Welding method of high-strength steel plate
By detecting the dilution rate of high-strength steel welded joints and calculating the target welding material composition, the problem of poor low-temperature impact toughness in welding high-strength steel thin plates is solved, and the performance of joints is improved after welding is achieved.
Patent Information
- Application Number
- CN202411238944.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-05
AI Technical Summary
The thin-specification double-sided submerged arc welding process of high strength steel has a high dilution rate, which leads to a decrease in the low-temperature impact toughness of the welded joints, and the performance of the weld zone is quite different from the mechanical properties of the welded metal of the matching welding material.
By welding the high-strength steel test plate, the dilution rate of the welded joint is detected, and the chemical element content of the target welding material is calculated based on the chemical element content of the test plate and the welded metal composition of the welding material, and re-welded using the target welding material. Ensure that the composition of the weld area after welding is consistent and improve the low-temperature impact toughness.
By accurately adjusting the composition of the welding material, we ensure that the performance of the joint after welding meets the technical requirements, and the low-temperature impact toughness of high-strength steel welded joints is significantly improved.
Smart Images

Figure CN118926656A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of high-strength steel welding, and in particular to a welding method for high-strength steel plates. Background Art
[0002] Compared with materials with ordinary strength levels, high-strength steel has smaller cross-sectional dimensions and lower quality, and is widely used in engineering machinery, building structures, marine engineering, energy, bridges and other fields. Submerged arc welding has the advantages of stable welding quality, high welding productivity, no arc light and little smoke, and is widely used in the field of high-strength steel welding.
[0003] At present, the dilution rate of double-sided submerged arc welding of thin-gauge high-strength steel is higher than that of multi-layer multi-pass welding. After welding with this double-sided submerged arc welding process, the performance of the joint weld zone obtained is quite different from the mechanical properties of the deposited metal of the matching welding material, especially the low-temperature impact toughness of the joint is seriously reduced. Summary of the invention
[0004] The present application provides a high-strength steel plate welding method to solve the following technical problem: how to improve the low-temperature impact toughness of high-strength steel welded joints.
[0005] In the present aspect, the present application provides a method for welding a high-strength steel plate, wherein the thickness of the high-strength steel is ≤20 mm, and the method comprises:
[0006] Welding at least two high-strength steel test plates using the current welding material to obtain a high-strength steel welded joint test plate;
[0007] Performing metallographic structure testing on the welded joint of the high-strength steel welded joint test plate to obtain the dilution rate of the welded joint;
[0008] Obtaining the chemical element content of the target welding material according to the chemical element content of the high-strength steel test plate, the chemical element content of the deposited metal of the current welding material, and the dilution rate;
[0009] The target welding material is used to weld at least two new high-strength steel test plates to obtain a target high-strength steel welded joint plate.
[0010] Optionally, the chemical element content of the target welding material satisfies the following relationship:
[0011] a=(b-η*c) / (1-η)
[0012] Where a represents the chemical element content of the target welding material, b represents the chemical element content of the deposited metal of the current welding material, c represents the chemical element content of the high-strength steel test plate, and η represents the dilution rate.
[0013] Optionally, obtaining the chemical element content of the target welding material according to the chemical element content of the high-strength steel test plate, the chemical element content of the deposited metal of the current welding material, and the dilution rate includes:
[0014] The chemical element content of the target welding material is obtained according to the chemical element content of the high-strength steel test plate, the chemical element content of the deposited metal of the current welding material and the dilution rate; wherein the chemical element content of the high-strength steel test plate and the chemical element content of the deposited metal of the current welding material are obtained by direct reading spectroscopy.
[0015] Optionally, the method of welding at least two high-strength steel test plates using the current welding material to obtain a high-strength steel welded joint sample plate includes:
[0016] Get the thickness of the high-strength steel test plate;
[0017] Obtaining welding heat input according to the thickness of the high-strength steel test plate;
[0018] Under the welding heat input condition, at least two of the high-strength steel test plates are welded using the current welding material to obtain a high-strength steel welded joint test plate.
