Lepidolite lithium extraction slag-based cementing material and preparation method thereof

By using lithium mica lithium slag powder combined with cement and anhydrous sodium sulfate, an efficient lithium mica lithium slag-based gelling material is generated, which solves the problems of low lithium slag utilization and environmental pollution, and achieves high-performance gelling material The industrialized production reduces costs and improves the comprehensive utilization rate of lithium slag.

CN118930081APending Publication Date: 2024-11-12GANZHOU NONFERROUS METALLURGICAL RES INST
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411090746.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, lithium mica extracting lithium waste slag has low utilization rate, complex preparation process, high environmental requirements, and the performance of lithium slag gelling materials is not enough to replace cement, which cannot effectively solve the problems of lithium slag storage pollution and smelting slag solid waste emissions. .

Method used

Lithium mica lithium slag powder, cement and anhydrous sodium sulfate as the main raw materials, and ettringite is generated through mechanical activation and chemical reactions, improving the compactness and strength of the cementitious material, and the mass percentage of lithium mica lithium slag powder and cement It is 50%~60%, and the anhydrous sodium sulfate is 3~6%. The process is simple and suitable for industrial production.

Benefits of technology

The high utilization rate of lithium mica extracted lithium slag-based gelling materials has been achieved, and the compressive strength is higher than standard cement, which reduces the proportion of cement, reduces production costs, and solves the problems of lithium slag storage pollution and smelting slag solid waste emissions. , increasing the ecological benefits and economic profits of enterprises.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930081A_ABST
    Figure CN118930081A_ABST
Patent Text Reader

Abstract

The invention discloses a lepidolite lithium extraction slag-based cementing material and a preparation method thereof, and belongs to the technical field of building materials. The lepidolite lithium extraction slag-based cementing material is prepared from lepidolite lithium extraction slag powder, cement and anhydrous sodium sulfate, and the preparation method comprises the following steps: carrying out ball milling on a lepidolite lithium extraction slag raw material, and uniformly mixing with the cement to obtain a lithium slag-cement system; and uniformly mixing the lithium slag-cement system with anhydrous sodium sulfate to obtain the lepidolite lithium extraction slag-based cementing material. According to the cementing material, the lepidolite lithium extraction slag is used as a main raw material, so that recycling, high-valued and reduction treatment of solid waste can be realized, the comprehensive utilization rate of the solid waste can be improved, the investment in the aspect of discharge management of the smelting slag solid waste can be reduced, and the industrial development requirements of national energy conservation, environmental protection and circular economy are highly met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a cementitious material, in particular to a lepidolite lithium extraction slag-based cementitious material and a preparation method thereof, belonging to the technical field of building materials. Background Art

[0002] With the continuous breakthroughs in new energy technologies, the lithium battery industry has developed rapidly, and the market demand for lithium mineral resources has continued to increase. In recent years, a wave of lithium mineral resource development and utilization has been formed. Spodumene and lithium mica are the main mineral resources for the production of lithium carbonate and lithium hydroxide. In my country, lithium mica mines are particularly widely distributed and have large resource reserves. After years of development and utilization, a large amount of lithium mica lithium extraction waste slag has been produced. According to statistics, 30 tons of lithium slag is produced for every ton of lithium carbonate produced. As of now, the amount of lithium slag in the country has reached hundreds of millions of tons. It is urgent to carry out research on the comprehensive utilization of lithium slag, explore new technologies and processes, provide more efficient, environmentally friendly and green comprehensive utilization methods, and broaden the channels for comprehensive utilization of lithium slag.

[0003] Cementitious materials, also known as binders, are widely used in the fields of construction and mine filling. Cement is currently the most commonly used cementitious material. According to statistics, the country consumes more than 2 billion tons of cement clinker each year, which does not take advantage of the "dual carbon" development goals, and the cost of cement is high. In terms of mine filling, practice shows that the cost of mine filling accounts for 1 / 3 to 2 / 3 of the mining cost, and the cost of filling cementitious materials accounts for more than 2 / 3 of the filling cost, which seriously compresses the profits of mining companies. Therefore, the development of low-cementitious materials using waste is the only way to improve the economic benefits of enterprises and achieve sustainable development.

