Anti-ablation composite layer material and corresponding composite layer preparation method

Through laser cladding technology, the tantalum copper composite layer was prepared on the surface of the copper alloy and the introduction of zirconium and titanium elements were solved, and the problem of poor ablation resistance of copper alloy was improved, achieving the improvement of electrical and thermal conductivity and mechanical properties, elongation and ablation resistance were achievable Significant improvement in performance.

CN118932331AActive Publication Date: 2024-11-12HUAZHONG UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410997462.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

Copper alloys have poor ablation resistance under extreme ablation conditions, and the prior art is difficult to take into account the strength, thermal conductivity and ablation resistance of the coating, and the mechanical properties of the tantalum copper composite layer are limited.

Method used

The tantalum copper composite layer is prepared on the surface of the copper alloy by laser cladding. Alloy elements such as zirconium and titanium are introduced to improve the uniformity and interface bonding of the tantalum copper system, forming a tantalum copper composite layer, using the high melting point of tantalum and low copper. The melting point achieves spontaneous sweat cooling effect and improves the ablation resistance.

Benefits of technology

The ablation resistance and service life of copper alloys were significantly improved, and a tantalum copper composite layer with excellent electrical and thermal conductivity and good mechanical properties was obtained. The elongation and ablation resistance reached 10% and above and 3 times that of copper alloys respectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932331A_ABST
    Figure CN118932331A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of laser surface treatment, and discloses an anti-ablation composite layer material and a corresponding composite layer preparation method.The anti-ablation composite layer material powder used for forming an anti-ablation coating on the surface of copper alloy comprises metal tantalum elementary substance powder and copper-titanium-chromium-zirconium alloy powder at the same time, the particle size of tantalum particles ranges from 2 micrometers to 50 micrometers, and the particle size of titanium particles ranges from 2 micrometers to 50 micrometers. The particle size of the copper-titanium-chromium-zirconium alloy powder is 75-150 [mu] m; the mass percent of the metal tantalum elementary substance powder is 10%-80%, and the mass percent of the copper-titanium-chromium-zirconium alloy powder is 20%-90%. By introducing alloy elements such as zirconium, titanium and chromium which are compatible with tantalum and copper, the uniformity of a tantalum-copper system can be effectively improved, and agglomeration and nonuniformity caused by incompatibility of the tantalum-copper alloy are avoided; meanwhile, the alloy elements can also form coherent or semi-coherent interfaces with tantalum and copper, so that the stress concentration of the tantalum-copper composite layer during plastic deformation is relieved, and the ductility of the tantalum-copper composite material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of laser surface treatment, and more specifically, relates to an anti-ablation composite layer material and a corresponding composite layer preparation method. The obtained anti-ablation coating has the characteristics of high strength, high conductivity, and ablation resistance. Background Art

[0002] Copper alloys have technical advantages such as high electrical and thermal conductivity and good plasticity, and are widely used in the fields of electricity, electronics, metallurgy, and national defense. However, copper alloys have the disadvantage of low ablation resistance, which reduces their service life under extreme ablation conditions, limiting their application to a certain extent.

[0003] Preparing an anti-ablation coating on the surface of copper alloy is an effective way to increase its service life. Domestic and foreign researchers have tried to use the method of thermal spraying refractory metal coatings to increase its service life, but they cannot take into account the strength, toughness, electrical conductivity, thermal conductivity and anti-ablation properties of the coating, making it difficult to use under extreme working conditions. Under extreme ablation and thermal stress, the design of copper alloy surface coating materials and the selection of preparation processes must have the following characteristics: first, it has good bonding strength with the copper alloy substrate and the coating itself has high strength and plasticity (elongation); second, the coating material has a high melting point and melting enthalpy; third, it must not be at the expense of significantly sacrificing the electrical conductivity and thermal conductivity of the copper alloy.