[0019] Optionally, obtaining the welding heat input according to the thickness of the high-strength steel test plate includes:
[0020] If 5 mm ≤ the thickness of the high-strength steel test plate ≤ 10 mm, the welding heat input is 10 kJ / cm to 15 kJ / cm.
[0021] Optionally, obtaining the welding heat input according to the thickness of the high-strength steel test plate includes:
[0022] If 10mm<the thickness of the high-strength steel test plate≤20mm, the welding heat input is 16kJ / cm~35kJ / cm.
[0023] Optionally, the yield strength of the high-strength steel test plate is ≥460MPa.
[0024] Optionally, the chemical elements of the high-strength steel test plate include: C, Si, Mn, Ni, Mo, Cu, Nb, V and Ti.
[0025] Optionally, the groove form of the high-strength steel test plate includes one of the following: I-type and X-type.
[0026] Optionally, the target welding material includes one of the following: flux-cored welding wire and solid welding wire; wherein the diameter of the flux-cored welding wire is 3.2 mm to 5.0 mm.
[0027] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0028] The welding method of the high-strength steel plate provided in the embodiment of the present application uses the current welding material to weld the high-strength steel test plate to obtain the high-strength steel welded joint test plate; performs metallographic structure detection on the welded joint of the high-strength steel welded joint test plate to obtain the dilution rate of the welded joint; obtains the chemical element content of the target welding material according to the chemical element content of the high-strength steel test plate, the chemical element content of the deposited metal of the current welding material and the dilution rate; and re-welds the high-strength steel test plate with the target welding material to obtain the target high-strength steel welded joint plate. This method takes into account the dilution rate of the high-strength steel base material in the weld bead, and can obtain the chemical element content of the target welding material required in a high-dilution rate welding environment, thereby accurately ensuring that the composition of the weld zone after welding is consistent with the target composition, and the performance of the joint after welding meets the technical requirements, and finally improves the low-temperature impact toughness of the high-strength steel welded joint. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0030] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0031] Figure 1 A schematic diagram of a process for welding a high-strength steel plate provided according to some embodiments of the present application;
[0032] Figure 2 A schematic diagram of a "T"-shaped weld bead of a high-strength steel plate provided in accordance with Example 1 of the present application;
[0033] Figure 3 . Schematic diagram of an "X"-shaped weld bevel of a high-strength steel plate provided in Example 2 of the present application. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0035] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0036] In this application, the terms "including", "comprising", etc. mean "including but not limited to".
[0037] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0038] As the strength grade of materials increases, the composition system of high-strength steel and its matching welding materials becomes increasingly different. When the welding material is used for multi-layer and multi-pass welding or surfacing with a small dilution rate, the composition of the weld zone is not much different from the composition of the deposited metal, and the performance meets the welding requirements. However, under welding conditions with a large dilution rate, the proportion of the parent material component in the weld zone composition increases, and the obtained weld zone composition is greatly different from the selected welding material composition, and the performance cannot meet the welding requirements. Therefore, the present application provides a welding method for high-strength steel plates, Figure 1 A schematic diagram of a high-strength steel plate welding method provided according to some embodiments of the present application; see Figure 1 , the thickness of the high-strength steel is ≤20 mm, and the method comprises:
[0039] S1. Weld at least two high-strength steel test plates using the current welding material to obtain a high-strength steel welded joint test plate;
[0040] In some embodiments, the method of welding at least two high-strength steel test plates using the current welding material to obtain a high-strength steel welded joint test plate includes:
[0041] Get the thickness of the high-strength steel test plate;
[0042] Obtaining welding heat input according to the thickness of the high-strength steel test plate;
[0043] Under the welding heat input condition, at least two of the high-strength steel test plates are welded using the current welding material to obtain a high-strength steel welded joint test plate.
[0044] In some embodiments, obtaining the welding heat input according to the thickness of the high-strength steel test plate includes:
[0045] If 5 mm ≤ the thickness of the high-strength steel test plate ≤ 10 mm, the welding heat input is 10 kJ / cm to 15 kJ / cm.
