Preparation process of hydrolyzable and dispersible wet tissue
The hydrolyzable and rinsed wet tissues prepared with specific materials and processes solves the environmental pollution problem of ordinary wet tissues, achieves rapid decomposition and antibacterial properties, and is suitable for a variety of usage scenarios.
Patent Information
- Application Number
- CN202411214943.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
AI Technical Summary
Ordinary wet tissues are difficult to degrade, resulting in environmental pollution and water pollution problems.
Using conifer or broad-leaved wood, natural cotton fibers and viscose fibers, combined with water-soluble binders and antibacterial agents, hydrolyzable and flushable wet tissues through specific impregnation and drying processes to ensure rapid decomposition and degradation in water. .
It realizes the rapid decomposition of wet tissues in water and degradation in the natural environment, reduces environmental pollution, has antibacterial properties, is suitable for personal care and medical scenarios, and improves the comfort of use.
Smart Images

Figure CN118932767A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wet tissue preparation, in particular to a preparation process of hydrolyzable and flushable wet tissue. Background Art
[0002] Wet wipes are pre-moistened papers used for personal cleaning and hygiene. They are compactly packaged and easy to carry, suitable for daily and travel use. As people's living standards continue to improve, wet wipes are widely used in daily cleaning, personal care, baby care and other fields due to their convenience and hygiene.
[0003] However, ordinary wet wipes are mainly made of difficult-to-degrade synthetic fibers and chemical adhesives. If people discard them directly into the environment after use, it will cause serious environmental pollution problems. Especially after flushing them into the toilet, ordinary wet wipes are easy to accumulate in the sewer pipes, causing pipe blockage and treatment difficulties, which brings great pressure to the sewage treatment system and increases the pollution to water bodies and the environment. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a preparation process for hydrolyzable and flushable wet tissues, which solves the problem that ordinary wet tissues are difficult to degrade and may cause pollution to water bodies and the environment.
[0005] To achieve the above objectives, the present invention is implemented by the following technical scheme: A preparation process of a hydrolyzable and flushable wet tissue, comprising the following steps: S1: Material preparation: wood pulp fiber is selected from coniferous trees or broad-leaved trees, cotton fiber is selected from natural cotton fiber, regenerated cellulose fiber is selected from viscose fiber, water-soluble adhesive is selected from polyvinyl alcohol, wet strength enhancing agent is selected from cationic polymer-cationic starch, wetting agent is selected from glycerin or propylene glycol, and moisturizing agent is selected from aloe extract or urea; S2: Fiber pulp preparation: wood pulp fiber, cotton fiber and regenerated cellulose fiber are mixed in a certain proportion, added into water to make fiber pulp, and the fiber pulp is beaten into an appropriate concentration using a pulping machine. The fiber length should be controlled during the pulping process; S3: Fiber web forming, spraying the fiber slurry evenly onto the mesh of the web forming machine, and removing excess water by vacuum absorption or mechanical pressing; S4: adhesive coating, preparing a water-soluble adhesive into a solution of appropriate concentration, uniformly coating the solution on the fiber web by spraying or dipping, and then pressing the solution after coating; S5: Drying, sending the fiber web coated with the adhesive into a drying device for drying, using hot air drying, infrared drying or microwave drying; S6: impregnation treatment, mixing the wetting agent and the moisturizing agent in proportion to prepare an impregnation solution, impregnating the dried fiber web into the impregnation solution, taking the fiber web out of the impregnation solution, and removing excess liquid by squeezing.
[0006] Preferably, in step S1, the wood pulp fiber accounts for 50%-70%, the cotton fiber accounts for 20%-30%, and the regenerated cellulose fiber accounts for 10%-20%.
[0007] Preferably, in step S1, the water-soluble adhesive is added at 2%-5%, the wet strength enhancing agent is added at 0.5%-1.5%, the wetting agent is added at 1%-3%, and the moisturizing agent is added at 0.5%-2%.
[0008] Preferably, in the step S2, the fiber pulp concentration is 1%-3%, the beating time is 30-60 minutes, the fiber length is controlled to be 1-3 mm, the web thickness in the step S3 is 0.2-0.5 mm, the vacuum dehydration pressure is set to 0.1-0.3 MPa, the adhesive solution concentration in the step S4 is 5%-10%, the coating amount is 2-5 g / m², the drying temperature in the step S5 is 60-80°C, and the drying time is 10-20 minutes, in the step S6, the wetting agent is added at 2%-5%, the moisturizing agent is added at 1%-3%, the antibacterial agent is added at 0.2%-0.5%, the impregnation time is 1-3 minutes, and the pressing pressure is 0.1-0.2 MPa.
