High-toughness fireproof foaming polyurethane as well as preparation method and application thereof
By using technical means such as polymer polyols, crosslinked polystyrene and flame retardant composites and long-chain fatty acid modified oxide whiskers, foamed polyurethane has been solved in the flame retardant process, low toughness and high flue gas are solved. The problem of this problem is to achieve the preparation of high toughness and low smoke flame retardant materials, meeting the needs of automotive interiors and construction industries.
Patent Information
- Application Number
- CN202411125547.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing foamed polyurethanes have problems with low toughness and high flue gas during the flame retardant process, which is difficult to meet the demand for high toughness and low smoke flame retardant materials in the automotive interior and construction industries.
Using polymer polyols, crosslinked polystyrene and flame retardant composites, long-chain fatty acid modified oxide whiskers and specific amine catalysts, the specific preparation method and combination formula are used to form excellent flame retardant properties and Tough, high toughness, fire-resistant foamed polyurethane.
The high toughness and low smoke properties of foamed polyurethane are achieved, the amount of flame retardant and smoke density are reduced, and the comprehensive performance and environmental protection of the material are improved.
Smart Images

Figure BDA0004996287850000131
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of foamed polyurethane, and in particular relates to a high-toughness fireproof foamed polyurethane and a preparation method and application thereof. Background Art
[0002] Foamed polyurethane is a foam-like material formed by a foaming process. It is made of polyurethane material and has properties such as lightness, sound insulation, and heat preservation. These properties are derived from its unique pore structure. It plays an important role in many fields, such as furniture manufacturing, sound-absorbing materials in the construction industry, interior decoration of vehicles, and cushioning pads for sports equipment.
[0003] At present, polyurethane foam is mostly used as sound-absorbing material for automobile interior and construction industry. However, the molecular chain of polyurethane foam is a linear structure, which is relatively rigid, making it difficult for the material to effectively resist deformation when subjected to external force, thus showing poor toughness. In addition, during the foaming process, the foaming agent will leave many air holes in the material after evaporation. The softness of these holes will also be reduced, but this structure also makes the material easy to deform when subjected to external force, thus affecting its toughness.
[0004] CN117659488B provides a light-weight, high-toughness foaming material and its preparation method and application. The preparation method comprises the following steps: reacting amino silicone oil with double-ended epoxy polyether under solvent conditions to obtain a polyether cross-linked polysiloxane solution; adding polyisocyanate and polyether polyol to the polyether cross-linked polysiloxane solution, reacting under tertiary amine catalyst conditions to obtain a polyurethane-cross-linked polysiloxane composite solution, vacuum removing the organic solvent and granulating to obtain an organosilicon-modified polyurethane reinforcing masterbatch; mixing the obtained organosilicon-modified polyurethane reinforcing masterbatch with polyurethane rubber particles, flame retardant and foaming agent, and then extruding and foaming to obtain a light-weight, high-toughness polyurethane foaming material. In this technology, amino silicone oil is used to form a good three-dimensional reinforcement network in the final polyurethane matrix, which significantly improves the strength and toughness of the foamed material. However, the inventor found during the research process that although amino silicone oil can increase the toughness of polyurethane foam materials to a certain extent, the effect is not particularly significant, and the increase of amino silicone oil often increases the smoke of polyurethane foam materials during the flame retardant process. With the continuous advancement of technology and the continuous expansion of the market, its application prospects will be broader. At the same time, the performance requirements for foamed polyurethane are also getting higher and higher. Flame retardancy is a property pursued by foamed materials, and it is hoped to reduce the smoke content during the flame retardant process.
[0005] Therefore, there is an urgent need for a new high-toughness fire-resistant polyurethane foam, which not only has excellent toughness and flame retardancy, but also has low smoke during the flame retardant process, and can meet the requirements of sound-absorbing materials for automotive interiors and the construction industry. Summary of the invention
[0006] The object of the present invention is to provide a fireproof polyurethane foam with high toughness, and the polyurethane foam has excellent flame retardancy and toughness.
[0007] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a high-toughness fire-resistant foamed polyurethane. The raw materials of the high-toughness fire-resistant foamed polyurethane include, by weight: 100 parts of polymer polyol, 20-40 parts of a composite of cross-linked polystyrene and flame retardant, 1-5 parts of foam stabilizer, 0.5-3 parts of amine catalyst, 10-30 parts of long-chain fatty acid modified oxide whiskers, 5-10 parts of foaming agent, and 100-200 parts of isocyanate.