[0046] In some embodiments, obtaining the welding heat input according to the thickness of the high-strength steel test plate includes:
[0047] If 10mm<the thickness of the high-strength steel test plate≤20mm, the welding heat input is 16kJ / cm~35kJ / cm.
[0048] In some embodiments, the groove form of the high-strength steel test plate includes one of the following: I-type and X-type.
[0049] In some embodiments, the yield strength of the high-strength steel test plate is ≥460 MPa.
[0050] In some embodiments, the chemical elements of the high-strength steel test plate include: C, Si, Mn, Ni, Mo, Cu, Nb, V and Ti.
[0051] In the embodiment of the present application, a high-strength steel welding test plate is prepared, a welding groove is opened, and a high-strength steel butt weld with a thickness of 5 to 20 mm is welded by a submerged arc welding process. According to the welding material selection principle of "equal strength matching", while considering that the low-temperature impact toughness of the welding material meets the use requirements, a suitable submerged arc welding material is selected. An "I"-shaped or "X"-shaped groove can be used to perform a double-sided submerged arc welding process with one pass on the front and back. This welding process has the advantages of high efficiency and stable welding quality. In order to ensure the welding quality and weld bead formation of the welded joint, the submerged arc welding process parameters are selected according to the plate thickness to ensure the mechanical properties of the weld bead. Exemplarily, if 5mm≤the thickness of the high-strength steel test plate≤10mm, the welding heat input may be 10kJ / cm, 11kJ / cm, 12kJ / cm, 13kJ / cm, 14kJ / cm, 15kJ / cm, etc.; if 10mm<the thickness of the high-strength steel test plate≤20mm, the welding heat input may be 16kJ / cm, 17kJ / cm, 18kJ / cm, 20kJ / cm, 22kJ / cm, 24kJ / cm, 25kJ / cm, 26kJ / cm, 28kJ / cm, 29kJ / cm, 30kJ / cm, 31kJ / cm, 32kJ / cm, 33kJ / cm, 34kJ / cm, 35kJ / cm, etc. The yield strength of the high-strength steel test plate may be ≥460MPa, and further, the yield strength of the high-strength steel test plate may be 460MPa to 690MPa. The chemical elements of the high-strength steel test plate may include: C, Si, Mn, Ni, Mo, Cu, Nb, V and Ti, and may also include N, B, Cr, etc.
[0052] S2. Performing metallographic structure testing on the welded joint of the high-strength steel welded joint test plate to obtain the dilution rate of the welded joint;
[0053] In an embodiment of the present application, the metallographic structure of the weld joint is taken, and a photograph of the weld morphology is obtained by etching. The area of the weld and the area of the high-strength steel material melted into the weld are obtained using image analysis software. The dilution rate of the joint under the welding process is calculated. The dilution rate = the area of the high-strength steel material melted into the weld / the area of the weld, which can be set as the ratio of the area of the melted base material of a single weld to the area of the molten pool of a single weld.
[0054] S3, obtaining the chemical element content of the target welding material according to the chemical element content of the high-strength steel test plate, the chemical element content of the deposited metal of the current welding material, and the dilution rate;
[0055] In some embodiments, the chemical element content of the target welding material satisfies the following relationship (1):
[0056] a=(b-η*c) / (1-η)
[0057] Where a represents the chemical element content of the target welding material, b represents the chemical element content of the deposited metal of the current welding material, c represents the chemical element content of the high-strength steel test plate, and η represents the dilution rate.
[0058] In some embodiments, obtaining the chemical element content of the target welding material according to the chemical element content of the high-strength steel test plate, the chemical element content of the deposited metal of the current welding material, and the dilution rate includes:
[0059] The chemical element content of the target welding material is obtained according to the chemical element content of the high-strength steel test plate, the chemical element content of the deposited metal of the current welding material and the dilution rate; wherein the chemical element content of the high-strength steel test plate and the chemical element content of the deposited metal of the current welding material are obtained by direct reading spectroscopy.