[0004] The use of refractory metals can improve the ablation resistance of copper alloys. Compared with the use of a single refractory metal as a coating, the composite layer prepared by selecting a combination of refractory metals and copper as a coating material has better electrical and thermal conductivity. The "self-sweating material" composed of refractory metals (tungsten / molybdenum / tantalum, etc.) and low-melting-point metals (copper, etc.) forms a "self-sweating cooling effect" on the refractory metal through the melting and volatilization of the low-melting-point metal at high temperature to meet the needs of high-temperature ablation conditions. Tungsten-copper and molybdenum-copper alloys are common "spontaneous sweating materials" with good electrical conductivity, thermal conductivity and ablation resistance. However, since tungsten-copper and molybdenum-copper are incompatible in both liquid and solid phases, when laser cladding technology is used to prepare the coating, tungsten / molybdenum and copper in the molten pool are easily separated and agglomerated, resulting in low strength and plasticity, which is difficult to meet the requirements of mechanical properties for extreme working conditions. Tantalum, which is also a refractory metal, has a high melting point, strength and elongation, and tantalum and copper are mutually soluble in the liquid phase, which makes it possible to prepare tantalum-copper coatings by laser cladding.

[0005] The main technologies for preparing coatings are spraying and laser cladding. The spray coating is mechanically bonded to the substrate, and the bonding strength is low. The coating is easy to peel off under extreme working conditions. Laser cladding technology is a process method that uses a high-energy density laser beam to melt the powder material added to the surface of the workpiece and form a metallurgical bonding coating with the substrate. Compared with surfacing, spraying, electroplating and vapor deposition, laser cladding technology has a series of advantages such as low coating dilution rate, dense structure, metallurgical bonding with the substrate, and small heat-affected zone. It is an effective way to prepare high-performance composite layers on the surface of copper and its alloys. The use of laser cladding technology to prepare a tantalum-copper composite layer on the surface of a copper alloy can greatly improve the ablation resistance of the copper alloy, thereby increasing its service life. However, due to the incompatibility of tantalum and copper in the solid phase, tantalum is easy to agglomerate in the prepared tantalum-copper composite layer, and the tantalum-copper interface bonding strength is low, the elongation of the cladding layer will be low, and the mechanical properties will be very limited. Summary of the invention

[0006] In response to the demand for improvement of the poor ablation resistance of copper alloys under extreme working conditions, the purpose of the present invention is to provide an ablation-resistant composite layer material and a corresponding composite layer preparation method, and utilize a laser cladding process to laser-clad a tantalum-copper composite material on the surface of a copper alloy to form a tantalum-copper composite layer. Tantalum has a high melting point and can greatly improve the ablation resistance of the copper alloy substrate. In addition, the molten pool and molten powder droplets formed in real time during the laser cladding process can achieve mutual solubility of tantalum and copper in the liquid phase; however, due to the immiscibility of tantalum and copper in the solid phase, the elongation of the obtained tantalum-copper composite layer will be low. In order to improve the mechanical properties of the tantalum-copper composite layer, the present invention introduces alloy elements such as zirconium, titanium, chromium, etc. that are compatible with both tantalum and copper. On the one hand, it can effectively improve the uniformity of the tantalum-copper system and avoid the agglomeration and unevenness of the tantalum-copper alloy due to incompatibility in the liquid phase; on the other hand, the above alloy elements can also form an interface in which tantalum and copper form a coherent or semi-coherent relationship. This interface can reduce the lattice mismatch, thereby alleviating the stress concentration of the tantalum-copper composite layer during plastic deformation and improving the elongation of the tantalum-copper composite material.

[0007] The invention can improve the ablation resistance of the copper alloy workpiece and prolong the service life.

[0008] To achieve the above-mentioned purpose, according to one aspect of the present invention, there is provided an anti-ablation composite layer material powder for forming an anti-ablation coating on the surface of a copper alloy, characterized in that it comprises metal tantalum powder and copper-titanium-chromium-zirconium alloy powder at the same time, wherein the particle size of the tantalum particles is 2-50 μm, and the particle size of the copper-titanium-chromium-zirconium alloy powder is 75-150 μm; the copper-titanium-chromium-zirconium alloy powder is composed of the following elements in percentage by mass: 0.60-0.70% Cr, 0.060-0.075% Zr, 2.00-10.00% Ti and the remainder Cu; the mass percentage of metal tantalum powder in the anti-ablation composite layer material powder is 10%-80%, and the mass percentage of copper-titanium-chromium-zirconium alloy powder in the anti-ablation composite layer material powder is 20% to 90%.

