Environment-friendly release agent for insert injection molding decorative film as well as preparation method and application of environment-friendly release agent

By using environmentally friendly release agents of water-based systems in the insert injection molding decorative film process, the problem of insufficient environmental protection and wear resistance in the existing technology is solved, and a low-cost and environmentally friendly insert injection molding decorative film process is realized, which improves hardening Wear resistance and chemical resistance of the protective layer.

CN118931388APending Publication Date: 2024-11-12SHANGHAI HUAGONG AIMAR NEW MATERIAL CO LTD

Patent Information

Application Number
CN202411063900.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing fluorine or silicone release agents have environmental problems in the insert injection molding decorative film process, high cost, uneven surface tension, high equipment requirements and insufficient wear resistance of the hardened protective layer.

Method used

An environmentally friendly release agent with an aqueous system, including Mengdan wax emulsion, alcohol, alkali liquid, leveling agent, wetting agent and defoaming agent, is prepared by blending process for release of insert injection molding decorative film The layer is printed on the PET base film to improve the wear resistance of the hardened protective layer.

Benefits of technology

It realizes environmental protection, low cost, simple printing, and improves the wear resistance and chemical resistance of the hardened protective layer, reduces environmental pollution and human body hazards, reduces equipment requirements, and enhances the friction resistance of the hardened protective layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004978808530000061
    Figure BDA0004978808530000061
  • Figure BDA0004978808530000071
    Figure BDA0004978808530000071
  • Figure BDA0004978808530000081
    Figure BDA0004978808530000081
Patent Text Reader

Abstract

The invention relates to an environment-friendly release agent for an insert injection molding decorative film and a preparation method and application thereof.The release agent is prepared from, by weight, 0.5-5 parts of a first component and 10-20 parts of a second component, the first component is prepared from, by weight, 1-20 parts of montan wax emulsion, 4-80 parts of water and 0.01-0.05 part of alkali liquor, and the second component is prepared from, by weight, 0.5-5 parts of a second component; the second component is prepared from the following components in parts by weight: 10 to 100 parts of alcohol, 5 to 50 parts of water, 0.01 to 0.05 part of flatting agent, 0.01 to 0.05 part of wetting agent and 0.01 to 0.05 part of defoaming agent. Compared with the prior art, the invention belongs to a more environment-friendly water-based system, and can improve the chemical resistance and wear resistance of a hardened protective layer on the surface of the insert injection molding decorative film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of release agents, and relates to an environmentally friendly release agent for an inlay injection molding decorative film, a preparation method and an application thereof. Background Art

[0002] The film insert molding process (INS process) uses the method of thermal plastic forming or high pressure forming to stretch the acrylonitrile-butadiene-styrene copolymer (ABS) sheet (usually 0.5mm thick) with the decorative film thermally transferred three times, and then cut out the insert according to the product shape, and then accurately place the insert in the injection mold cavity for injection molding. The INS process is now mostly used in the automotive interior industry. The main structure of the automotive interior decorative film includes a release layer, a hardened protective layer, a decorative layer and an adhesive layer which are sequentially printed on a polyethylene terephthalate (PET) base film (thickness is generally 25-50μm), and then dried and solidified to form a film. The thermal transfer process is to first thermally transfer the decorative film pre-printed on the PET base film with the adhesive layer facing downward (generally the thermal transfer temperature is 80-200℃, and the thermal transfer pressure is 1-10bar) to the ABS substrate. The PET base film needs to be peeled off after the thermal transfer, and the hardened protective layer is exposed to the outermost layer as a film protective layer to meet the product-related test requirements. Since the hardened protective layer (generally acrylic coatings, polyurethane coatings, and polycarbonate coatings) adheres to the PET base film after the thermal transfer process and is not easy to peel off, a release layer is required between the PET base film and the hardened protective layer to help peel off the PET base film.

[0003] The release layer is generally a polymer organic film-forming coating with a certain amount of fluorine or silicone additives, namely fluorine or silicone release agents. The principle is to isolate the hardened protective layer through the fluorine or silicone on the surface after the release agent is dried and cured, so that the PET base film can be peeled off together with the release layer, leaving the hardened protective layer on the INS decorative film.