[0060] In the embodiment of the present application, the composition of the deposited metal refers to the composition of the welding material required for the high-strength steel, without considering the diluted welding material. This welding material itself meets the performance requirements, and the parent material composition is the chemical composition of the high-strength steel itself. Since the weld composition is diluted by the parent material under this process, the new welding material composition is redesigned. The chemical element content of the target welding material * (1-dilution rate) + the chemical element content of the high-strength steel * dilution rate = the chemical element content of the deposited metal of the current welding material, so after conversion, the chemical element content of the target welding material = (the chemical element content of the deposited metal of the current welding material - dilution rate * the chemical element content of the high-strength steel) / (1-dilution rate). Therefore, the spectral component detection equipment is used to obtain the chemical element content of the high-strength steel test plate and the chemical element content of the deposited metal of the current welding material, and the chemical element content of the target welding material is obtained according to the calculation formula (1). In addition, if the element content is calculated to be a negative number, the element content is set to 0.
[0061] S4. Use the target welding material to weld at least two new high-strength steel test plates to obtain a target high-strength steel welded joint plate.
[0062] In some embodiments, the target welding material includes one of the following: a flux-cored welding wire and a solid welding wire; wherein the diameter of the flux-cored welding wire is 3.2 mm to 5.0 mm.
[0063] In the embodiment of the present application, the target welding material can be one of a flux-cored welding wire and a solid welding wire. The manufacturing process of the flux-cored welding wire is to draw and manufacture the flux-cored welding wire by wrapping the flux powder in a carbon steel strip. The diameter of the flux-cored welding wire can be 3.2 mm, 3.5 mm, 3.8 mm, 4.0 mm, 4.5 mm, 5.0 mm, etc. The method obtains the required welding material composition in a high dilution rate welding environment by calculating the dilution rate, and can accurately ensure that the composition of the weld zone after welding is consistent with the target composition. The welding wire composition can be regulated by the flux-cored welding wire manufacturing process, and the performance of the joint after welding meets the technical requirements.
[0064] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0065] Example 1
[0066] Step 1: Prepare a 200*150*13mm EH550 marine steel welding test plate, with a welding current of 650A, a welding voltage of 30V, a welding heat input of 30kJ / cm, and an "I" type weld groove. After pairing, complete the double-sided submerged arc welding of the welding test plate;
[0067] Step 2: Take the metallographic structure of the welded joint, use 4% nitric acid alcohol etching solution to detect the cross section of the welded joint, and calculate the dilution rate of the joint under the welding process. The dilution rate of the welded joint is 62%; Figure 2 A schematic diagram of a "T"-shaped weld bead of a high-strength steel plate according to Example 1 of the present application is shown in FIG. Figure 2 The image area calculation software is used to obtain the weld area B, the melted base material areas A1 and A2 on both sides of the weld groove, and the joint dilution rate = (A1+A2) / B.
[0068] Step three, obtain the main chemical element content of the EH550 material and the matching welding material deposited metal by a direct reading spectrometer, and calculate the chemical element content of the target welding material = (chemical element content of the deposited metal of the current welding material-dilution rate*chemical element content of the high-strength steel test plate) / (1-dilution rate); please refer to the chemical element content of the target welding material provided in Example 1, the chemical element content of the deposited metal of the current welding material, and the chemical element content of the high-strength steel test plate shown in Table 1.
[0069] Table 1 Chemical element contents of target welding materials, chemical element contents of deposited metal of current welding materials and chemical element contents of high-strength steel test plates (wt%)
[0070] element C[%] Si[%] Mn[%] Cr[%] Cu[%] Mo[%] Nb[%] Ni[%] Ti[%] V[%] Deposited metal 0.090 0.22 1.37 0.15 0.16 0.46 0.006 0.76 0.005 0.007 High strength steel test plate 0.135 0.25 1.2 0 0.15 0.2 0.012 0.15 0.015 0.04 Required welding materials 0.02 0.17 1.65 0.39 0.17 0.88 0 1.76 0 0
[0071] Step 4: according to the chemical element content of the target welding material obtained in step 3, a flux-cored welding wire is produced, and the diameter of the welding wire is 4.0 mm;
[0072] Step 5: Double-sided submerged arc welding of EH550 material is performed using self-developed welding wire. The impact value of the joint weld area is excellent. Please refer to the KV2 impact value test results of the welding weld area of the high-strength steel plate provided in Example 1 shown in Table 2.
