Self-temperature-regulating asphalt phase-change material as well as preparation method and application thereof

By adding polyethylene glycol and silica sol to the asphalt mixture, the temperature of the road surface is automatically adjusted, which solves the problem of freezing asphalt pavement in winter, improves safety and durability, and Reduced the use and environmental impact of chemical snow melting agents.

CN118931500APending Publication Date: 2024-11-12刘伟男
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410998103.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing asphalt pavement is susceptible to temperature and load in winter, resulting in icing that increases traffic accident risk and maintenance costs, and reliance on chemical snow melting agents is not environmentally friendly.

Method used

The self-regulating phase change material prepared by polyethylene glycol and silica sol is integrated into the asphalt mixture to achieve automatic temperature regulation on the road surface and accelerate the melting of snow and ice.

Benefits of technology

Improves the safety and durability of the road in winter, reduces the use of chemical snow melting agents, reduces maintenance costs and environmental impacts, and extends the service life of the road.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931500A_ABST
    Figure CN118931500A_ABST
Patent Text Reader

Abstract

The invention discloses a self-temperature-regulating asphalt phase-change material as well as a preparation method and application thereof. The self-temperature-regulating asphalt phase-change material is prepared from the following raw materials in parts by weight: polyethylene glycol and silica sol in a mass ratio of (3-7): 10; according to the self-temperature-regulating phase-change material disclosed by the invention, the raw materials and the dosage are limited, so that the prepared self-temperature-regulating phase-change material is a solid-solid phase-change material, the melting enthalpy value is more than or equal to 50J / g, the phase change point is 17 + / -2 DEG C, and the enthalpy attenuation rate is less than or equal to 5%; therefore, the phase-change material is doped into the asphalt mixture, and the characteristic of high latent heat value of the phase-change material is utilized, so that the pavement has an automatic temperature regulation function, the frost resistance of the pavement can be effectively improved, the possibility of pavement icing can be reduced through the temperature self-regulation function, the service life of the pavement is prolonged, and the negative influence on the environment is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of phase change materials, and in particular to a self-temperature regulating asphalt phase change material and a preparation method and application thereof. Background Art

[0002] With the rapid development of social economy and highway transportation, asphalt pavement is widely used in the construction of highways, urban roads, airports and other transportation facilities due to its high flatness, good driving comfort and low noise. According to statistics, asphalt pavement accounts for about 50% of the existing roads, and more than 90% of the highways under construction, reconstruction or major and medium repairs use asphalt pavement. However, asphalt is a typical viscoelastic material, which determines that the performance of asphalt pavement is easily affected by load and temperature. Especially with global warming and abnormal climate, winter road maintenance faces more and more challenges. Icy roads not only increase the risk of traffic accidents, but also greatly increase the cost of road maintenance. In order to meet this challenge, it is particularly important to use advanced material technology to optimize road construction and maintenance methods.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] The first purpose of the present invention is to provide a self-temperature-regulating asphalt phase change material and its preparation method and application. The present invention integrates the phase change material into the asphalt mixture to develop a road surface material that can automatically adjust the temperature in winter and accelerate the melting process of snow and ice.

[0005] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0006] The first aspect of the present invention provides a self-temperature-adjusting asphalt phase change material, wherein the self-temperature-adjusting asphalt phase change material is prepared from the following raw materials in parts by weight:

[0007] The mass ratio of polyethylene glycol to silica sol is (3-7):10.

[0008] Preferably, the polyethylene glycol is polyethylene glycol 2000.

[0009] Preferably, the silica sol has a silicon dioxide content of 28% to 32% and a pH value of 9 to 9.4.

[0010] The second aspect of the present invention provides a method for preparing the above-mentioned self-temperature regulating asphalt phase change material, the preparation method comprising the following steps:

[0011] (a) weighing each raw material according to weight;

[0012] (b) adding polyethylene glycol to the heated silica sol and stirring until the silica sol is in a gel state to obtain a gel mixture;

[0013] (c) The gel mixture is placed at room temperature for a period of time, and then dried and ground to obtain the self-temperature-regulating asphalt phase change material.

[0014] Preferably, in the step (b), the temperature of the heated silica sol is 55-65° C.; and the stirring speed is 250-350 rpm.

[0015] Preferably, in step (c), the standing time is 20 to 28 hours; the drying temperature is 70 to 90° C., and the drying is performed until the mass does not change.

[0016] Preferably, in the step (c), the particle size of the self-temperature regulating asphalt phase change material after grinding is 2 to 4 mm.

[0017] A third aspect of the present invention provides an application of the self-temperature-regulating asphalt phase change material in urban roads, highways and bridges.