[0009] Preferably, in the step S5, after the drying step, a softening process is added, and the softener is selected from silicone oil emulsion or cationic softener, and the softener addition amount is 1%-2% of the total weight of the fiber. The softener is added to the water in proportion and stirred evenly, the dried fiber web is spread on the workbench, and the softener solution is evenly sprayed on the surface of the fiber web using a spraying device, and the spraying amount is controlled at 1-2g / m². The treated fiber web is gently flattened using a roller, and the flattened fiber web is sent to the drying device again for drying.
[0010] Preferably, in the step S6, an antibacterial agent is added during the impregnation of the wet tissue, and phenoxyethanol is selected as the antibacterial agent. The amount of the antibacterial agent added is 0.1%-0.3% of the total weight of the fiber.
[0011] Preferably, after step S6, the treated wet tissue substrate is cut into a desired size and shape, and the cut wet tissues are packaged in single or multiple pieces using biodegradable packaging materials.
[0012] Preferably, the cutting size is a rectangle of 15 cm x 20 cm, and the biodegradable packaging material is selected from polylactic acid, polyhydroxyalkanoate or starch-based plastic.
[0013] The present invention provides a preparation process of a hydrolyzable and flushable wet tissue, which has the following beneficial effects: 1. The wet tissue prepared by the present invention through the specific steps of material preparation, fiber pulp preparation, fiber web forming, adhesive coating, drying, and impregnation treatment has the properties of being hydrolyzable and flushable, so that the wet tissue can be quickly decomposed in water and degraded in the natural environment, thereby reducing the pollution to water bodies and the environment.
[0014] 2. The present invention adds an antibacterial agent when the wet wipes are impregnated, so that the antibacterial agent in the wet wipes can effectively inhibit the growth of bacteria and maintain the hygiene of the wipes. The wet wipes with antibacterial properties can reduce the risk of bacterial infection during use, thereby making the wet wipes suitable for personal care and medical scenarios and protecting the health of users.
[0015] 3. The present invention can enhance the comfort of wet wipes when used by adding a softening process after the drying step, making the wet wipes suitable for baby care, facial cleansing and other scenarios that require a gentle touch. The soft texture reduces friction and irritation to the skin and is suitable for users with sensitive skin, thereby achieving the effect of increasing the softness of the wet wipes and making them suitable for use by more people.
[0016] 4. The wet tissue prepared by the present invention through the specific steps of material preparation, fiber pulp preparation, fiber web forming, adhesive coating, drying, and impregnation treatment can be directly thrown into the toilet and flushed away, reducing pollution to the garbage can and the environment, being more hygienic and convenient, thereby achieving the effect of being convenient for users to use and handle. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The present invention is a flow chart of the preparation process of the hydrolyzable and flushable wet tissue. DETAILED DESCRIPTION
[0018] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] Embodiment 1: Please see attached Figure 1 The present invention provides a process for preparing a hydrolyzable and flushable wet tissue, comprising the following steps: S1: Material preparation: wood pulp fiber is selected from coniferous trees or broad-leaved trees, cotton fiber is selected from natural cotton fiber, regenerated cellulose fiber is selected from viscose fiber, water-soluble adhesive is selected from polyvinyl alcohol, wet strength enhancing agent is selected from cationic polymer-cationic starch, wetting agent is selected from glycerin or propylene glycol, and moisturizing agent is selected from aloe extract or urea; S2: Fiber pulp preparation: wood pulp fiber, cotton fiber and regenerated cellulose fiber are mixed in a certain proportion and added into water to make fiber pulp. The fiber pulp is beaten into an appropriate concentration using a pulping machine to ensure that the fibers are evenly dispersed. During the pulping, the fiber length should be controlled to make the fibers have an appropriate length. S3: Fiber web forming, spraying the fiber slurry evenly onto the mesh of the web forming machine, removing excess water by vacuum absorption or mechanical pressing to form a uniform fiber web; S4: Adhesive coating: preparing a water-soluble adhesive into a solution of appropriate concentration, uniformly coating the solution on the fiber web by spraying or dipping, and then pressing the solution after coating to allow the adhesive to fully penetrate into the fiber web; S5: Drying, sending the fiber web coated with the adhesive into a drying device for drying, using hot air drying, infrared drying or microwave drying to quickly evaporate the water in the fiber web to form a dry wet tissue substrate; S6: impregnation treatment, mixing the wetting agent, moisturizing agent and antibacterial agent in proportion to prepare an impregnation solution, impregnating the dried fiber web into the impregnation solution to allow it to fully absorb the effective ingredients in the impregnation solution, taking the fiber web out of the impregnation solution, and removing excess liquid by squeezing.
[0020] In step S1, wood pulp fiber accounts for 60%, cotton fiber accounts for 25%, and regenerated cellulose fiber accounts for 15%.
[0021] In step S1, 4% of water-soluble binder, 1% of wet strength enhancer, 2% of wetting agent and 1% of moisturizer were added.