[0009] According to another aspect of the present invention, the present invention provides a method for preparing an anti-ablation composite layer on a copper alloy surface, characterized in that it comprises the following steps:

[0010] S1. Preparing an anti-ablation composite layer material powder for forming an anti-ablation coating on the surface of a copper alloy, comprising a metal tantalum powder and a copper-titanium-chromium-zirconium alloy powder, wherein the tantalum particles have a particle size of 2-50 μm, and the copper-titanium-chromium-zirconium alloy powder has a particle size of 75-150 μm; the copper-titanium-chromium-zirconium alloy powder is composed of the following elements in percentage by mass: 0.60-0.70% Cr, 0.060-0.075% Zr, 2.00-10.00% Ti and the remainder Cu;

[0011] S2. Pre-treating the surface of the copper alloy substrate by laser roughening or sandblasting to roughen the surface to improve the laser absorption rate;

[0012] S3. Based on the laser cladding process, the laser beam is obliquely incident on the surface of the copper alloy substrate obtained in step S2, and at the same time, the evenly mixed anti-ablation composite layer material powder is fed into the laser molten pool or spread on the surface of the copper alloy substrate by a powder feeding method, wherein the mass percentage of the metal tantalum single substance powder in the anti-ablation composite layer material powder is 10%-80%, and the mass percentage of the copper-titanium-chromium-zirconium alloy powder in the anti-ablation composite layer material powder is 20%-90%; then, a tantalum-copper composite layer is formed on the surface of the copper alloy substrate by a laser cladding process; the thickness of the obtained tantalum-copper composite layer is 0.5-5mm.

[0013] As a further preferred embodiment of the present invention, in step S3, the parameter conditions adopted by the laser cladding process are as follows: the spot area of ​​the laser beam is set to 25 mm 2 -50 mm 2, laser power is set to 8000W-14000W, scanning speed is set to 300mm / min-2000mm / min, powder feeding gas flow is set to 5L / min-12L / min and protective gas flow is set to 5L / min-25L / min;

[0014] Preferably, the light spot is a light spot with Gaussian energy distribution; more preferably, the light spot is a flat-top light spot with uniform energy distribution.

[0015] As a further preferred embodiment of the present invention, in step S1, the metal tantalum powder and the copper-titanium-chromium-zirconium alloy powder are respectively placed in different powder hoppers of a double powder hopper, and the double powder hoppers are used to synchronously feed powder to achieve uniform mixing of the anti-ablation coating material powder and powder feeding in step S3.

[0016] As a further preferred embodiment of the present invention, in step S3, the angle between the laser beam in the laser scanning direction and the normal direction of the copper alloy substrate surface is 5-45 degrees to avoid damage to optical components caused by reflection of the laser beam.

[0017] According to another aspect of the present invention, the present invention provides a copper alloy surface anti-ablation composite layer obtained by the above-mentioned preparation method.

[0018] Compared with the prior art, the above technical solution conceived by the present invention can achieve the following beneficial effects:

[0019] 1. The tantalum-copper cladding material used in the present invention has both the good electrical and thermal conductivity of copper alloy and the high melting point and good ablation resistance of tantalum. The present invention adopts a laser cladding process. The laser cladding process uses a laser to melt the surface to be processed to form a molten pool. At the same time, the laser will also melt the powder. In this way, the present invention will be able to achieve mutual dissolution of tantalum and copper in the liquid phase to form a tantalum-copper alloy. Compared with the simple refractory metal tantalum, the tantalum-copper alloy has higher electrical and thermal conductivity, and the low-melting point component copper will melt and volatilize during the ablation process. Its latent heat of melting will form a "spontaneous sweating cooling effect" on the refractory metal tantalum, thereby improving the ablation resistance of the composite layer. In addition, the present invention uses laser cladding technology to prepare a tantalum-copper composite layer on the surface of a copper alloy, which can obtain a smaller heat-affected zone and deformation, and obtain a higher composite layer / substrate interface bonding strength.

[0020] 2. In addition, the present invention can further promote the formation of a semi-coherent interface between tantalum and copper by introducing the Ti element into the coating, improve the interface bonding between tantalum and copper, and increase the elongation of the composite layer. The present invention can improve the compatibility of tantalum and copper by introducing the titanium element into the coating, promote the uniform distribution of refractory metal tantalum dendrites, improve the interface bonding state between tantalum and copper, and enhance the comprehensive mechanical properties of the tantalum-copper composite layer.