[0004] Disadvantages of existing fluorine or silicone release layer technology:

[0005] (1) Most of them are organic solvent coatings, which require the use of a large amount of organic solvents. During production, the organic solvents evaporate into the air, polluting the environment and harming the human body, which is not environmentally friendly;

[0006] (2) After printing and drying, there is a large amount of fluorine or silicone on the surface, and the surface tension of the entire surface will be too small or uneven, resulting in the hardened protective layer coating cannot be evenly applied, increasing the product defect rate;

[0007] (3) The polymer organic film-forming coating and fluorine- or silicone-containing additives in its formula are special materials and have high costs;

[0008] (4) In order to ensure that the appearance of the post-coated hardened protective layer is not affected, the uniformity and flatness of the release layer coating are required to be high, and precision coating equipment has to be used for printing and coating, which places high requirements on the equipment and equipment personnel.

[0009] Patent CN116120836A discloses a release agent and its preparation method, application and electroplated aluminum, wherein the raw materials for its preparation include montan wax, resin, emulsifier, defoamer and leveling agent; wherein the resin includes one or more of silicone resin, silicone-modified acrylic resin, styrene-maleic anhydride copolymer and polyurethane. However, the release agent in the patent does not increase the friction resistance of the hardened protective layer; additional resin needs to be added to dissolve the montan wax; the resin will be transferred to the surface of the hardened protective layer, which will affect the chemical resistance of the hardened protective layer.

[0010] Patent CN104726022A discloses an environmentally friendly water-based composite wax emulsion release material for electroplated aluminum and its preparation method, which is prepared from the following raw materials in parts by weight: 10-25 parts of montan wax, 2-8 parts of water-based resin, 2-7 parts of emulsifier, 1-5 parts of pH adjuster, 1-5 parts of wetting agent, and 60-80 parts of water. However, the water-based resin component in the patent will also be transferred to the surface of the hardened layer, which will affect the chemical resistance and friction resistance of the hardened layer itself. Summary of the invention

[0011] The purpose of the present invention is to overcome at least one defect of the above-mentioned prior art and to provide an environmentally friendly release agent, preparation method and application for insert injection molding decorative film. The present invention belongs to a more environmentally friendly water-based system, and can also improve the chemical resistance and wear resistance of the hardened protective layer on the surface of the insert injection molding decorative film.

[0012] The purpose of the present invention can be achieved by the following technical solutions:

[0013] One of the technical solutions of the present invention is to provide an environmentally friendly release agent for an inlay injection molding decorative film, the release agent comprising 0.5-5 parts by weight of a first component and 10-20 parts by weight of a second component.

[0014] The first component includes: 1-20 parts of montan wax emulsion, 4-80 parts of water and 0.01-0.05 parts of alkali solution.

[0015] The second component includes: 10-100 parts of alcohol, 5-50 parts of water, 0.01-0.05 parts of leveling agent, 0.01-0.05 parts of wetting agent and 0.01-0.05 parts of defoaming agent.

[0016] Furthermore, the solid content of the montan wax emulsion is 10-30%, and the montan wax emulsion includes Yijiu Chemical Technology TL-501A or Wengkaier Trade E-7093 / 1.

[0017] Furthermore, the alkali solution includes aqueous ammonia, aqueous sodium hydroxide solution or aqueous potassium hydroxide solution, the concentration of the aqueous ammonia is 22-28%, and the concentrations of the aqueous sodium hydroxide solution and the aqueous potassium hydroxide solution are both 0.01-0.02 mol / L.

[0018] Furthermore, the alcohol includes ethanol or isopropanol.

[0019] Furthermore, the leveling agent includes Digo 346, 3499 or 333, the wetting agent includes Evonik 420, Digo 3455 or 3400, the defoaming agent includes Digo 1785, ET3070 or 035.

[0020] One of the technical solutions of the present invention is to provide a method for preparing the environmentally friendly release agent for the inlay injection molding decorative film, the method comprising the following steps:

[0021] S1. Preparation of the first component,

[0022] S1.1, adding alkali solution to water to adjust the pH, blending, and obtaining a mixed solution;

[0023] S1.2, adding the montan wax emulsion to the mixed solution, blending, and obtaining a first component;

[0024] S2. Preparation of the second component,

[0025] respectively blending alcohol, water, a leveling agent, a wetting agent and a defoaming agent to obtain a second component;

[0026] S3. Preparation of release agent,

[0027] The first component is added to the second component, and the mixture is blended to obtain an environmentally friendly release agent for an inlay injection molding decorative film.