[0018] A fourth aspect of the present invention provides a self-temperature-regulating asphalt mixture, wherein the self-temperature-regulating asphalt mixture comprises an asphalt mixture and the self-temperature-regulating asphalt phase change material.

[0019] Preferably, the content of the self-temperature-regulating asphalt phase change material in the self-temperature-regulating asphalt mixture is 0.3% to 0.45%;

[0020] The asphalt mixture is SBS modified asphalt mixture Sup-13.

[0021] Compared with the prior art, the beneficial effects of the present invention include at least:

[0022] The present invention integrates phase change materials into asphalt mixtures to develop a road surface material that can automatically adjust temperature in winter and accelerate the melting process of snow and ice. This technology can not only increase the service life of roads and reduce winter maintenance costs, but also help protect the environment and reduce dependence on chemical de-icing agents.

[0023] The present invention uses phase change materials in road construction to enable the road surface to automatically adjust its temperature when the temperature changes, realize active heating in winter, accelerate the melting of ice and snow, thereby reducing the possibility of road icing, and realize the autonomous temperature adjustment and ice and snow melting functions of the road surface, thereby improving the safety and durability of the road in winter; compared with traditional chemical snow melting methods, this technology reduces the use of chemical snow melting agents and is environmentally friendly. At the same time, it utilizes the heat energy conversion of phase change materials during the melting and solidification process to improve energy utilization efficiency; in addition, the road surface automatically adjusts its temperature due to temperature changes, which can significantly reduce ice and snow accumulation, reduce the risk of sliding, improve driving safety on roads in winter, and extend the service life of roads and reduce maintenance requirements by reducing damage to roads caused by freezing and melting cycles. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following is a brief introduction to the drawings required for the specific embodiments or the description of the prior art. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn according to the actual scale.

[0025] Figure 1 These are the research results on the properties of the self-temperature-regulating asphalt phase change materials prepared with different mass ratios of polyethylene glycol and silica sol in the embodiments of the present invention. DETAILED DESCRIPTION

[0026] The following embodiments of the technical solution of the present invention are described in detail in conjunction with the embodiments. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and are therefore only used as examples, and cannot be used to limit the protection scope of the present invention.

[0027] It should be noted that, unless otherwise specified, the technical terms or scientific terms used in this application should have the common meanings understood by those skilled in the art to which the present invention belongs.

[0028] The embodiment of the present invention provides a self-temperature-adjusting asphalt phase change material, and the self-temperature-adjusting asphalt phase change material is prepared from the following raw materials in parts by weight:

[0029] The mass ratio of polyethylene glycol to silica sol is (3-7):10.

[0030] The self-temperature-regulating phase change material of the present invention is limited by the raw materials and the dosage, so that the prepared self-temperature-regulating phase change material is a solid-solid phase change material with a melting enthalpy value ≥50J / g, a phase change point of 17±2°C, and an enthalpy decay rate ≤5%. Therefore, the self-temperature-regulating phase change material is added to the asphalt mixture, and its high latent heat value is utilized to make the road surface have the function of self-temperature regulation. This configuration can not only effectively improve the antifreeze performance of the road surface, but also reduce the possibility of road surface icing through the temperature self-regulation function, extend the service life of the road surface, and reduce the negative impact on the environment.

[0031] In one embodiment, the polyethylene glycol is polyethylene glycol 2000. In other embodiments, the polyethylene glycol may also be polyethylene glycol 1000 or polyethylene glycol 6000.

[0032] The phase transition temperatures of polyethylene glycols with different molecular weights are different and can be selected according to actual needs.

[0033] In one embodiment, the silica sol has a silicon dioxide content of 28% to 32% and a pH value of 9 to 9.4.

[0034] Another embodiment of the present invention provides a method for preparing the above-mentioned self-temperature regulating asphalt phase change material, the preparation method comprising the following steps:

[0035] (a) weighing each raw material according to weight;

[0036] (b) adding polyethylene glycol to the heated silica sol and stirring until the silica sol is in a gel state to obtain a gel mixture;

[0037] (c) The gel mixture is placed at room temperature for a period of time, and then dried and ground to obtain the self-temperature-regulating asphalt phase change material.

[0038] In one embodiment, in the step (b), the temperature of the heated silica sol is 55-65° C.; and the stirring speed is 250-350 rpm.

[0039] In one embodiment, in the step (c), the standing time is 20 to 28 hours; the drying temperature is 70 to 90° C., and the drying is performed until the mass does not change.

[0040] In one embodiment, in the step (c), the particle size of the self-temperature-regulating asphalt phase change material after grinding is 2 to 4 mm.