[0021] The introduction of Ti element in the composite layer of the present invention is achieved by using copper-titanium-chromium-zirconium alloy powder as a raw material, and then using a laser cladding process to form a tantalum-copper composite layer containing titanium element. In addition to introducing Ti element, the copper-titanium-chromium-zirconium alloy powder also introduces zirconium element and chromium element at the same time. The introduction of zirconium, titanium, chromium and other elements can promote the formation of a semi-coherent interface between tantalum and copper, and improve the elongation of the composite layer.

[0022] 3. In addition, based on the present invention, it is preferred that the mass of the metal tantalum powder accounts for 10% to 80% of the total mass of the uniformly mixed powder, and the copper-titanium-chromium-zirconium alloy powder accounts for 20% to 90% of the total mass of the uniformly mixed powder. By adjusting the mass ratio of tantalum in the tantalum-copper alloy, a tantalum-copper composite layer with good electrical and thermal conductivity, high melting point and good ablation resistance is obtained. The obtained tantalum-copper composite layer has good electrical and thermal conductivity, mechanical properties and excellent ablation resistance, wherein the electrical conductivity of the tantalum-copper composite layer is ≥10% IACS, the elongation is ≥10%, and the ablation resistance is more than 3 times that of the copper alloy.

[0023] Compared with the simple refractory metal anti-ablation material, the tantalum-copper self-sweating composite material proposed in the present invention controls the mass proportion of the metal tantalum powder and the copper-titanium-chromium-zirconium alloy powder in the anti-ablation composite material powder used to form the anti-ablation composite layer to 10%-80% and 20%-90% respectively through the reasonable design of the tantalum-copper ratio. The formed anti-ablation composite layer has higher electrical and thermal conductivity, which takes into account the anti-ablation performance of the high-conductivity refractory metal of the copper alloy. Moreover, during the arc ablation process, the low-melting-point copper melts and absorbs heat, which will form a self-sweating cooling effect on the ablation of the refractory metal. In addition, in view of the technical difficulties of the incompatibility of refractory metal tantalum and copper in the solid phase, the present invention introduces titanium, chromium, zirconium-nickel and other elements to construct a tantalum-copper coherent / semi-coherent phase interface, which can effectively improve the strength and elongation of the tantalum-copper composite material, and obtain a self-sweating anti-ablation material with both electrical, thermal and mechanical properties. It opens up a new technical route for the design of anti-ablation materials under extreme working conditions.

[0024] The present invention adopts surface engineering technology to prepare the anti-ablation material on the surface of the copper alloy to form an anti-ablation composite layer, which can give full play to the good high conductivity of the copper alloy substrate and significantly reduce the material cost. The coating prepared by the traditional thermal spraying technology is mechanically combined with the substrate. Because the coating substrate bonding force is low, the coating peeling problem is prone to occur under extreme working conditions. To this end, the present invention adopts laser cladding technology to prepare a composite layer on the surface of the copper alloy substrate, which has technical advantages such as high composite layer / substrate bonding force, small heat-affected zone and deformation. At the same time, in view of the problem of high reflectivity of copper alloy to laser, the present invention adopts a method of increasing the surface roughness of copper alloy to improve the laser absorption rate; and in the laser cladding process, it is preferred to deflect the laser head by a certain angle so that the angle between the laser beam in the laser scanning direction and the normal direction of the copper alloy substrate surface is 5-45 degrees, which can effectively avoid the damage of reflected light to optical components and obtain a stable processing effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the laser cladding forming process with dual powder hoppers synchronously feeding powder in an embodiment of the present invention.

[0026] Figure 2 This is a cross-sectional SEM comparison of the laser cladding tantalum-copper composite layer with and without titanium added; Figure 2 (a) is a cross-sectional SEM image of the laser-clad tantalum-copper composite layer without titanium element added obtained in Example 1; Figure 2 (b) is a cross-sectional SEM image of the laser-clad tantalum-copper composite layer with titanium added obtained in Example 3.

[0027] Figure 3 It is a high-resolution transmission electron microscope image of the cross section of the laser cladding tantalum-copper composite layer with and without titanium added; Figure 3 (a) is a high-resolution transmission electron microscope image of the cross section of the laser-clad tantalum-copper composite layer without titanium element added obtained in Example 1. Figure 3 (b) is a high-resolution transmission electron microscopy image of the cross section of the laser-clad tantalum-copper composite layer with titanium added obtained in Example 3.