[0008] Furthermore, the raw materials of the high-toughness fire-resistant foamed polyurethane include, by weight: 100 parts of polymer polyol, 30-35 parts of a composite of cross-linked polystyrene and flame retardant, 1.5-2 parts of a foam stabilizer, 1-1.5 parts of an amine catalyst, 20-25 parts of long-chain fatty acid modified oxide whiskers, 6-7 parts of a foaming agent, and 120-150 parts of an isocyanate.
[0009] In the present invention, in order to better increase the comprehensive performance of the polyurethane foam in the present invention, further, the polymer polyol is selected from a combination of polyether polyol and polyester polyol, preferably in a weight ratio of (60-80): (20-40), preferably 70:30.
[0010] Furthermore, the polyether polyol is selected from polyether polyols based on sucrose and diols.
[0011] Furthermore, the hydroxyl value of the polyether polyol is 400-460 mgKOH / g.
[0012] The polyether polyol in the present invention can be obtained from the market, preferably I NOVOL R8243 polyether polyol purchased from Shandong I NOVOL New Materials Co., Ltd., which is a polyether polyol based on sucrose and diol and has a hydroxyl value of 430 mgKOH / g.
[0013] Furthermore, the polyester polyol is selected from phthalic anhydride polyester polyol.
[0014] Furthermore, the hydroxyl value of the phthalic anhydride polyester polyol is 305-325 mgKOH / g.
[0015] The phthalic anhydride polyester polyol in the present invention can be obtained from commercial products, and preferably is phthalic anhydride polyester polyol RAYNOL PS-3152, which has a hydroxyl value of 315 mgKOH / g.
[0016] In the system of the present invention, the interaction between polyether polyol and polyester polyol can form better pores, so that the foamed polyurethane product has excellent mechanical properties. At the same time, the addition of phthalic anhydride polyester polyol can also reduce the thermal conductivity of the product.
[0017] Furthermore, the preparation method of the composite of cross-linked polystyrene and flame retardant comprises the following steps:
[0018] S1: adding initiator AIBN, styrene, hydroxymethyl acrylamide and divinylbenzene to 3# aviation kerosene to obtain a reaction material;
[0019] S2: Take 1 / 4 to 1 / 3 of the weight of the reaction material and the flame retardant, mix them and heat them to 70-90°C to react for 40-60 minutes, then add the remaining reaction material dropwise, and control the addition to be completed within 2-3 hours. After the addition is completed, continue to react at 70-90°C for 1.5-2 hours, finally filter, and dry the solid phase to constant weight to obtain a composite of cross-linked polystyrene and flame retardant.
[0020] Furthermore, the mass of the initiator AIBN is 1-3wt% of the mass of styrene, preferably 1.2-1.5wt%.
[0021] Furthermore, the mass ratio of styrene, hydroxymethyl acrylamide and divinylbenzene is 1:(0.2-0.5):(0.1-0.2), preferably 1:(0.3-0.4):(0.12-0.15).
[0022] Furthermore, the mass ratio of the 3# aviation kerosene to styrene is (0.5-3):1, preferably (1.5-2):1.
[0023] Furthermore, the mass ratio of styrene to flame retardant is (0.1-0.5):1, preferably (0.3-0.35):1.
[0024] Furthermore, the flame retardant is selected from a combination of a metal hydroxide and a nitrogen-phosphorus flame retardant, and preferably the mass ratio of the metal hydroxide to the nitrogen-phosphorus flame retardant is 1:(2-3).
[0025] Furthermore, the metal hydroxide is selected from aluminum hydroxide and / or magnesium hydroxide, preferably aluminum hydroxide.
[0026] Furthermore, the average mesh size of the metal hydroxide is 2000-3000 mesh.
[0027] The metal hydroxides in the present invention can be obtained from commercial sources, for example, aluminum hydroxide can be purchased from Qinghe County Ruijiang Metal Materials Co., Ltd.
[0028] Furthermore, the nitrogen-phosphorus flame retardant is selected from at least one of Clariant's halogen-free flame retardant ExolitAP462, Solvay's phosphorus-nitrogen halogen-free flame retardant Amgard PA2 and Clariant's halogen-free flame retardant ExolitAP766, preferably Clariant's halogen-free flame retardant ExolitAP462.