[0004] The new cementitious material is a technological innovation of the existing filling materials, combining the progress of filling material technology with the comprehensive utilization of "three wastes". Using lithium slag from lithium mica as the raw material of cementitious materials to partially or completely replace cement can not only solve the environmental pollution problem caused by the large-scale storage of lithium slag on the surface, recycle and reduce the amount of smelting slag, and improve the comprehensive utilization rate of lithium slag, but also reduce the investment in the management of solid waste emissions from smelting slag. The productization of lithium slag-based cementitious materials can also add considerable ecological benefits and economic profits to enterprises.

[0005] A Chinese patent (publication number CN118125735A) discloses a method for preparing thallium-rich powder and cement cement powder by synergistically utilizing lithium slag and oil sludge. Highly active cementitious materials are prepared by using lithium slag and oil sludge resources through multiple grinding and calcination processes. However, its preparation process is complex (multiple calcinations) and the preparation environment requirements are high (different calcination temperature requirements each time, and the drying temperature is 90~180℃).

[0006] A Chinese patent (publication number CN117756487A) discloses a lithium slag cementitious material and its preparation method. The lithium slag cementitious material is mixed and stirred with cement, lithium slag, aggregate, water reducer, connector, basalt fiber, silica fume and water. However, the raw materials for preparation are of various types, the particle size of lithium slag is required to be high (4-6μm), and the preparation environment is high (reaction temperature is 60-120℃).

[0007] A Chinese patent (publication number CN117105554A) discloses a composite lithium slag-steel slag synergistic solid waste composite powder and its preparation method. Different types of lithium slag and steel slag are mixed, and under the mechanical force of the grinding disc and grinding roller, lithium slag-steel slag synergistic solid waste composite powder is obtained. However, the composite powder preparation uses steel slag as the main raw material (72%~82%) and various types of lithium slag as auxiliary materials (30%~20%), and the lithium slag utilization rate is not high.

[0008] Therefore, improving the utilization rate of lithium-extracting waste residue from lepidolite and preparing a gelling material with excellent performance are problems that technicians in this field need to solve urgently. Summary of the invention

[0009] In view of the shortcomings of the prior art, the first object of the present invention is to provide a lithium mica slag-based cementitious material with high utilization rate of lithium mica waste residue, simple composition and higher compressive strength than standard cement.

[0010] Another object of the present invention is to provide a method for preparing a lepidolite slag-based cementitious material, which has low raw material cost, simple process and is conducive to industrial production. In particular, the method uses lepidolite slag as the main raw material, which can not only solve the environmental pollution problem caused by large-scale storage of lithium slag, but also reduce the investment in smelting slag solid waste emission management, and obtain high-value-added cementitious materials, and can also add considerable ecological benefits and economic profits to enterprises.

[0011] In order to achieve the above technical objectives, the present invention provides a lithium-extracted lepidolite slag-based cementitious material, which is composed of the following components in parts by mass: 100 parts of lithium-extracted lepidolite slag powder and cement; 3 to 6 parts of anhydrous sodium sulfate; wherein the lithium-extracted lepidolite slag powder and cement are composed in a mass percentage of 50% to 60%: 50% to 40%.

[0012] The lithium-extracting slag powder of lepidolite contains a large proportion of silicon oxide, aluminum oxide and calcium oxide. After mechanical activation, these components can be stimulated by anhydrous sodium sulfate to chemically react with calcium oxide or calcium hydroxide in cement to generate ettringite (3CaO·AI2O3·3CaSO4·(30-32)H2O), which is a calcium aluminum sulfate mineral. When ettringite reacts with water, a colloidal substance is generated to fill the pores between the cementitious materials, thereby improving the density and strength of the cementitious materials. In the early stage, the filling effect of the ettringite is more obvious, thereby improving the early strength of the cementitious materials. In the later stage, the strengthening effect of the ettringite is more obvious, thereby improving the long-term strength of the cementitious materials.