[0028] Figure 1 In the figure, the meanings of the various reference numerals are as follows: 1—laser beam, 2—No. 1 powder hopper, 3—No. 2 powder hopper, 4—metal tantalum particles, 5—copper-titanium-chromium-zirconium powder with added titanium element or copper-chromium-zirconium powder without added titanium element, 6—tantalum-copper composite layer, 7—molten pool, 8—copper alloy matrix, 9—laser beam scanning direction. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0030] Figure 1 It is a schematic diagram of the process of laser cladding a tantalum-copper composite layer on the surface of a copper alloy according to an embodiment of the present invention. As can be seen from the figure, metallic tantalum is placed in a No. 1 powder hopper 2, and chromium-zirconium-titanium-copper powder with added titanium element (or chromium-zirconium-copper powder without added titanium element) is placed in a No. 2 powder hopper 3. Under the action of the laser beam 1, the surface of the copper alloy matrix 8 is melted to form a molten pool 7, and the metallic tantalum powder and the copper alloy powder are melted and then solidified to form a tantalum-copper composite layer 6.

[0031] Example 1

[0032] The method for preparing a tantalum-copper composite layer by laser cladding on a copper alloy surface specifically comprises the following steps:

[0033] The copper alloy surface is pretreated to make the surface rougher so as to reduce the reflectivity of the copper alloy substrate surface to the laser, thereby improving energy utilization.

[0034] The laser beam is tilted by 5 degrees (i.e., the angle between the laser beam along the scanning direction and the normal direction of the copper alloy surface is 5 degrees), and the metal tantalum with a particle size of 2-50 μm and the copper-chromium-zirconium powder without titanium element with a particle size of 75-150 μm are placed in different powder feeding hoppers. Ta powder is prepared by plasma rotary atomization, and the copper-chromium-zirconium powder without titanium element is prepared by argon atomization, including the following elements in mass percentage: 0.60% Cr, 0.060% Zr and the balance Cu.

[0035] The powder feeder was adjusted so that the powder feeding rate of metal tantalum was 12 g / min, the powder feeding rate of chromium zirconium copper powder was 8 g / min, and the mass percentage of tantalum was 60%.

[0036] Adjust the laser beam spot size to 25mm 2 The spot is a spot with energy Gaussian distribution, the laser power is set to 14000W, the scanning speed is set to 300mm / min, the powder feeding gas flow rate is set to 5L / min, and the shielding gas flow rate is set to 5L / min.

[0037] Open the automatic powder feeder and turn on the laser. Under the action of the laser, the surface of the copper alloy melts to form a molten pool. At the same time, the metal tantalum and chromium-zirconium-copper powders melt and then solidify to finally form a tantalum-copper cladding layer.

[0038] Set the laser power to 12000W, turn on the automatic powder feeder, turn on the laser, and clad the second layer.

[0039] Set the laser power to 10000W, turn on the automatic powder feeder, turn on the laser, and clad the third layer.

[0040] Set the laser power to 8000W, turn on the automatic powder feeder, turn on the laser, and clad the fourth layer.

[0041] The formed tantalum-copper composite layer has a total of 4 layers with a thickness of 2.5 mm.

[0042] The test shows that the conductivity of the cladding layer is 35% IACS, and its ablation performance is more than 3 times that of Cr-Zr-Cu C18000 copper alloy. Because the cladding layer cracked, the tensile properties could not be tested.

[0043] Example 2

[0044] The method for preparing a tantalum-copper composite layer by laser cladding on a copper alloy surface specifically comprises the following steps:

[0045] The copper alloy surface is pretreated to make the surface rougher so as to reduce the reflectivity of the copper alloy substrate surface to the laser, thereby improving energy utilization.

[0046] The laser beam is tilted by 20 degrees (i.e., the angle between the laser beam along the scanning direction and the normal direction of the copper alloy surface is 20 degrees), and the metal tantalum with a particle size of 2-50 μm and the copper-titanium-chromium-zirconium powder containing titanium elements with a particle size of 75-150 μm are placed in different powder feeding hoppers. The copper-titanium-chromium-zirconium powder containing titanium elements is prepared by vacuum melting method, including the following elements in mass percentage: 0.70% Cr, 0.075% Zr, 2.00% Ti and the balance Cu.

[0047] The powder feeder was adjusted so that the powder feeding rate of metal tantalum was 16 g / min, the powder feeding rate of chromium zirconium titanium copper powder was 4 g / min, and the mass percentage of tantalum was 80%.