[0029] In order to make foamed polyurethane have excellent fire resistance, but under the condition of achieving excellent flame retardant effect and reducing the amount of flame retardant, the foamed polyurethane produces a lot of smoke when used. The inventors of the present invention have found that the use of a specific cross-linked polystyrene and flame retardant composite in the present invention can not only achieve excellent flame retardant effect using a small amount of composite, but also the foamed polyurethane finally prepared has low smoke. In the absence of hydroxymethyl acrylamide in the experiment, the smoke of the foamed polyurethane increased during the combustion experiment. After the experiment, the inventors speculated that it may be because there are amino groups in the composite of cross-linked polystyrene and flame retardant, and the amino groups react with isocyanate and participate in the condensation reaction of polyurethane, so that the composite can be better dispersed in the polyurethane foaming system, increasing its flame retardancy, and the benzene ring structure increases the heat resistance of the polyurethane foam, which can increase the carbonization amount of the foam during the combustion process, thereby inhibiting the generation of smoke.
[0030] The foam stabilizer refers to a surfactant having the ability to prolong and stabilize the foam for a long time. Further, the foam stabilizer is selected from silicone foam stabilizers, preferably at least one of silicone foam stabilizer AK-8803, silicone foam stabilizer AK-8805, silicone foam stabilizer AK-8811 and silicone foam stabilizer AK-8832.
[0031] The amine catalyst is selected from at least one of N,N-bis(3-dimethylaminopropyl)-N-isopropanolamine, N,N-dimethylcyclohexylamine, pentamethyldiethyltriamine, dimethylaminoethoxyethanol and ethylenediamine.
[0032] Furthermore, the amine catalyst is selected from a mixture of N,N-dimethylcyclohexylamine and ethylenediamine, preferably the mass ratio of N,N-dimethylcyclohexylamine to ethylenediamine is 1:(2-5), preferably 1:(2.5-3).
[0033] In the present invention, the inventor unexpectedly discovered that the use of two catalysts, N,N-dimethylcyclohexylamine and ethylenediamine, can reduce the formaldehyde content in the product. Experimental speculation is that this may be because the synergistic effect of N,N-dimethylcyclohexylamine and ethylenediamine can make the reaction proceed more smoothly, reduce the multiple reaction, and thus reduce the content of impurities (such as formaldehyde).
[0034] Furthermore, the preparation method of the long-chain fatty acid modified oxide whiskers includes: mixing anhydrous ethanol, long-chain fatty acids, and oxide whiskers and oscillating them under ultrasound for 20-40 minutes, then filtering, washing the filter cake with anhydrous ethanol several times (for example, 2-3 times), and finally drying to obtain long-chain fatty acid modified oxide whiskers.
[0035] Furthermore, when preparing long-chain fatty acid modified oxide whiskers, the weight ratio of anhydrous ethanol, long-chain fatty acid and oxide whiskers is 1:(20-30):(0.5-0.8), preferably 1:25:0.65, and the anhydrous ethanol used does not include all the anhydrous ethanol used in washing.
[0036] Furthermore, the long-chain fatty acid is selected from C12-C18 long-chain fatty unsaturated carboxylic acids, preferably at least one of lauric acid, palmitic acid and stearic acid, and further preferably stearic acid.
[0037] Furthermore, the oxide whiskers are selected from at least one of magnesium oxide whiskers, manganese oxide whiskers and tetrapod-shaped zinc oxide whiskers, preferably tetrapod-shaped zinc oxide whiskers.
[0038] Furthermore, the average particle size of the four-needle zinc oxide whisker is 1500-3000 mesh, preferably 2000 mesh.
[0039] The four-needle zinc oxide whisker in the present invention can be obtained commercially, and is purchased from Qinghe County Chaotai Metal Materials Co., Ltd.
[0040] In the present invention, when preparing the long-chain fatty acid modified oxide whiskers, the washing method is a conventional method in the art and will not be elaborated herein.
[0041] Furthermore, when preparing the long-chain fatty acid modified oxide whiskers, the drying conditions are: drying at 50-60° C. for 8-10 hours.
[0042] In the present invention, the use of the long-chain fatty acid modified oxide whiskers in the present invention can better increase the toughness of the foamed polyurethane, which may be because the long chains in the long-chain fatty acid modified oxide whiskers can rotate freely, so that the entire foaming system has a certain toughness space. At the same time, the oxide whiskers modified by the long-chain fatty acids can increase the foaming ratio, reduce the density, and enhance the toughness of the foam. In addition, it is found in the study that when the oxide whiskers are four-needle zinc oxide whiskers, the toughness of the final foamed polyurethane is better, which may be because the special anisotropy of the four-needle zinc oxide whiskers can further increase the foaming ratio, and at the same time enable the foaming system to form a more delicate and uniform pore structure, so that the toughness will not be reduced while the foam strength is increased.