[0041] Another embodiment of the present invention provides an application of the above-mentioned self-temperature-regulating asphalt phase change material in urban roads, highways and bridges.

[0042] Yet another embodiment of the present invention provides a self-temperature-regulating asphalt mixture, wherein the self-temperature-regulating asphalt mixture comprises an asphalt mixture and the self-temperature-regulating asphalt phase change material.

[0043] In one embodiment, the content of the self-temperature-regulating asphalt phase change material in the self-temperature-regulating asphalt mixture is 0.3% to 0.45%;

[0044] The asphalt mixture is SBS modified asphalt mixture Sup-13.

[0045] The technical solution of the present invention is further described in detail below through specific embodiments.

[0046] The raw materials used in the following examples are as follows:

[0047] The specific indicators of polyethylene glycol 2000 are shown in Table 1:

[0048] Table 1

[0049] Appearance (25℃) <![CDATA[Hydroxyl value (mgKOH·g -1 )]]> Freezing point / ℃ White flake solid 51~63 48~50

[0050] The specific indicators of silica sol are shown in Table 2:

[0051] Table 2

[0052]

[0053] Example 1

[0054] This embodiment is a method for preparing a self-temperature-adjusting asphalt phase change material, and the preparation method comprises the following steps:

[0055] According to the mass ratio of PEG2000 and silica sol of 1:2, the silica sol solution was heated to 60°C in a water bath and PEG2000 was gradually added, and an electric stirrer was used to stir at a speed of 300 rpm until the mixture reached a gel state. The gel mixture was aged at room temperature for 24 hours, and then transferred to an oven at 80°C for drying until the weight no longer changed. Finally, the dried material was taken out and ground to prepare a self-temperature regulating asphalt phase change material.

[0056] The performance of the self-temperature regulating asphalt phase change material was tested, and the test results are shown in Table 3;

[0057] Table 3

[0058]

[0059]

[0060] Example 2

[0061] Study on the influence of the addition amount of self-temperature regulating asphalt phase change material on the performance of asphalt mixture in this embodiment:

[0062] In order to clarify the specific effects of different addition ratios of phase change materials on the performance of SBS modified asphalt mixture (Sup-13), a series of tests including splitting strength, freeze-thaw splitting, stability and low-temperature crack resistance were carried out in the construction site laboratory; the test results are shown in Table 4;

[0063] Table 4

[0064]

[0065] Note: RT1 represents the splitting strength without freeze-thaw cycles, RT2 represents the splitting strength after freeze-thaw cycles, and TSR represents the freeze-thaw splitting strength ratio.

[0066] It can be seen from Table 4 that with the increase of phase change material content, the low-temperature crack resistance of asphalt mixture first improves and then deteriorates, and the low-temperature crack resistance is optimal when the content is 0.3%. With the increase of phase change material content, the water stability of asphalt mixture gradually decreases, especially when the content exceeds 0.5%.

[0067] Example 3

[0068] This example is a study on the properties of self-temperature regulating asphalt phase change materials prepared with different mass ratios of polyethylene glycol and silica sol:

[0069] SBS (IC) modified asphalt mixture was selected for experimental research; the subsequent experiments were carried out according to the addition amount of self-temperature regulating asphalt phase change material of 0.3%;

[0070] Self-temperature-adjusting asphalt phase change materials with a ratio of PEG2000 to silica sol of 3:10, 5:10 and 7:10 were prepared;

[0071] The phase change asphalt mixture specimen with a size of 300mm×300mm×50mm was formed by the wheel rolling method. After being placed at room temperature for 24 hours, a 30mm deep hole was drilled in the center of the bottom. After burying the temperature sensor, the phase change asphalt mixture was placed in a rutting tester for heating (heating temperature 60℃) to carry out a temperature control effect test, and the change pattern of the internal temperature of the asphalt mixture with the heating time was recorded until the temperature reached 60℃.

[0072] The asphalt mixture without self-temperature regulating asphalt phase change material was used as a reference. The results were recorded as follows: Figure 1 As shown;

[0073] Depend on Figure 1 It can be seen that when the temperature is higher than 40°C, the phase change material can effectively reduce the high temperature duration of asphalt mixture. When the heating time is less than 60 minutes, the temperature of each group of asphalt mixture is basically the same; when the time exceeds 60 minutes, the temperature of the asphalt mixture mixed with phase change material gradually becomes lower than that of the ordinary asphalt mixture, but as time goes on, the temperature of each group of asphalt mixture tends to be consistent; however, when the ratio of PEG2000 to silica sol is 5:10, the cooling effect is the best.