[0048] Adjust the laser beam spot size to 30mm 2 The spot is a flat-top spot with uniform energy distribution. The laser power is set to 14000W, the scanning speed is 500mm / min, the powder feeding gas flow rate is 8L / min, and the shielding gas flow rate is 10L / min.

[0049] Open the automatic powder feeder and turn on the laser. Under the action of the laser, the surface of the copper alloy melts to form a molten pool. At the same time, the metallic tantalum and copper-titanium-chromium-zirconium powders melt and then solidify, eventually forming a tantalum-copper cladding layer containing titanium element.

[0050] The formed tantalum-copper composite layer has a total of one layer with a thickness of 0.5 mm.

[0051] Tests show that the conductivity of the cladding layer is 10% IACS, and its ablation performance is more than 4 times that of chromium zirconium copper C18000 copper alloy. The cladding layer is intact and not cracked.

[0052] Example 3

[0053] The method for preparing a tantalum-copper composite layer by laser cladding on a copper alloy surface specifically comprises the following steps:

[0054] The copper alloy surface is pretreated to make the surface rougher so as to reduce the reflectivity of the copper alloy surface to the laser, thereby improving the energy utilization rate.

[0055] The laser beam is tilted 30 degrees (i.e., the angle between the laser beam along the scanning direction and the normal direction of the copper alloy surface is 30 degrees), and metallic tantalum with a particle size of 2-50μm and copper-titanium-chromium-zirconium powder containing titanium element with a particle size of 75-150μm are placed in different powder feeding hoppers respectively, wherein the mass percentage of the copper-titanium-chromium-zirconium powder is: 0.60% Cr, 0.06% Zr, 8.00% Ti and the remainder Cu.

[0056] The powder feeder was adjusted so that the powder feeding rate of metal tantalum was 12 g / min, the powder feeding rate of copper-titanium-chromium-zirconium powder was 8 g / min, and the mass percentage of tantalum was 60%.

[0057] Adjust the laser beam spot area to 40mm 2 The spot is a flat-top spot with uniform energy distribution. The laser power is set to 14000W, the scanning speed is 1000mm / min, the powder feeding gas flow rate is 10L / min, and the shielding gas flow rate is 15L / min.

[0058] Open the automatic powder feeder and turn on the laser. Under the action of the laser, the surface of the copper alloy melts to form a molten pool. At the same time, the metallic tantalum and copper-titanium-chromium-zirconium powders melt and then solidify, eventually forming a tantalum-copper composite layer containing titanium element.

[0059] Set the laser power to 12000W, turn on the automatic powder feeder, turn on the laser, and clad the second layer.

[0060] Set the laser power to 10000W, turn on the automatic powder feeder, turn on the laser, and clad the third layer.

[0061] Set the laser power to 8000W, turn on the automatic powder feeder, turn on the laser, and clad the fourth layer.

[0062] The formed tantalum-copper composite layer has a total of 4 layers with a thickness of 2.5 mm.

[0063] The test shows that the conductivity of the cladding layer is 30% IACS, and its ablation performance is more than 3 times that of Cr-Zr-Cu C18000 copper alloy. The cladding layer is intact and not cracked, and the tensile performance results are shown in Table 1.

[0064] Example 4

[0065] The method for preparing a tantalum-copper composite layer by laser cladding on a copper alloy surface specifically comprises the following steps:

[0066] The copper alloy surface is pretreated to make the surface rougher so as to reduce the reflectivity of the copper alloy surface to the laser, thereby improving the energy utilization rate.

[0067] The laser beam is tilted at 45 degrees (i.e., the angle between the laser beam scanning direction and the normal direction of the copper alloy surface is 45 degrees), and metal tantalum with a particle size of 2-50 μm and copper-titanium-chromium-zirconium powder containing titanium element with a particle size of 75-150 μm are placed in different powder feeding hoppers. The mass percentage of the copper-titanium-chromium-zirconium powder is: 0.68% Cr, 0.073% Zr, 8.00% Ti and the balance Cu.

[0068] The powder feeder was adjusted so that the powder feeding rate of metal tantalum was 2 g / min, the powder feeding rate of copper-titanium-chromium-zirconium powder was 18 g / min, and the mass percentage of tantalum was 10%.