[0043] Furthermore, the foaming agent is a combination of cyclopentane and methyl formate, preferably with a weight ratio of 1:(0.2-0.6), and more preferably 1:(0.3-0.4).
[0044] Furthermore, the isocyanate is selected from at least one of diphenylmethane diisocyanate, polyphenyl polymethylene polyisocyanate, carbodiimide-modified diphenylmethane diisocyanate and polyphenyl polymethylene polyisocyanate, preferably polyphenyl polymethylene polyisocyanate (model: PM200 Wanhua polymer MDI).
[0045] The second aspect of the present invention provides a method for preparing the above-mentioned foamed polyurethane, comprising the following steps:
[0046] (1) Weigh each raw material by weight;
[0047] (2) Stirring the composite polymer polyol, the composite of polystyrene and flame retardant, foam stabilizer, amine catalyst, long-chain fatty acid modified oxide whisker, and foaming agent at 1000-1500 rpm for 40-60 minutes to obtain a mixture A;
[0048] (3) Stirring the mixture A and isocyanate at 2000-2500 rpm for 30-50 seconds to obtain a mixture B;
[0049] (4) Pour the mixed material B into a mold and allow it to foam statically, then perform a aging treatment and demold to obtain a foamed polyurethane.
[0050] Furthermore, the standing foaming time is 1-2 minutes; the aging treatment conditions are: aging at 105-115° C. for 1.5-2 hours.
[0051] The third aspect of the present invention provides the use of the foamed polyurethane of the present invention in automobile interior decoration and architectural sound-absorbing materials.
[0052] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0053] 1. The present invention can overcome the defect of low toughness of existing foamed polyurethane by using long-chain fatty acid-modified oxide whiskers, and can be used in automobile interiors and architectural sound-absorbing materials with good mechanical effects.
[0054] 2. The composite of polystyrene and flame retardant used in the present invention can achieve flame retardant effect with low energy consumption while reducing the dosage of active ingredients in the flame retardant, and can also reduce the smoke density of the foamed polyurethane product during the combustion and flame retardant process.
[0055] 3. In the present invention, the specific amine catalyst can promote the reaction to proceed smoothly, so that the prepared foamed polyurethane product has a very low formaldehyde content and has excellent environmental protection. DETAILED DESCRIPTION
[0056] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0057] Example 1
[0058] The present embodiment provides a high-toughness fire-resistant foamed polyurethane. The raw materials of the high-toughness fire-resistant foamed polyurethane include, by weight: 100 parts of polymer polyol, 32 parts of a compound of polystyrene and a flame retardant, 1.8 parts of a foam stabilizer, 1.2 parts of an amine catalyst, 25 parts of long-chain fatty acid-modified oxide whiskers, 7 parts of a foaming agent, and 130 parts of an isocyanate.
[0059] The polymer polyol is selected from a combination of polyether polyol and polyester polyol, with a weight ratio of 70:30; the polyether polyol is purchased from INOVOLR8243 polyether polyol of Shandong INOV New Materials Co., Ltd., which is a polyether polyol based on sucrose and diol with a hydroxyl value of 430 mgKOH / g;
[0060] The polyester polyol is phthalic anhydride polyester polyol RAYNOLPS-3152, and its hydroxyl value is 315 mgKOH / g;
[0061] The preparation method of the composite of cross-linked polystyrene and flame retardant comprises:
[0062] S1: Initiator AIBN, styrene, hydroxymethyl acrylamide and divinyl benzene are added to 3# aviation kerosene to obtain a reaction material; S2: 1 / 3 weight of the reaction material is mixed with the flame retardant and heated to 80°C for reaction for 50 minutes, and then the remaining reaction material is added dropwise, and the addition is completed within 2.5 hours. After the addition is completed, the reaction is continued at 80°C for 2 hours, and finally filtered and the solid phase is dried to constant weight to obtain a composite of cross-linked polystyrene and flame retardant;
[0063] The mass of initiator AIBN is 1.3wt% of the mass of styrene; the mass ratio of styrene, hydroxymethyl acrylamide and divinylbenzene is 1:0.32:0.15; the mass ratio of 3# aviation kerosene to styrene is 1.8:1; the mass ratio of styrene to flame retardant is 0.32:1; the flame retardant is selected from a combination of metal hydroxide and nitrogen-phosphorus flame retardant, and the mass ratio of metal hydroxide to nitrogen-phosphorus flame retardant is 1:2.5; the metal hydroxide is aluminum hydroxide, with an average mesh size of 200 mesh, purchased from Qinghe County Ruijiang Metal Materials Co., Ltd.; the nitrogen-phosphorus flame retardant is Clariant's halogen-free flame retardant ExolitAP462;