[0074] Example 4

[0075] This embodiment is a self-temperature regulating asphalt mixture and a construction process

[0076] Except for the precise and effective addition of the self-temperature-adjusting asphalt phase change material according to the designed proportion, the rest of the mixing, transportation, paving and road marking operations are exactly the same as the process of paving the surface layer of the modified asphalt mixture Sup-13.

[0077] 1. The addition of self-temperature-adjusting asphalt phase change material is carried out by metering equipment and automatically completed through the conveying system. Before adding the self-temperature-adjusting asphalt phase change material, the mineral material is dry-mixed first, and then while the asphalt is sprayed, the self-temperature-adjusting asphalt phase change material is automatically added to the mixer through the pipeline according to the settings of the computer control system to ensure that it is fully mixed with other materials.

[0078] 2. Laying and compacting:

[0079] Ensure that the asphalt mixture used meets the preset standards and quality requirements. The paving process begins with spreading the mixture evenly on the road base, and then compacting the laid asphalt using a road compactor to ensure that the material is tightly bonded to the foundation without voids or loose parts. Throughout the paving process, the temperature and thickness of the material need to be continuously monitored to ensure consistency and uniformity, thereby improving the service life and performance of the road. In addition, the construction team must follow strict safety regulations to ensure the safety of construction personnel and vehicles.

[0080] Compacting of the mixture:

[0081] 1) After the mixture is spread and leveled, the road surface should be checked immediately, any irregularities should be manually adjusted promptly, and then compacted fully and evenly.

[0082] 2) Compaction work should be carried out according to the combination and procedures of compaction equipment determined by the test road.

[0083] 3) Compaction is divided into three stages: initial compaction, repeated compaction and final compaction.

[0084] a. Initial compaction: It should be carried out immediately after paving (high temperature compaction) with a static two-wheel roller (2 times), and the initial compaction temperature should be controlled at 130℃-145℃. The initial compaction should be carried out with a light steel drum roller or a vibrating roller with vibration turned off. When compacting, the driving wheel should face the paver. The compaction route and direction should not be changed suddenly to cause the mixture to move. After the initial compaction, check the flatness and road camber, and make adjustments if necessary.

[0085] b. Re-compaction: Re-compaction is carried out immediately after initial compaction. It is completed with a vibratory roller and a tire roller. Generally, the vibratory roller is used for 3-4 times, and then the tire roller is used for 4-6 times to achieve the compaction degree.

[0086] c. Final compaction: Final compaction is carried out immediately after re-compaction. Final compaction is carried out using a double-wheel steel drum roller with vibration turned off to eliminate wheel marks (the final temperature is greater than 70-80℃).

[0087] 4) Initial compaction and vibration rolling should be carried out at a low speed to avoid displacement and cracking of hot materials. Rolling should be carried out at a higher temperature after paving. Generally, initial compaction should not be lower than 130℃. The higher the temperature, the easier it is to improve the smoothness and compaction of the road surface. Change the habit of waiting until the mixture temperature drops to 110℃ before rolling.

[0088] 5) The rolling work should be carried out according to the test results determined by the test road.

[0089] 6) During rolling, the roller shall not stop, turn or brake.

[0090] 7) The roller shall not stay on the rolled mixture with a temperature higher than 70°C. At the same time, effective measures shall be taken to prevent oil, lubricating fingers, automobiles or other organic impurities from spilling onto the road surface during the operation or parking of the roller.

[0091] 8) During compaction, if the temperature of the mixture at the joints (including longitudinal joints, transverse joints or construction joints formed due to other reasons) can no longer meet the compaction temperature requirements, a heater should be used to increase the temperature of the mixture to the required compaction temperature, and then compact it until there are no seams.

[0092] 9) During the paving and rolling process, special personnel should be organized to carry out quality inspection and control and defect repair. The compaction degree should be checked in time, and if it is found to be insufficient, the compaction should be supplemented in time within the specified temperature. The surface of the road surface that has been rolled should not be repaired.

[0093] 3. Performance testing

[0094] The on-site test data after the pavement construction was completed are shown in Table 5. All indicators meet the requirements of the specifications.

[0095] Table 5

[0096]

[0097] 4. Benefit Analysis

[0098] 4.1 Economic Benefits

[0099] Although the initial investment of this invention is relatively high, it provides significant economic benefits over the entire life cycle of the road. Compared with traditional chemical deicing agents, this method can effectively avoid damage to the road structure and the surrounding environment through the active temperature adjustment function, thereby greatly reducing the frequency and cost of road repair and maintenance.