[0013] When the proportion of lithium mica slag powder in the lithium mica slag-based cementitious material of the present invention reaches 60%, the consolidation strength of the cementitious material can still exceed the conventional standard cement strength (32.5MPa), while if the proportion of lithium mica slag powder is less than 50%, the cement dosage is too high, which will increase the cost of the cementitious material and reduce the practical application value. Anhydrous sodium sulfate is used as an activating material, and its activating activity on lithium mica slag powder is much higher than other conventional alkaline activators, such as sodium hydroxide, etc., and its dosage is too low to fully activate the lithium mica slag powder, and too high dosage will increase the cost of the cementitious material, and due to its strong corrosiveness, it is not convenient for production and maintenance of production equipment, which increases additional costs.

[0014] As a preferred solution, the main chemical composition and mass content of lithium slag powder extracted from lithium mica are: SiO2≥30%, Al2O3≥15%, CaO≥15%, and the remaining chemical components include SO3, Fe2O3, Na2O, F, K2O, MgO, etc.

[0015] As a preferred solution, the particle size of the lithium slag powder extracted from lepidolite satisfies D 97 =100~48μm. D 97 =100μm, which means that the mass of particles with a diameter less than 100μm accounts for 97%; D 97 =48μm means that the mass of particles with a diameter less than 48μm accounts for 97%. During the mechanical ball milling activation process of lithium mica slag, the activation activity of lithium mica slag increases with its D 97 The particle size gradually increases with the decrease of particle size, but its growth rate shows a gradually decreasing trend. 97 When the particle size reaches 48 μm, further ball milling of lithium-extracting lepidolite slag does not significantly increase its excitation activity, but instead increases the grinding cost, thereby increasing the production cost of the cementitious material.

[0016] As a preferred solution, the lithium-extraction slag-based cementitious material from lepidolite contains 5 to 6 parts by mass of anhydrous sodium sulfate.

[0017] The present invention also provides a method for preparing a lepidolite slag-based cementitious material, which comprises the following steps: S1: ball-milling the lithium-extraction slag raw material of lepidolite to obtain the lithium-extraction slag powder of lepidolite; S2: mixing lithium slag powder extracted from lepidolite with cement to obtain a lithium slag-cement system; S3: Evenly mix the lithium slag-cement system and anhydrous sodium sulfate to obtain a lithium-extracted lepidolite slag-based cementitious material.

[0018] As a preferred solution, the particle size of the lithium slag raw material from lithium mica is ≤2 mm. The lithium slag raw material from lithium mica is further ball-milled to an appropriate particle size and mechanically activated, which not only increases the specific surface area but also reduces the activation energy of the excitation, which is beneficial to the subsequent chemical excitation process.

[0019] As a preferred solution, the lithium slag-based cementitious material is mixed with water to form a slurry with a mass percentage concentration of 70% to 75%. The lithium slag-based cementitious material is slurried, solidified, and cured for 28 days, and the strength is greater than 32.5 MPa.

[0020] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects: (1) The lithium slag-based cementitious material of the present invention uses lithium slag from lithium mica as the main raw material, which can not only solve the environmental pollution problem caused by the large-scale storage of lithium slag on the surface, but also realize the resource utilization of lithium slag from lithium mica to obtain high-value-added lithium slag-based cementitious material products, which can add considerable ecological benefits and economic profits to enterprises.

[0021] (2) The utilization rate of lithium-extraction waste slag from lithium mica in the lithium-extraction waste slag-based cementitious material of the present invention is high, which greatly reduces the proportion of cement and is beneficial to reducing the cost of cementitious materials.

