3 nanosheets grow vertically on the α-Bi2O3 nanorods.
[0035] The α-Bi2O3 / α-Bi2O3 homojunction photocatalyst of the present invention comprises α-Bi2O3 nanorods and α-Bi2O3 nanosheets; wherein the α-Bi2O3 nanosheets grow vertically on the α-Bi2O3 nanorods, and the special homogeneous structure provides a larger specific surface area and more reaction sites, thereby improving the photocatalytic activity.
[0036] In a second aspect, the present invention provides a method for preparing an α-Bi2O3 / α-Bi2O3 homojunction photocatalyst, characterized in that the preparation method comprises: mixing a precursor solution with a surfactant, adding an acidic medium for reaction;
[0037] Wherein, the precursor is Bi2O3 nanorods.
[0038] The α-Bi2O3 / α-Bi2O3 homojunction photocatalyst of the present invention is prepared by mixing porous α-Bi2O3 nanorods as a precursor with a surfactant at room temperature (15-30°C), adding an acidic medium, and synthesizing the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst by simple stirring. The steps are simple, the reaction conditions are mild, the cost is low, and the process is green and environmentally friendly.
[0039] According to a preferred embodiment of the present invention, in order to make the α-Bi2O3 nanorods grown on the α-Bi2O3 nanorods thinner, the solvent of the precursor solution is selected from one or two or more of ethylene glycol, water, ethanol and isopropanol.
[0040] According to a preferred embodiment of the present invention, in order to make α-Bi2O3 nanosheets grow vertically and orderly on α-Bi2O3 nanorods, the surfactant is selected from one or two or more of cetyltrimethylammonium bromide, cetyltrimethylammonium chloride and dodecyltrimethylammonium bromide.
[0041] According to a preferred embodiment of the present invention, in order to etch the α-Bi2O3 nanorods, the acidic medium is nitric acid and / or sulfuric acid.
[0042] According to a preferred embodiment of the present invention, in order to make α-Bi2O3 nanosheets grow vertically and orderly on α-Bi2O3 nanorods, the mass ratio of the precursor to the surfactant is 1:0.5-2, for example, it can be 1:0.5, 1:1, 1:1.5 or 1:2.
[0043] According to a preferred embodiment of the present invention, in order to gradually etch the α-Bi2O3 nanorods, the molar concentration of the acidic medium is 10-75mmol / L, for example, it can be 10mmol / L, 15mmol / L, 20mmol / L, 25mmol / L, 30mmol / L, 35mmol / L, 40mmol / L, 45mmol / L, 50mmol / L, 55mmol / L, 60mmol / L, 65mmol / L, 70mmol / L or 75mmol / L.
[0044] According to a preferred embodiment of the present invention, in order to control the etching rate of α-Bi2O3 nanorods and ensure the vertical and uniform growth of α-Bi2O3 nanosheets, the reaction conditions include: temperature of 15-30°C, time of 10-30min, and stirring rate of 50-150rpm, for example, the temperature may be 15°C, time of 10min, and stirring rate of 50rpm; the temperature may be 20°C, time of 15min, and stirring rate of 100rpm; the temperature may be 25°C, time of 25min, and stirring rate of 120rpm, or the temperature may be 30°C, time of 30min, and stirring rate of 150rpm.
[0045] In a third aspect, the present invention provides an α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared by the preparation method described in the second aspect.
[0046] In a fourth aspect, the present invention provides an application of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst as described in the first aspect or the third aspect in the restoration of polluted water bodies.
[0047] The α-Bi2O3 / α-Bi2O3 homojunction photocatalyst of the present invention has excellent photocatalytic performance of catalytic reduction of hexavalent chromium [Cr(VI)] and degradation of bisphenol A, and has good photostability and reusability, and has broad application prospects.