[0028] Further, in step S1.1, the pH is adjusted to 8-9, the blending temperature is room temperature, the stirring speed is 300-700 r / min, and the time is 5-15 min;

[0029] In step S1.2, the blending temperature is 50-80° C., the stirring speed is 800-1200 r / min, and the time is 20-40 min.

[0030] Furthermore, the blending temperature in steps S2 and S3 is room temperature, the stirring speed is 300-700 r / min, and the time is 5-15 min.

[0031] One of the technical solutions of the present invention is to provide an application of the environmentally friendly release agent for the insert injection molding decorative film, wherein the release agent is applied to the release layer on the base film in the insert injection molding (INS) decorative film, and the release agent is gravure printed on the base film to obtain the release film.

[0032] As a preferred technical solution, the material of the base film includes polyethylene terephthalate (PET) or polypropylene (PP).

[0033] Furthermore, the engraving depth of the gravure printing roller is 2-8 μm, the printing speed is 5-15 m / min, the drying tunnel length is 5-15 m, and the drying tunnel temperature is 70-90° C.

[0034] The release layer has a thickness of 0.1-1 μm.

[0035] As a preferred technical solution, a hardening protective layer is arranged on the release layer on the other side of the base film.

[0036] As a preferred technical solution, the material of the hardened protective layer includes polyurethane or polyvinylidene fluoride, and the polyurethane includes two-component thermosetting polycarbonate polyurethane or one-component thermoplastic acrylic polyurethane.

[0037] As a preferred technical solution, the decorative film is thermally transferred onto the substrate.

[0038] As a preferred technical solution, the material of the substrate includes acrylonitrile-butadiene-styrene copolymer (ABS) or polycarbonate (PC).

[0039] As a preferred technical solution, the temperature of the thermal transfer is 80-200° C. and the pressure is 1-5 bar.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] (1) The release agent and its preparation method of the present invention do not require high temperature curing and long-term aging treatment, are easy to print, thin in thickness, and low in cost, and have the advantages of small organic solvent volatilization, low peel strength, and increased chemical resistance and wear resistance of the INS decorative film;

[0042] (2) The formulation system of the present invention is a water-based system, which has less environmental pollution and harm to human body, and has low volatile organic compounds (VOC), which is more environmentally friendly;

[0043] (3) The present invention utilizes a hot stirring dispersion process to better disperse the montan wax emulsion in water, so that the montan wax is more evenly coated on the surface of the substrate without adding additional resin;

[0044] (4) The dry film thickness of the release agent coating of the present invention is 0.1-1 μm, and the coating cost is relatively low;

[0045] (5) The release agent of the present invention will be transferred to the hardened protective layer after thermal transfer, thereby increasing the smoothness of the hardened protective layer, thereby increasing the friction resistance and reagent resistance of the hardened protective layer;

[0046] (6) The present invention does not require the addition of additional resin, only montan wax. Montan wax is a very long non-polar carbon chain with a very strong polar center, so it has strong corrosion resistance. Therefore, the transfer of montan wax to the hardened protective layer will not affect the reagent resistance of the hardened protective layer itself;

[0047] (7) The formulation of the present invention can be printed onto a base film by gravure printing, which is simple and convenient to operate and more efficient. DETAILED DESCRIPTION

[0048] The present invention is described in detail below in conjunction with specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and a specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0049] Unless otherwise specified, the equipment used in the following examples are all conventional equipment in the art; the reagents used are all commercially available products or prepared by conventional methods in the art unless otherwise specified. Anything not described in detail in the following examples can be achieved by conventional experimental means in the art.

[0050] Embodiments 1 to 6:

[0051] An environmentally friendly release agent for an inlay injection molding decorative film, comprising 0.5-5 parts of component A and 15 parts of component B, by weight.

[0052] Component A includes: 10 parts of montan wax emulsion (solid content is 25%, Yijiu Chemical Technology TL-501A), 40 parts of deionized water and 0.03 parts of ammonia water (concentrated ammonia water, concentration is 25%).

[0053] Component B includes: 50 parts of ethanol, 25 parts of deionized water, 0.03 parts of leveling agent (Digo 346), 0.03 parts of wetting agent (Evonik 420) and 0.03 parts of defoamer (Digo 1785).