[0073] Table 2 KV2 impact value test results of the weld zone of high-strength steel plate
[0074]
[0075] Example 2
[0076] Step 1: Prepare a 200*150*20mm EH690 marine steel welding test plate, with a welding current of 700A, a welding voltage of 33V, a welding heat input of 35kJ / cm, and an "X" type weld groove. After pairing, complete the double-sided submerged arc welding of the welding test plate;
[0077] Step 2: Take the metallographic structure of the welded joint, use 4% nitric acid alcohol etching solution to detect the cross section of the welded joint, and calculate the dilution rate of the joint under the welding process. The dilution rate of the welded joint is 43%; Figure 3 For a schematic diagram of an "X"-shaped weld bead of a high-strength steel plate according to Example 2 of the present application, see Figure 3 The image area calculation software is used to obtain the weld area B, the melted base material areas A1 and A2 on both sides of the weld groove, and the joint dilution rate = (A1+A2) / B.
[0078] Step three, obtain the main chemical element content of the EH690 material and the matching welding material deposited metal by a direct reading spectrometer, and calculate the chemical element content of the target welding material = (chemical element content of the deposited metal of the current welding material-dilution rate*chemical element content of the high-strength steel test plate) / (1-dilution rate); please refer to the chemical element content of the target welding material provided in Example 2 shown in Table 3, the chemical element content of the deposited metal of the current welding material, and the chemical element content of the high-strength steel test plate.
[0079] Table 3 Chemical element contents of target welding materials, chemical element contents of deposited metal of current welding materials and chemical element contents of high-strength steel test plates (wt%)
[0080] element C[%] Si[%] Mn[%] Cr[%] Cu[%] Mo[%] Nb[%] Ni[%] Ti[%] V[%] Deposited metal 0.058 0.20 1.80 0.45 0.05 0.51 0.006 2.65 0.005 0.005 High strength steel test plate 0.10 0.25 1.20 0.5 0.25 0.45 0.02 1.00 0.015 0.05 Required welding materials 0.03 0.16 2.25 0.41 0 0.55 0 3.89 0 0
[0081] Step 4: according to the chemical element content of the target welding material obtained in step 3, a flux-cored welding wire is produced, and the diameter of the welding wire is 4.0 mm;
[0082] Step 5: Double-sided submerged arc welding of EH690 material is performed using self-developed welding wire. The impact value of the joint weld area is excellent. Please refer to the KV2 impact value test results of the welding weld area of the high-strength steel plate provided in Example 2 shown in Table 4.
[0083] Table 4 KV2 impact value test results of the weld zone of high-strength steel plate
[0084]
[0085] Comparative Example 1
[0086] Step 1: Prepare a 200*150*13mm EH550 marine steel welding test plate, with a welding current of 650A, a welding voltage of 30V, a welding heat input of 30kJ / cm, and an "I" type weld groove. After pairing, use the current welding material to complete double-sided submerged arc welding of the welding test plate;
[0087] Step 2: After welding, the components of the weld zone are diluted by the components of the parent material, and the impact performance of the weld center is shown in Table 5, and the impact value of the weld zone is greatly reduced. Please refer to the KV2 impact value test results of the weld zone of the high-strength steel plate provided in Comparative Example 1 shown in Table 5.