[0048] In a fifth aspect, the present invention provides a method for reducing hexavalent chromium in polluted water, characterized in that the method comprises: mixing a photocatalyst with water containing hexavalent chromium, adjusting pH, adsorbing in the dark, and then irradiating with visible light;
[0049] Wherein, the photocatalyst is the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst described in the first aspect or the third aspect.
[0050] According to a preferred embodiment of the present invention, in order to enable the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst to better catalyze the degradation of Cr(VI), the concentration of the photocatalyst in the water body is 0.5-2 mg / mL, for example, it can be 0.5 mg / mL, 1 mg / mL, 1.5 mg / mL or 2 mg / mL.
[0051] According to a preferred embodiment of the present invention, in order to achieve adsorption-desorption equilibrium, the light-proof adsorption time is 20-40 minutes, preferably 30 minutes.
[0052] According to a preferred embodiment of the present invention, in order to completely degrade Cr(VI) by the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst, the irradiation conditions include: a time of 10-20 min, a light intensity of 80-100 mW / cm 2 For example, the time is 10 minutes and the light intensity is 80mW / cm 2 ; time is 15min, light intensity is 90mW / cm 2 Or the time is 20min, the light intensity is 100mW / cm 2 .
[0053] According to a preferred embodiment of the present invention, in order to completely degrade Cr(VI) by the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst, the visible light is provided by a xenon lamp and / or sunlight.
[0054] According to a preferred embodiment of the present invention, in order to achieve a higher efficiency in the degradation of Cr(VI) by the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst, the concentration of the hexavalent chromium is 50-150 mg / L.
[0055] In a sixth aspect, the present invention provides a method for degrading bisphenol A in polluted water, characterized in that the method comprises: mixing a photocatalyst with water containing bisphenol A, adjusting the pH, adsorbing in the dark, and then irradiating with visible light;
[0056] Wherein, the photocatalyst is the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst described in the first aspect or the third aspect.
[0057] According to a preferred embodiment of the present invention, in order to achieve a better sterilization effect, the concentration of the photocatalyst in the water body is 0.5-2 mg / mL.
[0058] According to a preferred embodiment of the present invention, in order to achieve adsorption-desorption equilibrium, the light-proof adsorption time is 20-40 minutes, preferably 30 minutes.
[0059] According to a preferred embodiment of the present invention, in order to completely degrade BPA by the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst, the irradiation conditions include: a time of 10-20 min, a light intensity of 80-100 mW / cm 2 For example, the time is 10 minutes and the light intensity is 80mW / cm 2 ; time is 15min, light intensity is 90mW / cm 2 Or the time is 20min, the light intensity is 100mW / cm 2 .
[0060] According to a preferred embodiment of the present invention, in order to completely degrade BPA by the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst, the visible light is provided by a xenon lamp and / or sunlight.
[0061] According to a preferred embodiment of the present invention, in order to achieve a higher efficiency in the degradation of BPA by the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst, the concentration of bisphenol A is 20 mg / L.
[0062] According to a preferred embodiment of the present invention, the room temperature is 15-30°C.
[0063] The present invention will be described in detail below by way of examples. In the following examples, the drugs and medicaments are all conventional commercial products.
[0064] Preparation Example 1
[0065] Bi(OHC2O4)·H2O was calcined at 400℃ for 3h to prepare Bi2O3 nanorods, denoted as NR-BO.
[0066] Example 1
[0067] 0.05g Bi2O3 nanorods were added to 16mL of a mixed solution of ethylene glycol and deionized water in a volume ratio of 1:1, and 0.05g of hexadecyltrimethylammonium bromide (CTAB) was used as a surfactant. At room temperature, the magnetic stirring rate was 100rpm, and 4mL of 144mmol / L nitric acid solution was added to make the concentration of nitric acid in the reaction system 28.8mmol / L. Stirring was continued for 30min, the obtained product was filtered, washed with deionized water to remove impurities, placed in an oven at 60℃, and dried for 4h to obtain α-Bi2O3 / α-Bi2O3 homojunction photocatalyst, recorded as BO-2.