[0054] The preparation method of the environmentally friendly release agent for the above-mentioned inlay injection molding decorative film has the following specific steps:

[0055] S1. Preparation of component A,

[0056] S1.1, by weight, add 0.03 parts of ammonia water to 40 parts of deionized water to adjust the pH to 8.5, blend in a container at room temperature of 25°C, stirring speed of 500 r / min, and stirring for 10 minutes to obtain a mixed solution;

[0057] S1.2, by weight, add 10 parts of montan wax emulsion to the mixed solution, blend in a closed container at 65°C, stirring speed 1000 r / min, stirring for 30 min to obtain component A;

[0058] S2. Preparation of component B,

[0059] By weight, 50 parts of ethanol, 25 parts of deionized water, and 0.03 parts of leveling agent (Digo) were added. 346), 0.03 parts of wetting agent (Evonik 420) and 0.03 parts of defoamer (Digo 1785) were mixed in a sealed container at room temperature of 25°C, stirring at a speed of 500 r / min, and stirring for 10 min to obtain component B;

[0060] S3. Preparation of release agent,

[0061] A certain amount of component A was added to component B by weight, and the mixture was mixed in a sealed container at room temperature of 25° C., with a stirring speed of 500 r / min and stirring for 10 minutes to prepare an environmentally friendly release agent for insert injection molding decorative film.

[0062] The above-mentioned environmentally friendly release agent for insert injection molding decorative film is used. The release agent is applied to the release layer on the base film in the insert injection molding (INS) decorative film. The above-mentioned release agent is printed on the polyethylene terephthalate (PET) base film through a gravure printing machine with certain equipment parameters (gravure printing parameters: gravure printing plate roller engraving depth 2-4μm, printing speed 10m / min, drying tunnel length 10m, drying tunnel temperature 80°C) to obtain a PET release film with a release layer thickness of 0.3μm.

[0063] A polyurethane hardened protective layer is printed and coated on the release layer of the prepared PET release film, and the polyurethane is a two-component thermosetting polycarbonate polyurethane.

[0064] The decorative film was thermally transferred onto an acrylonitrile-butadiene-styrene copolymer (ABS) substrate at a temperature of 130°C and a pressure of 3 bar.

[0065] The effects of different engraving depths of the printing plate roller of the release film in the examples and different ratios of component A to component B on the peeling strength, peeling force, glossiness of the hardened protective layer and friction resistance were tested.

[0066] Table 1 Peel strength, peel force, glossiness and friction resistance of the release film in Examples 1 to 6

[0067]

[0068] Comparative Examples 1 to 4:

[0069] Existing conventional fluorine-containing (Daikin chemicals ME-313) or silicone (Dow Chemical MEM-0349) release agent is used to prepare PET release film through slit precision coating.

[0070] The effects of different thicknesses of conventional fluorine-containing or silicone release films on peel strength, peel force, glossiness of the hardened protective layer and friction resistance in the comparative examples were tested.

[0071] Table 2 Peel strength, peel force, glossiness and friction resistance of the release film in Comparative Examples 1 to 4

[0072]

[0073] As shown in Table 1 and Table 2, it can be seen that the release agent formula in the embodiment has less effect on the gloss of the hardened protective coating, the peeling force and peeling strength are almost the same as those in Comparative Examples 1 to 4, and the wear resistance of the hardened protective layer is increased. In summary, the release agent formula in the embodiment can replace and be superior to the conventional fluorine-containing or silicone release agent formula in Comparative Examples 1 to 4. Because the fluorine-containing or silicone release agent in Comparative Examples 1 to 4 is not transferred to the surface of the hardened protective layer during the thermal transfer process, it has no effect on the surface of the hardened protective layer, while the montan wax in the embodiment is coated on the PET substrate. During the thermal transfer process, the interaction between the montan wax and the PET substrate molecules (such as hydrogen bonding, etc.) is weakened. When it is lower than the interaction between the montan wax and the hardened protective layer molecules, the montan wax is transferred to the surface of the hardened protective layer. After the montan wax is transferred to the surface of the hardened protective layer, the surface tension of the hardened protective layer is reduced, and the surface is smoother, so the friction resistance of the hardened protective layer can be improved.

[0074] Comparative Example 5:

[0075] Without using a release agent, a polyurethane hardened protective layer is directly set on the PET base film.

[0076] Comparative Example 6:

[0077] A release agent with additional resin is added, such as the formulation of Example 3 in patent CN116120836A.

[0078] The effects of whether there is a release agent on the surface of the hardened protective layer in the examples and comparative examples, and whether additional resin is added to the release agent on the sunscreen corrosion resistance were tested.