[0064] The foam stabilizer is silicone foam stabilizer AK-8803;
[0065] The amine catalyst is a mixture of N,N-dimethylcyclohexylamine and ethylenediamine; the mass ratio of N,N-dimethylcyclohexylamine to ethylenediamine is 1:2.8;
[0066] The preparation method of long-chain fatty acid modified oxide whiskers comprises: mixing anhydrous ethanol, long-chain fatty acid and oxide whiskers, oscillating under ultrasonic wave for 30 minutes, filtering, washing the filter cake with anhydrous ethanol for 3 times, and finally drying to obtain long-chain fatty acid modified oxide whiskers;
[0067] When preparing the long-chain fatty acid modified oxide whiskers, the weight ratio of the anhydrous ethanol, the long-chain fatty acid, and the oxide whiskers is 1:25:0.65; the long-chain fatty acid is stearic acid; the oxide whiskers are four-needle zinc oxide whiskers with an average particle size of 2000 mesh, purchased from Qinghe Chaotai Metal Materials Co., Ltd.; when preparing the long-chain fatty acid modified oxide whiskers, the drying conditions are: drying at 60°C for 8 hours;
[0068] The blowing agent is a combination of cyclopentane and methyl formate, with a weight ratio of 1:0.35;
[0069] The isocyanate is polyphenyl polymethylene polyisocyanate (model: PM200 Wanhua Polymerization MDI);
[0070] The preparation method of foamed polyurethane is:
[0071] (1) Weigh each raw material by weight;
[0072] (2) stirring a composite polymer polyol, a composite of polystyrene and a flame retardant, a foam stabilizer, an amine catalyst, a long-chain fatty acid modified oxide whisker, and a foaming agent at 1200 rpm for 60 minutes to obtain a mixture A;
[0073] (3) Mixture A and isocyanate were stirred at 2000 rpm for 35 seconds to obtain mixture B;
[0074] (4) Mixture B was poured into a mold and allowed to stand for foaming for 1 minute, then aged at 110° C. for 2 hours, and demolded to obtain foamed polyurethane.
[0075] Example 2
[0076] The present embodiment provides a high-toughness fire-resistant foamed polyurethane. The raw materials of the high-toughness fire-resistant foamed polyurethane include, by weight: 100 parts of polymer polyol, 35 parts of a composite of polystyrene and a flame retardant, 2 parts of a foam stabilizer, 1 part of an amine catalyst, 25 parts of long-chain fatty acid-modified oxide whiskers, 6 parts of a foaming agent, and 120 parts of an isocyanate.
[0077] The polymer polyol is selected from a combination of polyether polyol and polyester polyol, with a weight ratio of 60:40; the polyether polyol is purchased from I NOVOL R8243 polyether polyol of Shandong I NOVOL New Materials Co., Ltd., which is a polyether polyol based on sucrose and diol with a hydroxyl value of 430 mgKOH / g;
[0078] The polyester polyol is phthalic anhydride polyester polyol RAYNOL PS-3152, and its hydroxyl value is 315 mgKOH / g;
[0079] The preparation method of the composite of cross-linked polystyrene and flame retardant comprises: S1 adding initiator AI BN, styrene, hydroxymethyl acrylamide and divinyl benzene to 3# aviation kerosene to obtain a reaction material; S2 taking 1 / 3 weight of the reaction material and mixing it with the flame retardant, heating it to 70°C and reacting it for 60 minutes, then dripping the remaining reaction material, controlling the dripping to be completed within 3 hours, continuing to react at 90°C for 1.5 hours after the dripping is completed, finally filtering, and drying the solid phase to constant weight to obtain the composite of cross-linked polystyrene and flame retardant;
[0080] The mass of the initiator AI BN is 1.5wt% of the mass of styrene; the mass ratio of styrene, hydroxymethyl acrylamide and divinyl benzene is 1:0.4:0.15; the mass ratio of 3# aviation kerosene to styrene is 2:1; the mass ratio of styrene to flame retardant is 0.35:1; the flame retardant is selected from a combination of metal hydroxide and nitrogen-phosphorus flame retardant, and the mass ratio of metal hydroxide to nitrogen-phosphorus flame retardant is 1:2; the metal hydroxide is aluminum hydroxide, with an average mesh size of 200 mesh, purchased from Qinghe County Ruijiang Metal Materials Co., Ltd.; the nitrogen-phosphorus flame retardant is Clariant's halogen-free flame retardant Exo lit AP 462;