[0068] Example 2
[0069] The method described in Example 1 was followed, except that when the concentration of the nitric acid solution in the reaction system was 14.4 mmol / L, an α-Bi2O3 / α-Bi2O3 homojunction photocatalyst was obtained, which was recorded as BO-1.
[0070] Example 3
[0071] The method described in Example 1 was followed, except that the concentration of the nitric acid solution was 72 mmol / L, to obtain an α-Bi2O3 / α-Bi2O3 homojunction photocatalyst, which was designated as BO-3.
[0072] Comparative Example 1
[0073] The method described in Example 1 was followed, except that when the concentration of the nitric acid solution in the reaction system was 288 mmol / L, Bi2O3 nanosheets were obtained, which were denoted as NS-BO.
[0074] Comparative Example 2
[0075] The method described in Example 1 was followed, except that "at room temperature" was replaced by "at 40°C", to obtain a product, which was recorded as BO-2 (40°C).
[0076] Comparative Example 3
[0077] The method described in Example 1 was followed, except that "at room temperature" was replaced by "at 60°C", to obtain a product, which was recorded as BO-2 (60°C).
[0078] Test Example 1
[0079] The α-Bi2O3 / α-Bi2O3 homojunction photocatalysts prepared in Examples 1-3, the Bi2O3 nanorods prepared in Preparation Example 1, and the Bi2O3 nanosheets prepared in Comparative Example 1 were subjected to X-ray diffraction (XRD) respectively. The XRD spectra are shown in FIG. Figure 1 shown.
[0080] Depend on Figure 1 It can be seen from the XRD spectrum that all diffraction peaks of the Bi2O3 nanorods prepared in Preparation Example 1 are precisely matched with the monoclinic α-Bi2O3 (JCPDS card number 71-2274), with high purity, and no obvious impurity peaks are observed. At the same time, under the conditions of different nitric acid concentrations, the diffraction peaks of the α-Bi2O3 / α-Bi2O3 homojunction photocatalysts prepared in Examples 1-3 and the Bi2O3 nanosheets prepared in Comparative Example 1 are consistent with the monoclinic α-Bi2O3 (JCPDS card number 71-2274). The results show that the α-Bi2O3 / α-Bi2O3 homojunction photocatalysts prepared in Examples 1-3 are completely composed of α-Bi2O3 and do not contain other components. Compared with other samples, the diffraction peaks of the Bi2O3 nanosheets prepared in Comparative Example 1 are significantly broadened, which can be attributed to its small crystal size.
[0081] Test Example 2
[0082] To further determine the structure of the product, the Bi2O3 nanorods prepared in Preparation Example 1, the α-Bi2O3 / α-Bi2O3 homojunction photocatalysts prepared in Examples 1-3, and the Bi2O3 nanosheets prepared in Comparative Example 1 were used as samples for scanning electron microscopy (SEM) analysis. The specific results are as follows: Figure 2 shown.
[0083] Depend on Figure 2a It can be seen that the Bi2O3 nanorods prepared in Preparation Example 1 present a porous nanorod-like structure;
[0084] Depend on Figure 2 It can be seen from bd that as the concentration of nitric acid increases from 14.4mmol / L to 72mmol / L, Bi2O3 nanosheets grow on the surface of Bi2O3 nanorods, and the density of nanosheets gradually increases. These results verify the successful synthesis of α-Bi2O3 nanosheets / α-Bi2O3 nanorod homojunctions. It is worth noting that these nanosheets grow almost vertically on the nanorods, providing a larger specific surface area and more reaction sites, thereby improving the photocatalytic activity;
[0085] Depend on Figure 2 e It can be seen that when the concentration of nitric acid exceeds 72mmol / L, the skeleton structure of Bi2O3 nanorods is destroyed and Bi2O3 nanosheets are generated.
[0086] Test Example 3
[0087] The product obtained in Comparative Example 2-3 was used as a sample and subjected to scanning electron microscopy (SEM) analysis. The specific results are as follows: Figure 3 shown.