[0079] Table 3 Sunscreen corrosion resistance of the hardened protective layer in Example 4 and Comparative Examples 5 and 6

[0080]

[0081] As shown in Table 3, it can be seen that the resin in Comparative Example 6 itself has poor sunscreen corrosion resistance, and after being transferred to the hardened protective layer, it will affect the sunscreen corrosion resistance of the hardened protective layer itself in Comparative Example 5, while the release agent formula in the embodiment does not affect the sunscreen corrosion resistance of the hardened protective layer itself.

[0082] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. An environmentally friendly release agent for insert injection molding decorative film, It is characterized in that The release agent comprises 0.5-5 parts of the first component and 10-20 parts of the second component by weight. The first component includes: 1-20 parts of montan wax emulsion, 4-80 parts of water and 0.01-0.05 parts of alkali solution. The second component includes: 10-100 parts of alcohol, 5-50 parts of water, 0.01-0.05 parts of leveling agent, 0.01-0.05 parts of wetting agent and 0.01-0.05 parts of defoaming agent.

2. An environmentally friendly release agent for insert injection molding decorative film according to claim 1, It is characterized in that The solid content of the montan wax emulsion is 10-30%, and the montan wax emulsion includes Yijiu Chemical Technology TL-501A or Wengkaier Trade 3. The environmentally friendly release agent for insert injection molding decorative film according to claim 1, It is characterized in that The alkali solution includes ammonia water, sodium hydroxide aqueous solution or potassium hydroxide aqueous solution. The concentration of the ammonia water is 22-28%, and the concentrations of the sodium hydroxide aqueous solution and the potassium hydroxide aqueous solution are both 0.01-0.02 mol / L.

4. The environmentally friendly release agent for insert injection molding decorative film according to claim 1, It is characterized in that The alcohol includes ethanol or isopropanol.

5. The environmentally friendly release agent for insert injection molding decorative film according to claim 1, It is characterized in that The leveling agent includes Digo or The wetting agent includes Evonik Digo or The defoaming agent includes Digo or 6. A method for preparing an environmentally friendly release agent for an inlay injection molding decorative film as claimed in any one of claims 1 to 5, It is characterized in that The method comprises the following steps: S1. Preparation of the first component, S1.1, adding alkali solution to water to adjust the pH, blending, and obtaining a mixed solution; S1.2, adding the montan wax emulsion to the mixed solution, blending, and obtaining a first component; S2. Preparation of the second component, respectively blending alcohol, water, a leveling agent, a wetting agent and a defoaming agent to obtain a second component; S3. Preparation of release agent, The first component is added to the second component, and the mixture is blended to obtain an environmentally friendly release agent for an inlay injection molding decorative film.

7. The method for preparing an environmentally friendly release agent for an inlay injection molding decorative film according to claim 6, It is characterized in that In step S1.1, the pH is adjusted to 8-9, the blending temperature is room temperature, the stirring speed is 300-700 r / min, and the time is 5-15 min; In step S1.2, the blending temperature is 50-80°C, the stirring speed is 800-1200 r / min, and the time is 20-40 min.

8. The method for preparing an environmentally friendly release agent for insert injection molding decorative film according to claim 6, It is characterized in that The blending temperature in steps S2 and S3 is room temperature, the stirring speed is 300-700 r / min, and the time is 5-15 min.

9. Use of an environmentally friendly release agent for an inlay injection molding decorative film as claimed in any one of claims 1 to 5, It is characterized in that The release agent is applied to a release layer on a base film in an inlay injection-molded decorative film, and the release agent is gravure-printed on the base film to obtain a release film.

10. Use of an environmentally friendly release agent for insert injection molding decorative film according to claim 9, It is characterized in that The engraving depth of the gravure printing plate roller is 2-8 μm, the printing speed is 5-15 m / min, the drying tunnel length is 5-15 m, and the drying tunnel temperature is 70-90° C. The release layer has a thickness of 0.1-1 μm.

Citation Information

Patent Citations

  • Environment-friendly water-based composite wax emulsion release material for electric aluminum and preparation method of material

    CN104726022A

  • Release agent, preparation method and application thereof and alumite

    CN116120836A

  • Alumite separating layer painting containing hyperbranched polymers and preparation method thereof

    CN104927656A

  • Wax emulsion for anti-sticking plate applied to leather embossing, preparation method of wax emulsion and leather embossing method

    CN107916309A

Cited By

  • Film release coating and missed coating detection method thereof

    CN120682722A