[0069] Adjust the laser beam spot area to 50mm 2 The spot is a flat-top spot with uniform energy distribution. The laser power is set to 14000W, the scanning speed is set to 2000mm / min, the powder feeding gas flow rate is set to 12L / min, and the shielding gas flow rate is set to 25L / min.

[0070] Open the automatic powder feeder and turn on the laser. Under the action of the laser, the surface of the copper alloy melts to form a molten pool. At the same time, the metallic tantalum and copper-titanium-chromium-zirconium powders melt and then solidify, eventually forming a tantalum-copper composite layer containing titanium element.

[0071] Set the laser power to 12000W, turn on the automatic powder feeder, turn on the laser, and clad the second layer.

[0072] Set the laser power to 10000W, turn on the automatic powder feeder, turn on the laser, and clad the third layer.

[0073] Set the laser power to 8000W, turn on the automatic powder feeder, turn on the laser, and clad the fourth layer.

[0074] Set the laser power to 8000W, turn on the automatic powder feeder, turn on the laser, and clad the fifth layer.

[0075] Set the laser power to 8000W, turn on the automatic powder feeder, turn on the laser, and clad the sixth layer.

[0076] Set the laser power to 8000W, turn on the automatic powder feeder, turn on the laser, and clad the seventh layer.

[0077] The formed tantalum-copper composite layer has a total of 7 layers with a thickness of 5.0 mm.

[0078] Tests show that the conductivity of the cladding layer is 45% IACS, and its ablation performance is more than twice that of chromium zirconium copper C18000 copper alloy. The cladding layer is intact and crack-free, with a tensile strength and yield strength of 652MPa and 511MPa respectively, and an elongation of 15%.

[0079] Figure 2 (a) and (b) are respectively cross-sectional SEM images of the tantalum-copper composite layer without titanium added obtained in Example 1 and the cross-sectional SEM images of the tantalum-copper composite layer with titanium added obtained in Example 3. By comparison, it can be seen that the tantalum particles in the tantalum-copper composite layer without titanium added are not fully melted, while the tantalum particles in the tantalum-copper composite layer with titanium added are fully melted to form dendrites.

[0080] Figure 3 (a) and (b) are respectively the high-resolution transmission electron microscopy images of the cross section of the tantalum-copper composite layer without titanium added obtained in Example 1 and the high-resolution transmission electron microscopy images of the cross section of the tantalum-copper composite layer with titanium added obtained in Example 3. In the tantalum-copper composite layer without titanium added, tantalum and copper form a diffusion interface layer, and in the tantalum-copper composite layer with titanium added, tantalum and copper form a copper-titanium phase interface layer, which forms a semi-coherent structure with tantalum and copper, respectively, improving the distribution of tantalum and the interface bonding of tantalum-copper.

[0081] Table 1 shows the mechanical properties of the tantalum-copper composite layer (i.e., Ta-Cu-Ti) with titanium added obtained in Example 3 of the present invention. The tantalum-copper composite layer (i.e., Ta-Cu) without titanium added obtained in Example 1 had cracks in the cladding layer and no tensile data was obtained. The results show that after adding titanium, the elongation of the tantalum-copper composite layer reaches 10.5%, which is attributed to the full melting of the tantalum particles and the interface reaction layer of the copper-titanium phase forming a semi-coherent structure with both tantalum and copper, which greatly alleviates the stress concentration of the tantalum-copper composite layer during plastic deformation, and further changes the movement of dislocations, making it easier for dislocations to pass through the tantalum-copper interface, thereby improving the elongation.

[0082] Table 1 Mechanical properties of tantalum-copper composite layer

[0083] Tensile strength(MPa) Yield strength (MPa) Total elongation (%) Ta-Cu --- ---- --- Ta-Cu-Ti 765 591 10.5

[0084] The present invention can realize the preparation of a tantalum-copper composite layer. The tantalum-copper composite layer has a strong bonding force with a copper alloy substrate, and the composite layer itself has excellent mechanical properties. Tantalum has a high melting point and can greatly improve the ablation resistance of the copper alloy substrate.