[0088] Depend on Figure 3 It can be seen that the reaction temperature has an effect on the morphology of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst. Obviously, at 40°C and 60°C, the morphology of the synthesized α-Bi2O3 / α-Bi2O3 homojunction photocatalyst is not beautiful.
[0089] Test Example 4
[0090] In order to further determine the structure and element distribution of the product, the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 was used as a sample for transmission electron microscopy (TEM) and high-resolution transmission electron microscopy (HRTEM) analysis. The specific results are as follows: Figure 4 shown.
[0091] Depend on Figure 4 It can be seen from a that the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 is Bi2O3 nanosheets grown on the surface of Bi2O3 nanorods, which is consistent with the SEM image. Figure 4 In b, the high-resolution transmission electron microscopy (HRTEM) image at the interface shows different lattice fringes, with interplanar spacings of 0.448 and 0.314 nm corresponding to the (110) and (012) planes of Bi2O3, respectively. The lattice interface shows that α-Bi2O3 nanorods nucleate and grow epitaxially in a directional manner on α-Bi2O3 nanorods, thus forming a high-quality interface.
[0092] Test Example 5
[0093] The width of the band gap has an important influence on the optical properties of the material. For semiconductor materials, the width of the band gap determines their conductivity. When light is irradiated on a semiconductor material, electrons in the energy band are excited by photons into the conduction band to form free electrons and holes. This excitation phenomenon is called photoexcitation. The narrower the band gap, the lower the energy of the photoexcitation, which means that the material has a stronger ability to absorb visible light. Therefore, the width of the band gap determines the degree of absorption of visible light by the material. The Bi2O3 nanorods prepared in Preparation Example 1 and the Bi2O3 nanosheets prepared in Comparative Example 1 were used as samples for UV-visible diffuse reflectance analysis. The specific results are as follows: Figure 5 shown.
[0094] Depend on Figure 5 It can be seen from a that the absorption band edge of the Bi2O3 nanosheets prepared in Comparative Example 1 is about 500nm, and the absorption band edge of the Bi2O3 nanorods prepared in Preparation Example 1 is about 462nm. The band gap of the Bi2O3 nanosheets prepared in Comparative Example 1 is wider than the band gap of the Bi2O3 nanorods prepared in Preparation Example 1. Figure 5 b Calculated, the band gap value of the Bi2O3 nanorods prepared in Preparation Example 1 is 2.48 eV, and the band gap value of the Bi2O3 nanosheets prepared in Comparative Example 1 is 2.68 eV.
[0095] Test Example 6
[0096] The surface photovoltage (SPV) technique based on Kelvin probe force microscopy (KPFM) can directly present the charge separation characteristics at the interface of homogeneous / heterogeneous structures. Fig. 9 shown.
[0097] Depend on Fig. 9 It can be seen that under dark light conditions, in the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1, the surface potential of the Bi2O3 nanosheets is -5.5mV, and the surface potential of the Bi2O3 nanorods is 28.4mV, indicating that the Bi2O3 nanorods have a higher potential level than the Bi2O3 nanosheets; under the action of light, the surface potential of the Bi2O3 nanosheets drops to -57.7mV, and the surface potential of the Bi2O3 nanorods rises to 77.6mV, indicating that the photoelectrons are transferred from the Bi2O3 nanorods to the Bi2O3 nanosheets through the junction interface. Therefore, the photogenerated holes gather on the surface of the Bi2O3 nanorods, and the electrons gather on the surface of the Bi2O3 nanosheets. In contrast, after light irradiation, the surface potential difference on both sides of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst interface increases greatly, reaching 135.3mV. This significant potential change can be attributed to the strong interfacial electric field (IEF), which can effectively promote the transfer of photogenerated electrons and holes through the carrier channels (Bi-O-Bi) on the α-Bi2O3 / α-Bi2O3 homojunction interface.