[0081] The foam stabilizer is silicone foam stabilizer AK-8832;
[0082] The amine catalyst is selected from a mixture of N,N-dimethylcyclohexylamine and ethylenediamine; the mass ratio of N,N-dimethylcyclohexylamine to ethylenediamine is 1:3;
[0083] The preparation method of long-chain fatty acid modified oxide whiskers comprises: mixing anhydrous ethanol, long-chain fatty acid and oxide whiskers, oscillating under ultrasonic wave for 20 minutes, filtering, washing the filter cake with anhydrous ethanol for 3 times, and finally drying to obtain long-chain fatty acid modified oxide whiskers;
[0084] When preparing long-chain fatty acid modified oxide whiskers, the weight ratio of anhydrous ethanol, long-chain fatty acid and oxide whiskers is 1:20:0.5; the long-chain fatty acid is stearic acid; the oxide whiskers are four-needle zinc oxide whiskers with an average particle size of 2000 mesh, purchased from Qinghe Chaotai Metal Materials Co., Ltd.; when preparing long-chain fatty acid modified oxide whiskers, the drying conditions are: drying at 60°C for 8 hours;
[0085] The blowing agent is a combination of cyclopentane and methyl formate, with a weight ratio of 1:0.3;
[0086] The isocyanate is polyphenyl polymethylene polyisocyanate (model: PM200 Wanhua Polymerization MDI);
[0087] The preparation method of foamed polyurethane is:
[0088] (1) Weigh each raw material by weight;
[0089] (2) stirring a composite polymer polyol, a composite of polystyrene and a flame retardant, a foam stabilizer, an amine catalyst, a long-chain fatty acid modified oxide whisker, and a foaming agent at 1500 rpm for 40 minutes to obtain a mixture A;
[0090] (3) Mixture A and isocyanate were stirred at 2500 rpm for 50 seconds to obtain mixture B;
[0091] (4) Pour the mixed material B into a mold and let it stand for foaming for 2 minutes, then age it at 115° C. for 2 hours and demold it to obtain a foamed polyurethane.
[0092] Comparative Example 1
[0093] The difference between this comparative example and Example 1 is that the preparation method of the composite of cross-linked polystyrene and flame retardant comprises: S1 adding initiator AI BN, styrene and divinylbenzene to 3# aviation kerosene to obtain a reaction material; S2 taking 1 / 3 of the weight of the reaction material and the flame retardant, mixing the mixture and heating to 80°C for reaction for 50 minutes, then dripping the remaining reaction material, controlling the dripping to be completed within 2.5 hours, continuing to react at 80°C for 2 hours after the dripping is completed, finally filtering, and drying the solid phase to constant weight to obtain a composite of cross-linked polystyrene and flame retardant; the mass of initiator AI BN is 1.3wt% of the mass of styrene; the mass ratio of styrene to divinylbenzene is 1:0.15; the mass ratio of 3# aviation kerosene to styrene is 1.8:1; the mass ratio of styrene to flame retardant is 0.32:1;
[0094] The flame retardant is selected from a combination of metal hydroxide and nitrogen-phosphorus flame retardant, and the mass ratio of metal hydroxide to nitrogen-phosphorus flame retardant is 1:2.5; the metal hydroxide is aluminum hydroxide, with an average mesh size of 200 meshes, purchased from Qinghe County Ruijiang Metal Materials Co., Ltd.; the nitrogen-phosphorus flame retardant is Clariant's halogen-free flame retardant Exol it AP 462.
[0095] Comparative Example 2
[0096] The difference between this comparative example and Example 1 is that a combination of a metal hydroxide and a nitrogen-phosphorus flame retardant in a mass ratio of 1:2.5 is used to replace the cross-linked polystyrene and the flame retardant; the metal hydroxide is aluminum hydroxide with an average mesh size of 200 meshes, which is purchased from Qinghe County Ruijiang Metal Materials Co., Ltd.; the nitrogen-phosphorus flame retardant is Clariant's halogen-free flame retardant Exo lit AP 462.
[0097] Comparative Example 3
[0098] The difference between this comparative example and Example 1 is that four-needle zinc oxide whiskers with an average particle size of 2000 mesh purchased from Qinghe Chaotai Metal Materials Co., Ltd. are used to replace the long-chain fatty acid modified oxide whiskers.
[0099] Comparative Example 4
[0100] The difference between this comparative example and Example 1 is that aluminum oxide crystals with an average particle size of 2000 mesh are used to replace the four-needle zinc oxide whiskers, which are purchased from Qinghe Chaotai Metal Materials Co., Ltd.