[0085] Anything not described in detail in the above embodiments can be set with reference to the laser cladding process in the prior art to form a metal cladding layer (for example, the shielding gas can be commonly used N2, Ar, etc.). The above embodiments are only examples. For example, the powder feeding amount of the powder feeder can also be adjusted according to the mass ratio of the metal tantalum and copper alloy powders. The mass ratio of the metal tantalum and copper alloy powders can be set according to the different requirements of the conductivity, mechanical properties and ablation resistance of the tantalum-copper composite layer. In addition, in addition to being mixed and fed through a double powder hopper, the metal tantalum and copper alloy powders can also be pre-mixed and then fed through a single powder hopper.

[0086] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An anti-ablation composite layer material powder for forming an anti-ablation coating on the surface of a copper alloy, characterized in that: It also includes metal tantalum powder and copper-titanium-chromium-zirconium alloy powder, wherein the particle size of the tantalum particles is 2-50μm, and the particle size of the copper-titanium-chromium-zirconium alloy powder is 75-150μm; the copper-titanium-chromium-zirconium alloy powder is composed of the following elements in percentage by mass: 0.60-0.70% Cr, 0.060-0.075% Zr, 2.00-10.00% Ti and the remainder Cu; the mass percentage of the metal tantalum powder in the anti-ablation composite layer material powder is 10%-80%, and the mass percentage of the copper-titanium-chromium-zirconium alloy powder in the anti-ablation composite layer material powder is 20% to 90%.

2. A method for preparing an anti-ablation composite layer on the surface of a copper alloy, characterized in that: The following steps are involved: S1. Preparing an anti-ablation composite layer material powder for forming an anti-ablation coating on the surface of a copper alloy, comprising a metal tantalum powder and a copper-titanium-chromium-zirconium alloy powder, wherein the tantalum particles have a particle size of 2-50 μm, and the copper-titanium-chromium-zirconium alloy powder has a particle size of 75-150 μm; the copper-titanium-chromium-zirconium alloy powder is composed of the following elements in percentage by mass: 0.60-0.70% Cr, 0.060-0.075% Zr, 2.00-10.00% Ti and the remainder Cu; S2. Pre-treating the surface of the copper alloy substrate by laser roughening or sandblasting to roughen the surface to improve the laser absorption rate; S3. Based on the laser cladding process, the laser beam is obliquely incident on the surface of the copper alloy substrate obtained in step S2, and at the same time, the evenly mixed anti-ablation composite layer material powder is fed into the laser molten pool or spread on the surface of the copper alloy substrate by a powder feeding method, wherein the mass percentage of the metal tantalum single substance powder in the anti-ablation composite layer material powder is 10%-80%, and the mass percentage of the copper-titanium-chromium-zirconium alloy powder in the anti-ablation composite layer material powder is 20%-90%; then, a tantalum-copper composite layer is formed on the surface of the copper alloy substrate by a laser cladding process; the thickness of the obtained tantalum-copper composite layer is 0.5-5mm.

3. The preparation method according to claim 2, characterized in that: In step S3, the parameters used in the laser cladding process are as follows: the spot area of ​​the laser beam is set to 25 mm 2 -50 mm 2 , laser power is set to 8000W-14000W, scanning speed is set to 300mm / min-2000mm / min, powder feeding gas flow is set to 5L / min-12L / min and protective gas flow is set to 5L / min-25L / min; Preferably, the light spot is a light spot with Gaussian energy distribution; more preferably, the light spot is a flat-top light spot with uniform energy distribution.

4. The preparation method according to claim 2, characterized in that: In step S1, the metal tantalum powder and the copper-titanium-chromium-zirconium alloy powder are respectively placed in different powder hoppers of the double powder hopper, and the double powder hoppers are used to synchronously feed powder to achieve uniform mixing of the anti-ablation coating material powder and powder feeding in step S3.

5. The preparation method according to claim 2, characterized in that: In step S3, the angle between the laser beam in the laser scanning direction and the normal direction of the surface of the copper alloy substrate is 5-45 degrees to avoid damage to optical components caused by reflection of the laser beam.

6. An anti-ablation composite layer on the surface of a copper alloy obtained by the preparation method according to any one of claims 2 to 5.

Citation Information

Patent Citations

  • Shaped charge cover material with combustion function and preparation method thereof

    CN108080632A

  • Copper-based alloy powder material, preparation method and application of copper-based alloy powder material, cladding layer and preparation method of cladding layer

    CN113604718A

  • Copper alloy high-conductivity wear-resistant ablation-resistant coating and preparation method thereof

    CN114892167A

  • Parts for vacuum film deposition apparatus and vacuum film deposition apparatus using the parts