[0100] Although commonly used de-icing agents such as sodium chloride and magnesium chloride are low-cost (about 1,500 yuan / ton), their corrosion to metal and bridge structures and damage to surrounding vegetation have shortened the service life of roads and increased maintenance costs. In addition, environmentally friendly de-icing agents such as acetic acid, although they have no effect on the road surface, cost as much as 12,000 yuan / ton, making their widespread use a heavy economic burden.

[0101] On the contrary, although the initial investment of self-temperature-adjusting road phase change material technology is relatively large, it has significant cost-effectiveness in the long run due to the reduction of daily maintenance needs of roads and the extension of the service life of the road surface. By reducing the number of maintenance times and extending the service life, it not only reduces the overall economic cost, but also improves the reliability and safety of road use.

[0102] 4.2 Social Benefits

[0103] This method significantly improves the safety and reliability of roads, especially in winter when ice is easy to form. By adding phase change materials to the asphalt mixture, this technology can actively heat the road surface, melt snow and ice in time, effectively prevent the formation of ice, and greatly reduce traffic accidents caused by icy roads, thereby ensuring traffic safety and smoothness. In addition, the use of phase change materials reduces the dependence on traditional chemical de-icing agents, which often pollute the environment and accelerate the corrosion of roads and vehicles. Therefore, this technology not only reduces environmental pressure, but also reduces the maintenance cost of public infrastructure and extends the service life of roads.

[0104] 4.3 Environmental benefits

[0105] Traditional chemical deicing agents, especially chloride salts, cause serious damage to the environment: (1) They have a huge impact on vegetation. Due to the long-term use of chloride salt deicing agents, the sodium and chloride ion content in the soil has increased significantly, leading to problems such as yellowing of urban green spaces, tree death, and compaction of soil structure; (2) They pose a threat to humans and animals. The toxic components in deicing agents penetrate into groundwater or directly flow into rivers through melted snow, which has a negative impact on aquatic life and ecological balance.

[0106] In contrast, active snow-melting asphalt pavement technology does not have harmful effects on the environment and road-related structures, thus avoiding the ecological damage caused by traditional snow-melting methods and demonstrating significant ecological benefits.

[0107] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.

Claims

1. A self-temperature regulating asphalt phase change material, characterized in that: The self-temperature regulating asphalt phase change material is prepared from the following raw materials in parts by weight: The mass ratio of polyethylene glycol to silica sol is (3-7):

10.

2. The self-temperature regulating asphalt phase change material according to claim 1, characterized in that: The polyethylene glycol is polyethylene glycol 2000.

3. The self-temperature regulating asphalt phase change material according to claim 1, characterized in that: The silica sol has a silicon dioxide content of 28% to 32% and a pH value of 9 to 9.

4.

4. The method for preparing the self-temperature regulating asphalt phase change material according to any one of claims 1 to 3, characterized in that: The steps include: (a) weighing each raw material according to weight; (b) adding polyethylene glycol to the heated silica sol and stirring until the silica sol is in a gel state to obtain a gel mixture; (c) The gel mixture is placed at room temperature for a period of time, and then dried and ground to obtain the self-temperature-regulating asphalt phase change material.

5. The preparation method according to claim 4, characterized in that: In the step (b), the temperature of the heated silica sol is 55-65° C. and the stirring speed is 250-350 rpm.

6. The preparation method according to claim 4, characterized in that: In the step (c), the standing time is 20 to 28 hours; the drying temperature is 70 to 90° C., and the drying is performed until the mass does not change.

7. The preparation method according to claim 4, characterized in that: In the step (c), the particle size of the self-temperature regulating asphalt phase change material after grinding is 2 to 4 mm.

8. Use of the self-temperature-regulating asphalt phase change material according to any one of claims 1 to 3 in urban roads, highways and bridges.

9. A self-temperature regulating asphalt mixture, characterized in that: The self-temperature-regulating asphalt mixture comprises an asphalt mixture and the self-temperature-regulating asphalt phase change material described in any one of claims 1 to 3.

10. The self-temperature regulating asphalt mixture according to claim 9, characterized in that: The content of the self-temperature-adjusting asphalt phase change material in the self-temperature-adjusting asphalt mixture is 0.3% to 0.45%; The asphalt mixture is SBS modified asphalt mixture Sup-13.

Citation Information

Cited By

  • Self-adaptive temperature control modified reinforcing agent for asphalt pavement as well as preparation method and application of self-adaptive temperature control modified reinforcing agent

    CN121378939A

  • High-performance PUSSPCM phase-change self-temperature-regulating asphalt suitable for summer pavement and preparation method of PUSSPCM phase-change self-temperature-regulating asphalt

    CN121610091A