[0101] Comparative Example 5
[0102] The difference between this comparative example and Example 1 is that the amine catalyst is N,N-dimethylcyclohexylamine.
[0103] Comparative Example 6
[0104] The difference between this comparative example and Example 1 is that the amine catalyst is ethylenediamine
[0105] Performance Testing
[0106] The following performance tests were performed on the foamed polyurethanes in Examples 1-2 and Comparative Examples 1-6 respectively:
[0107] 1. Determination of oxygen index: refer to ASTM D2863 standard.
[0108] 2. Determination of smoke density: refer to GB / T8323.2-2008 standard.
[0109] 3. 50% static compression strength: refer to GB / T 8813-2008 standard.
[0110] 3. Formaldehyde content test: refer to TS-BD-003 standard.
[0111] The test results are shown in Table 1:
[0112] 1Performance Test Results
[0113]
[0114] It can be seen from the above performance test results that the foamed polyurethane products in Examples 1-2 are excellent in flame retardancy, low smoke resistance, toughness (i.e., 50% static compression strength) and environmental protection, and especially the comprehensive performance of Example 1 is more excellent. According to the experimental results, it is speculated that this is because the long-chain fatty acid modified oxide whiskers in the specific foaming system of the present invention can overcome the defect of low toughness of the existing foamed polyurethane, and the use of a composite of polystyrene and flame retardant can achieve energy-saving flame retardant effect while reducing the amount of effective ingredients in the flame retardant, and can also reduce the smoke density of the foamed polyurethane product during the combustion and flame retardant process. The specific amine catalyst can promote the reaction to proceed smoothly, thereby making the prepared foamed polyurethane product have a very low formaldehyde content.
[0115] However, the comparative example did not adopt the necessary technical solution, resulting in that it was significantly worse than the embodiment in the corresponding performance test. In comparative example 1, when hydroxymethyl acrylamide was not added when preparing the composite of polystyrene and flame retardant, the smoke of the foamed polyurethane increased during the combustion experiment. This may be because when hydroxymethyl acrylamide was not added when preparing the composite of polystyrene and flame retardant, the composite of polystyrene and flame retardant could not react with isocyanate better, and the increase in carbonization was limited; further, when the flame retardant was directly used in the comparative example, its flame retardant effect was low, and the smoke during the combustion experiment was very high, proving that the composite of cross-linked polystyrene and flame retardant can reduce the smoke of foamed polyurethane during combustion; in comparative example 3, long-chain fatty acid modification was not used. The oxide whiskers will affect the 50% static compression strength of the foamed polyurethane, which proves that in the overall scheme of the present invention, the use of long-chain fatty acid-modified oxide whiskers can increase the toughness of the foamed polyurethane; in Comparative Example 4, four-needle oxide whiskers are not used, and other oxide whiskers are used, and the 50% static compression strength of the foamed polyurethane is lower than the toughness when the four-needle oxide whiskers are used; in Comparative Examples 5-6, the formaldehyde content of the foamed polyurethanes prepared by using a single N,N-dimethylcyclohexylamine or ethylenediamine is higher than that by using N,N-dimethylcyclohexylamine or ethylenediamine at the same time, which proves that in the present invention, N,N-dimethylcyclohexylamine and ethylenediamine can have a catalytic synergistic effect, reduce the occurrence of side reactions in the system, and make the foamed polyurethane have a low formaldehyde content.
[0116] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A high-toughness fire-resistant polyurethane foam, characterized in that: The raw materials of the high-toughness fire-resistant foamed polyurethane include, by weight: 100 parts of polymer polyol, 20-40 parts of a composite of cross-linked polystyrene and flame retardant, 1-5 parts of a foam stabilizer, 0.5-3 parts of an amine catalyst, 10-30 parts of long-chain fatty acid modified oxide whiskers, 5-10 parts of a foaming agent, and 100-200 parts of an isocyanate.
2. The high-toughness fire-resistant polyurethane foam according to claim 1, characterized in that: The polymer polyol is selected from a combination of polyether polyol and polyester polyol, and the weight ratio thereof is (60-80): (20-40).
3. The high-toughness fire-resistant polyurethane foam according to claim 2, characterized in that: The polyether polyol is selected from polyether polyols based on sucrose and diols; the hydroxyl value of the polyether polyol is 400-460 mgKOH / g; The polyester polyol is selected from phthalic anhydride polyester polyol; the hydroxyl value of the phthalic anhydride polyester polyol is 305-325 mgKOH / g.