[0098] Test Example 7
[0099] Using BO-2 prepared in Example 1 as a photocatalyst, a free radical capture experiment was carried out under simulated sunlight. The capture agents 1,4-benzoquinone (BQ), tert-butyl alcohol (TBA), ammonium oxalate (AO) and potassium iodate (KIO3) were used to capture O2 - , OH, holes (h + ) and electron (e - ), the result is as follows Fig.10 shown.
[0100] exist Fig.10 a, after adding BQ and KIO3 as scavengers, the photocatalytic performance of the α-Bi2O3 / α-Bi2O3 homojunction prepared in Example 1 was significantly inhibited. On the contrary, adding AO and TBA to the reaction system had no significant effect on the reduction of Cr(VI). It can be seen that ·O2 - and e - It is an important active substance in the photocatalytic reduction of Cr(VI). Fig.10 b It can be seen that ·O2 - and h + It is the key active substance for degrading BPA.
[0101] Depend on Fig.10 It can be seen that under dark conditions, the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 cannot produce ·OH and ·O2 - ; After 10 min of illumination, ·OH and ·O2 were observed - The corresponding obvious peaks indicate that the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 can generate sufficient ·OH and ·O2 under light. - Free radicals.
[0102] Through the KPFM test results of detection example 6 and the free radical capture experiment of detection example 7, we believe that the photocatalytic mechanism of α-Bi2O3 / α-Bi2O3 homojunction follows the Z-Scheme mechanism. Under simulated sunlight, photoelectrons are transferred from the conduction band of Bi2O3 nanorods to Bi2O3 nanosheets and recombine with holes on the valence band of Bi2O3 nanosheets, so that holes with higher potential are accumulated on Bi2O3 nanorods, while electrons with more negative potential are accumulated on Bi2O3 nanosheets. Electrons with more negative potential and·O2 - Free radicals participate in the photoreduction of Cr(VI), positive potential holes and O2 - Oxidized BPA.
[0103] Test Example 8
[0104] The Bi2O3 nanorods prepared in Preparation Example 1, the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 and the Bi2O3 nanosheets prepared in Comparative Example 1 were tested for N2 isothermal adsorption-desorption curves, and their BET specific surface areas were calculated, respectively. The results are shown in Table 1.
[0105] Table 1 Reaction rate constant k and apparent rate constant k1
[0106]
[0107]
[0108] The BET specific surface areas of NR-BO, BO-2 and NS-BO were calculated by N2 isotherm, and the results were 7.9617 m 2 / g, 25.4538m 2 / g and 43.8680m 2 / g, the reaction rate constants (k) of the three were normalized by BET specific surface area, and the apparent rate constant of BO-2 was obviously the largest. Therefore, we concluded that the excellent photocatalytic performance of BO-2 was attributed to the formed homogeneous structure rather than the BET specific surface area.
[0109] Application Example 1
[0110] At room temperature (25°C), 30 mg of the Bi2O3 nanorods prepared in Preparation Example 1, the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Examples 1-3, and the Bi2O3 nanosheets prepared in Comparative Example 1 were dispersed in 30 mL of Cr(VI) solution (50 mg / L), and an appropriate amount of citric acid was added to adjust the pH of the solution to 3. The suspension was stirred for 30 min in the dark to ensure the adsorption-desorption balance between the Cr(VI) solution and the photocatalyst; the light source (300 W Xe lamp) was turned on for irradiation, and an appropriate amount of the suspension was taken out every 1 min and centrifuged. The concentration of Cr(VI) in the supernatant was determined by UV-visible absorption spectroscopy, and the degradation rate of Cr(VI) was calculated. The degradation curve is shown in FIG. Figure 6 As shown in a.