[0022] (3) The lithium-extracting slag-based cementitious material of the present invention still has high consolidation strength when the proportion of cement is low, and its compressive strength is higher than that of ordinary cement.

[0023] (4) The preparation method of the lithium mica slag-based cementitious material of the present invention requires few types of raw materials, is simple in process, has a short process flow, has low environmental requirements, and meets the requirements of industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The present invention provides a schematic diagram of the process flow for preparing lithium-extracting lepidolite slag-based cementitious material.

[0025] Figure 2 The present invention relates to an XRD spectrum of lithium-extracting waste residue from lepidolite. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] The cement involved in the following examples is commercially available standard cement.

[0028] The chemical composition and percentage content of the lithium slag in the following specific embodiments are respectively: SiO2 (32.38%), Al2O3 (17.59%), CaO (17.49%), SO3 (14.53%), Fe2O3 (4.77%), Na2O (3.64%), F (3.59%), K2O (3.35%), MgO (1.12%), MnO (0.46%), Rb2O (0.35%), P2O5 (0.17%), SrO (0.13), and others (0.43).

[0029] like Figure 1 , 2 As shown, a lithium-extracting slag-based gelling material of lepidolite and a preparation method thereof are carried out according to the following steps: S1: Take lithium slag with a particle size of ≤2mm as raw material, and obtain a particle size of D by ball milling. 97 =100~48μm (97% of the particles are smaller than 100μm and 97% are smaller than 48μm); S2: mixing lithium slag powder and cement evenly to obtain a lithium slag-cement system, wherein the mass ratios of lithium slag and cement are 50%-60% and 50%-40% respectively; S3: Based on the lithium slag-cement system in step S2, add an appropriate amount of anhydrous sodium sulfate activator and mix them evenly, wherein the amount of anhydrous sodium sulfate is 3% to 6%, and anhydrous sodium sulfate is an admixture; S4: Based on the material components in step 3, add an appropriate amount of water (the concentration of lithium slag-based cementitious material slurry is 70%-75%), mix and stir evenly to obtain lithium slag-based cementitious material slurry.

[0030] The present invention is further described below in conjunction with embodiments: In the following embodiments, unless otherwise specified, the operations described are routine operations in the art.

[0031] In the following examples, unless otherwise specified, the raw materials used can be obtained through conventional commercial channels.

[0032] The lithium slag-based gelling materials of Examples 1 to 7 were prepared by the following method: S1: Take lithium slag with a particle size of ≤2mm as raw material, and obtain a particle size of D by ball milling. 97 =48μm (97% of the particles are smaller than 48μm); S2: mixing lithium slag powder and cement evenly to obtain a lithium slag-cement system, wherein the mass ratio of lithium slag to cement is 50% each; S3: Based on the lithium slag-cement system in step S2, anhydrous sodium sulfate is added in amounts of 1%, 3%, 4%, 5%, 6%, 7% and 9% respectively to stimulate the lithium slag-cement system and mix them evenly; S4: Based on the material components in step 3, add an appropriate amount of water, mix and stir evenly to obtain a lithium slag-based gelling material with a slurry concentration of 74%; The composition ratios of the lithium-extracting lepidolite slag-based cementitious materials in Examples 1 to 7 are shown in Table 1.

[0033] The lithium slag-based gelling materials of Comparative Examples 1 to 6 were prepared considering the following factors: S1: Consider lithium slag powder D from lepidolite 97 Particle size effect; S2: Consider the influence of different stimulants; The distribution ratios of the groups of lithium-extracted lepidolite slag-based cementitious materials in Comparative Examples 1 to 6 are shown in Table 2.

[0034] The prepared lithium slag-based cementitious material slurry was sampled (φ50×100mm) using a mold. After mold repair, demolding and curing for 28 days, the compressive strength of the sample was determined by the "Test Method for Strength of Cement Mortar" (GB / T17671-2021). The final test results are shown in Tables 1 and 2.