4. The high-toughness fire-resistant polyurethane foam according to any one of claims 1 to 3, characterized in that: The preparation method of the composite of cross-linked polystyrene and flame retardant comprises: S1: adding initiator AIBN, styrene, hydroxymethyl acrylamide and divinylbenzene to 3# aviation kerosene to obtain a reaction material; S2: Take 1 / 4 to 1 / 3 of the weight of the reaction material and the flame retardant, mix them and heat them to 70-90°C to react for 40-60 minutes, then add the remaining reaction material dropwise, and control the addition to be completed within 2-3 hours. After the addition is completed, continue to react at 70-90°C for 1.5-2 hours, finally filter, and dry the solid phase to constant weight to obtain a composite of cross-linked polystyrene and flame retardant.
5. The high-toughness fire-resistant polyurethane foam according to claim 4, characterized in that: The mass of the initiator AIBN is 1-3% of the mass of styrene; the mass ratio of styrene, hydroxymethyl acrylamide and divinylbenzene is 1:(0.2-0.5):(0.1-0.2); the mass ratio of 3# aviation kerosene to styrene is (0.5-3):1; the mass ratio of styrene to flame retardant is (0.1-0.5):1, preferably (0.3-0.35):
1.
6. The high-toughness fire-resistant polyurethane foam according to claim 4, characterized in that: The flame retardant is selected from a combination of a metal hydroxide and a nitrogen-phosphorus flame retardant, and the mass ratio thereof is 1:(2-3); the metal hydroxide is selected from aluminum hydroxide and / or magnesium hydroxide; the average mesh size of the metal hydroxide is 2000-3000 mesh; the nitrogen-phosphorus flame retardant is selected from at least one of Clariant's halogen-free flame retardant Exol it AP 462, Solvay's phosphorus-nitrogen halogen-free flame retardant Amgard PA2 and Clariant's halogen-free flame retardant ExolitAP 766.
7. The high-toughness fire-resistant polyurethane foam according to any one of claims 1 to 3, characterized in that: The foam stabilizer is selected from silicone foam stabilizers, preferably at least one of silicone foam stabilizer AK-8803, silicone foam stabilizer AK-8805, silicone foam stabilizer AK-8811 and silicone foam stabilizer AK-8832; the amine catalyst is selected from at least one of N,N-bis(3-dimethylaminopropyl)-N-isopropanolamine, N,N-dimethylcyclohexylamine, pentamethyldiethyltriamine, dimethylaminoethoxyethanol and ethylenediamine; the isocyanate is selected from at least one of diphenylmethane diisocyanate, polyphenyl polymethylene polyisocyanate, carbodiimide-modified diphenylmethane diisocyanate and polyphenyl polymethylene polyisocyanate.
8. The high-toughness fire-resistant polyurethane foam according to any one of claims 1 to 3, characterized in that: The preparation method of the long-chain fatty acid modified oxide whisker comprises: mixing anhydrous ethanol, long-chain fatty acid and oxide whisker, oscillating under ultrasonic wave for 20-40 minutes, filtering, washing the filter cake with anhydrous ethanol for several times, and finally drying to obtain the long-chain fatty acid modified oxide whisker; when preparing the long-chain fatty acid modified oxide whisker, the weight ratio of the anhydrous ethanol, long-chain fatty acid and oxide whisker is 1: (20-30): (0.5-0.8); the long-chain fatty acid is selected from the long-chain fatty unsaturated carboxylic acid of C12-C18; the oxide whisker is selected from at least one of magnesium oxide whisker, manganese oxide whisker and four-needle zinc oxide whisker.
9. A method for preparing the high-toughness fire-resistant foamed polyurethane according to any one of claims 1 to 8, characterized in that: The steps include: (1) Weigh each raw material by weight; (2) Stirring the composite polymer polyol, the composite of polystyrene and flame retardant, foam stabilizer, amine catalyst, long-chain fatty acid modified oxide whisker, and foaming agent at 1000-1500 rpm for 40-60 minutes to obtain a mixture A; (3) Stirring the mixture A and isocyanate at 2000-2500 rpm for 30-50 seconds to obtain a mixture B; (4) Pour the mixed material B into a mold and allow it to foam statically, then perform a aging treatment and demold to obtain a foamed polyurethane.
10. Use of the high-toughness fire-resistant foamed polyurethane according to any one of claims 1 to 8 in automobile interior or architectural sound-absorbing materials.
Citation Information
Patent Citations
A lightweight, high-toughness foam material and its preparation method and application
CN117659488B