[0111] Depend on Figure 6It can be seen that the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 exhibits excellent photocatalytic performance and can completely reduce 50 mg / L of Cr(VI) within 6 min, and its reducing ability is significantly stronger than other photocatalysts. Compared with the reported literature, the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 has excellent photocatalytic activity. As shown in Table 1, the reaction rate constant k for reducing Cr(VI) by the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 is 0.657 min -1 , which are 9.5 times and 1.3 times of the Bi2O3 nanorods prepared in Preparation Example 1 and the Bi2O3 nanosheets prepared in Comparative Example 1, respectively.
[0112] Application Example 2
[0113] The method described in Application Example 1 was used for implementation. The difference was that only the degradation rate of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 was tested for 30 mL, 50 mg / L Cr(VI) solution. The pH of the solution was adjusted to 2, 3, 5 and 7, respectively, and the degradation rate of Cr(VI) was calculated. The degradation curve is shown in Figure 6 As shown in b.
[0114] from Figure 6 It can be clearly seen in b that under neutral conditions (pH = 7), the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 has a stronger adsorption capacity for Cr(VI) than other pH conditions, but Cr(VI) can still be completely reduced after 15 minutes of illumination. As the pH decreases, the photoreduction time of Cr(VI) gradually shortens. Among them, when the pH is 2 and 3, the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 has the best reduction efficiency for Cr(VI).
[0115] Application Example 3
[0116] The method described in Application Example 1 was used for implementation. The difference was that the addition amounts of α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 were 15 mg and 60 mg respectively. The degradation rate of Cr(VI) was calculated. The degradation curve is shown in FIG. Figure 6 As shown in c.
[0117] Depend on Figure 6 c It can be seen that 50 mg / L Cr(VI) can be completely degraded within 3 min under the photocatalysis of 60 mg of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1, showing excellent photocatalytic performance.
[0118] Application Example 4
[0119] The method described in Application Example 1 was used, except that the concentrations of the Cr(VI) solutions were 100 mg / L and 150 mg / L, respectively. The degradation rate of Cr(VI) was calculated, and the degradation curve was as follows: Figure 6 As shown in d.
[0120] Depend on Figure 6 It can be seen from the figure that the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 has a removal rate of 80% for 150 mg / L Cr(VI) within 15 min. It can be seen that the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst still exhibits high photocatalytic activity for high concentrations of Cr(VI).
[0121] Comparative Example 4
[0122] The method described in Application Example 1 was used for implementation. The specific photocatalyst types, reaction conditions and reaction results are shown in Table 2.
[0123] Table 2 Comparison of photocatalytic reduction of Cr(VI) by different catalysts (Xe lamp, 300W)
[0124]
[0125]
[0126] It can be seen from Table 2 that, compared with other similar photocatalysts, the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 exhibits excellent photocatalytic performance towards Cr(VI).
[0127] Application Example 5
[0128] The method described in Application Example 1 was used to implement the experiment. The difference was that the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 was used to conduct 5 cycle experiments. The specific results are as follows: Figure 7 shown.
[0129] from Figure 7 a It can be seen that after 5 cycles of testing, the stability of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 is reliable and still exhibits excellent photocatalytic reduction ability for Cr(VI);
[0130] at the same time, Figure 7 b and Figure 7 The results of c effectively prove that the morphology and composition of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 have no obvious changes after the cycle test;
[0131] further, Figure 7d proves that after the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 photocatalytically reduced Cr(VI) (50 mg / L), all Cr(VI) was reduced to Cr(III).
[0132] Application Example 6
[0133] The method described in Application Example 1 was followed, except that "30 mL of Cr(VI) solution (50 mg / L)" was replaced with "30 mL of bisphenol A (BPA) (20 mg / L) solution", an appropriate amount of the suspension was taken out every 5 min and centrifuged, the concentration of bisphenol A in the supernatant was determined by UV-visible absorption spectroscopy, and the degradation rate of bisphenol A was calculated. The degradation curve is shown in FIG. Figure 8 shown.