[0035]

[0036]

[0037] From Table 1 and Table 2, it can be seen that the net slurry strength of lithium mica slag powder increases with its D 97 The particle size decreases and the growth rate gradually decreases (Comparative Examples 1-4). 97 =100~48μm, its net slurry strength is 0.52MPa~0.59MPa, too small D 97 The particle size increases the grinding cost of lithium slag from lepidolite, thereby increasing the preparation cost of the cementitious material. Therefore, the optimal particle size of the lithium slag powder from lepidolite of the present invention is D 97=100~48μm; based on the lithium slag-cement system, sodium hydroxide, sodium carbonate and anhydrous sodium sulfate are used to chemically excite it (Comparative Examples 5 and 6, Example 4), among which anhydrous sulfuric acid has the best excitation effect, and the strength of the cementitious material can reach 40.6MPa; the strength of the lithium mica slag-based cementitious material of the present invention increases first and then decreases with the increase of the anhydrous sodium sulfate dosage (Examples 1~7). When the anhydrous sodium sulfate dosage is 6%, the best strength is 43.7MPa. Excessive dosage of anhydrous sodium sulfate causes the needle-rod-shaped calcium aluminate to continuously extend and finally squeeze the pores, making the original space network skeleton unstable, and reducing the compressive strength of the cementitious material.

[0038] The lithium-extracting slag-based cementitious material comprises: lithium-extracting slag from lithium-extracting slag from lithium-extracting slag, cement, anhydrous sodium sulfate and water. The present invention uses common solid waste as the main raw material. The amount of cement and anhydrous sodium sulfate will affect the strength of the cementitious material, but the strength of the lithium-extracting slag-based cementitious material is greater than the standard strength of the benchmark cement (32.5MPa), that is, the lithium-extracting slag-based cementitious material realized by the present invention has better performance.

[0039] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the contents of the present invention's specification and drawings, or directly / indirectly applied in other related technical fields, are included in the patent protection scope of the present invention.

Claims

1. A lepidolite slag-based cementitious material, Features: It is composed of the following components by mass: 100 parts of lithium slag powder from lepidolite and cement; 3-6 parts of anhydrous sodium sulfate; The lithium slag powder extracted from lithium mica and cement are composed in a mass percentage of 50%~60%:50%~40%.

2. A lithium-extracting lepidolite slag-based cementitious material according to claim 1, Features: The particle size of the lithium slag powder extracted from lithium mica satisfies D 97 =100~48μm.

3. A lithium-extracting lepidolite slag-based cementitious material according to claim 1, Features: The main chemical composition and mass content of the lithium slag powder extracted from lepidolite are: SiO 2 ≥30%,Al 2 O 3 ≥15%,CaO≥15%.

4. A method for preparing a lithium-extracting lepidolite slag-based cementitious material according to claim 1, 2 or 3, Features: The following steps are involved: S1: ball-milling the lithium-extraction slag raw material of lepidolite to obtain the lithium-extraction slag powder of lepidolite; S2: mixing lithium slag powder extracted from lepidolite with cement to obtain a lithium slag-cement system; S3: Evenly mix the lithium slag-cement system and anhydrous sodium sulfate to obtain a lithium-extracted lepidolite slag-based cementitious material.

5. The method for preparing a lithium-extracting lepidolite slag-based cementitious material according to claim 4, Features: The particle size of the lithium-extracting lepidolite slag raw material is ≤2mm.

6. The method for preparing a lithium-extracting lepidolite slag-based cementitious material according to claim 4, Features: The lithium-extracting lepidolite slag-based gelling material is mixed with water to form a slurry with a mass percentage concentration of 70% to 75%.

Citation Information

Cited By

  • Lithium slag morphology regulation and control method and application

    CN119823598A

  • Secondary lithium extraction and resource utilization method of lithium extraction slag

    CN120776137A