[0088] Table 5 KV2 impact value test results of high-strength steel plate weld zone
[0089]
[0090] In summary, it can be seen from Examples 1 to 2 and Comparative Example 1 that the welding method of the high-strength steel plate provided in the embodiments of the present application, combined with the dilution rate of the high-strength steel base material in the weld, can obtain the required target welding material chemical element content in a high dilution rate welding environment, thereby accurately ensuring that the composition of the weld zone after welding is consistent with the target composition, and the performance of the joint after welding meets the technical requirements, thereby ultimately improving the low-temperature impact toughness of the high-strength steel welded joint.
[0091] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A welding method for high-strength steel plates, It is characterized in that The thickness of the high-strength steel is ≤20 mm, and the method comprises: Welding at least two high-strength steel test plates using the current welding material to obtain a high-strength steel welded joint test plate; Performing metallographic structure testing on the welded joint of the high-strength steel welded joint test plate to obtain the dilution rate of the welded joint; Obtaining the chemical element content of the target welding material according to the chemical element content of the high-strength steel test plate, the chemical element content of the deposited metal of the current welding material, and the dilution rate; The target welding material is used to weld at least two new high-strength steel test plates to obtain a target high-strength steel welded joint plate.
2. The method according to claim 1, It is characterized in that The chemical element content of the target welding material satisfies the following relationship: a=(b-η*c) / (1-η) Where a represents the chemical element content of the target welding material, b represents the chemical element content of the deposited metal of the current welding material, c represents the chemical element content of the high-strength steel test plate, and η represents the dilution rate.
3. The method according to claim 1, It is characterized in that The step of obtaining the chemical element content of the target welding material according to the chemical element content of the high-strength steel test plate, the chemical element content of the deposited metal of the current welding material, and the dilution rate includes: The chemical element content of the target welding material is obtained according to the chemical element content of the high-strength steel test plate, the chemical element content of the deposited metal of the current welding material and the dilution rate; wherein the chemical element content of the high-strength steel test plate and the chemical element content of the deposited metal of the current welding material are obtained by direct reading spectroscopy.
4. The method according to claim 1, It is characterized in that The method of welding at least two high-strength steel test plates using the current welding material to obtain a high-strength steel welded joint test plate comprises: Get the thickness of the high-strength steel test plate; Obtaining welding heat input according to the thickness of the high-strength steel test plate; Under the welding heat input condition, at least two of the high-strength steel test plates are welded using the current welding material to obtain a high-strength steel welded joint test plate.
5. The method according to claim 4, It is characterized in that The step of obtaining welding heat input according to the thickness of the high-strength steel test plate comprises: If 5 mm ≤ the thickness of the high-strength steel test plate ≤ 10 mm, the welding heat input is 10 kJ / cm to 15 kJ / cm.
6. The method according to claim 4, It is characterized in that The step of obtaining welding heat input according to the thickness of the high-strength steel test plate comprises: If 10mm<the thickness of the high-strength steel test plate≤20mm, the welding heat input is 16kJ / cm~35kJ / cm.
7. The method according to claim 1, It is characterized in that The yield strength of the high-strength steel test plate is ≥ 460MPa.
8. The method according to claim 1, It is characterized in that The chemical elements of the high-strength steel test plate include: C, Si, Mn, Ni, Mo, Cu, Nb, V and Ti.
9. The method according to claim 1, It is characterized in that The groove forms of the high-strength steel test plate include the following: I-type and X-type.
10. The method according to claim 1, It is characterized in that The target welding material includes one of the following: flux-cored welding wire and solid welding wire; wherein the diameter of the flux-cored welding wire is 3.2 mm to 5.0 mm.
Citation Information
Patent Citations
Submerged-arc welding method for ultrahigh-strength steel plate F460Z for ocean structure
CN102049599A
Method for improving Super304H austenite corrosion-resisting steel weld joint and organization and performance thereof
CN106862797A
Dilution-rate-based low-phase-change-point welding material design method
CN111195786A
Method for rapidly and nondestructively determining surfacing welding dilution rate
CN112255180A
Chemical component design method for stainless steel submerged-arc welding wire of bimetal composite plate
CN113798641A
Cited By
Preparation method of welded joint, welding wire and welded joint
CN120839213A
Welding method of steel for flat car girder
CN122322626A