[0134] like Figure 8 As shown, the degradation efficiency of α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 for BPA reaches 70% within 15 minutes, which is better than the Bi2O3 nanorods prepared in Preparation Example 1 and the Bi2O3 nanosheets prepared in Comparative Example 1. As shown in Table 1, the reaction rate constant k of α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 for BPA is 0.087 min -1 , which are 4.8 times and 1.27 times of those of Bi2O3 nanorods and Bi2O3 nanosheets, respectively.
[0135] Comparative Example 5
[0136] The method described in Application Example 6 was used for implementation. The specific photocatalyst types, reaction conditions and reaction results are shown in Table 3.
[0137] Table 3 Comparison of photocatalytic degradation of BPA by different catalysts (Xe lamp, 300W)
[0138]
[0139] It can be seen from Table 3 that, compared with other similar photocatalysts, the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared in Example 1 exhibits excellent photocatalytic performance towards BPA.
[0140] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0141] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0142] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. An α-Bi2O3 / α-Bi2O3 homojunction photocatalyst, characterized in that: The α-Bi2O3 / α-Bi2O3 homojunction photocatalyst comprises α-Bi2O3 nanorods and α-Bi2O3 nanosheets; wherein, The α-Bi2O3 nanosheets grow vertically on the α-Bi2O3 nanorods.
2. A method for preparing an α-Bi2O3 / α-Bi2O3 homojunction photocatalyst, characterized in that: The preparation method comprises: mixing a precursor solution with a surfactant, and adding an acidic medium to react; Wherein, the precursor is Bi2O3 nanorods.
3. The preparation method according to claim 2, characterized in that: The solvent of the precursor solution is selected from one or two or more of ethylene glycol, water, ethanol and isopropanol; Preferably, the surfactant is selected from one or two or more of cetyltrimethylammonium bromide, cetyltrimethylammonium chloride and dodecyltrimethylammonium bromide; More preferably, the acidic medium is nitric acid and / or sulfuric acid.
4. The preparation method according to claim 2 or 3, characterized in that: The mass ratio of the precursor to the surfactant is 1:0.5-2.
5. The preparation method according to any one of claims 2 to 4, characterized in that: The molar concentration of the acidic medium is 10-75 mmol / L.
6. The preparation method according to any one of claims 2 to 5, characterized in that: The reaction conditions include: temperature of 15-30° C., time of 10-30 min, and stirring rate of 50-150 rpm.
7. An α-Bi2O3 / α-Bi2O3 homojunction photocatalyst prepared by the preparation method as described in claims 2-6.
8. Use of the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst according to claim 1 or the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst according to claim 7 in the restoration of polluted water bodies.
9. A method for reducing hexavalent chromium in polluted water, characterized in that: The method comprises: mixing the photocatalyst with water containing hexavalent chromium, adjusting pH, adsorbing in the dark, and then irradiating with visible light; Wherein, the photocatalyst is the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst according to claim 1 or the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst according to claim 7; Preferably, the concentration of the photocatalyst in the water body is 0.5-2 mg / mL; Preferably, the light-proof adsorption time is 20-40 min, preferably 30 min; Preferably, the irradiation conditions include: time of 10-20 min, light intensity of 80-100 mW / cm 2 ; Preferably, the visible light is provided by a xenon lamp and / or sunlight; Preferably, the concentration of hexavalent chromium is 50-150 mg / L.
10. A method for degrading bisphenol A in polluted water, characterized in that: The method comprises: mixing the photocatalyst with water containing bisphenol A, adjusting the pH, adsorbing in the dark, and then irradiating with visible light; Wherein, the photocatalyst is the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst according to claim 1 or the α-Bi2O3 / α-Bi2O3 homojunction photocatalyst according to claim 7; Preferably, the concentration of the photocatalyst in the water body is 0.5-2 mg / mL; Preferably, the light-proof adsorption time is 20-40 min, preferably 30 min; Preferably, the irradiation conditions include: time of 10-20 min, light intensity of 80-100 mW / cm 2 ; Preferably, the visible light is provided by a xenon lamp and / or sunlight; Preferably, the concentration of bisphenol A is 20 mg / L.