[0022] In step S2, the fiber pulp concentration is 2%, the beating time is 45 minutes, the fiber length is controlled to be 2 mm, the web thickness in step S3 is 0.3 mm, the vacuum dehydration pressure is set to 0.2 MPa, the binder solution concentration in step S4 is 7%, the coating amount is 3 g / m², the drying temperature in step S5 is 70°C, the drying time is 15 minutes, and in step S6, the wetting agent is added by 2%, the moisturizing agent is added by 1%, the antibacterial agent is added by 0.2%, the impregnation time is 2 minutes, and the pressing pressure is 0.15 MPa.
[0023] In step S5, after the drying step, a softening process is added. The softener is selected from silicone oil emulsion or cationic softener. The softener addition amount is 1% of the total weight of the fiber. The softener is added to the water in proportion and stirred evenly to ensure that the softener is completely dissolved. The dried fiber web is spread flat on the workbench, and the softener solution is evenly sprayed on the surface of the fiber web using a spraying device. The spraying amount is controlled at 1g / m² so that the softener evenly covers the entire fiber web. The treated fiber web is gently flattened using a roller to allow the softener to penetrate evenly, and the flattened fiber web is sent to the drying device again for drying.
[0024] In step S6, an antibacterial agent is added during the impregnation of the wet tissue, and phenoxyethanol is selected as the antibacterial agent. The amount of the antibacterial agent added is 0.2% of the total weight of the fiber.
[0025] After step S6, the treated wet tissue substrate is cut into a desired size and shape, and the cut wet tissues are packaged in single or multiple pieces using biodegradable packaging materials.
[0026] Cut into rectangles of 15cmx20cm in size, and choose polylactic acid, polyhydroxyalkanoate or starch-based plastic as biodegradable packaging material.
[0027] Embodiment 2: Please refer to the attached Figure 1 The embodiment of the present invention provides a process for preparing a hydrolyzable and flushable wet tissue, comprising the following steps: S1: Material preparation: wood pulp fiber is selected from coniferous trees or broad-leaved trees, cotton fiber is selected from natural cotton fiber, regenerated cellulose fiber is selected from viscose fiber, water-soluble adhesive is selected from polyvinyl alcohol, wet strength enhancing agent is selected from cationic polymer-cationic starch, wetting agent is selected from glycerin or propylene glycol, and moisturizing agent is selected from aloe extract or urea; S2: Fiber pulp preparation: wood pulp fiber, cotton fiber and regenerated cellulose fiber are mixed in a certain proportion and added into water to make fiber pulp. The fiber pulp is beaten into an appropriate concentration using a pulping machine to ensure that the fibers are evenly dispersed. During the pulping, the fiber length should be controlled to make the fibers have an appropriate length. S3: Fiber web forming, spraying the fiber slurry evenly onto the mesh of the web forming machine, removing excess water by vacuum absorption or mechanical pressing to form a uniform fiber web; S4: Adhesive coating: preparing a water-soluble adhesive into a solution of appropriate concentration, uniformly coating the solution on the fiber web by spraying or dipping, and then pressing the solution after coating to allow the adhesive to fully penetrate into the fiber web; S5: Drying, sending the fiber web coated with the adhesive into a drying device for drying, using hot air drying, infrared drying or microwave drying to quickly evaporate the water in the fiber web to form a dry wet tissue substrate; S6: impregnation treatment, mixing the wetting agent, moisturizing agent and antibacterial agent in proportion to prepare an impregnation solution, impregnating the dried fiber web into the impregnation solution to allow it to fully absorb the effective ingredients in the impregnation solution, taking the fiber web out of the impregnation solution, and removing excess liquid by squeezing.
[0028] In step S1, wood pulp fiber accounts for 50%, cotton fiber accounts for 30%, and regenerated cellulose fiber accounts for 20%.
[0029] In step S1, 5% of water-soluble binder, 0.5% of wet strength enhancer, 3% of wetting agent and 2% of moisturizer were added.
[0030] In step S2, the fiber pulp concentration is 1.5%, the beating time is 50 minutes, the fiber length is controlled to be 1.5 mm, the web thickness in step S3 is 0.25 mm, the vacuum dehydration pressure is set to 0.25 MPa, the binder solution concentration in step S4 is 8%, the coating amount is 4 g / m², the drying temperature in step S5 is 75°C, the drying time is 12 minutes, and in step S6, the wetting agent is added by 3%, the moisturizing agent is added by 2%, the antibacterial agent is added by 0.3%, the impregnation time is 3 minutes, and the pressing pressure is 0.2 MPa.
[0031] In step S5, after the drying step, a softening process is added. The softener is selected from silicone oil emulsion or cationic softener. The softener addition amount is 1.5% of the total weight of the fiber. The softener is added to the water in proportion and stirred evenly to ensure that the softener is completely dissolved. The dried fiber web is spread flat on the workbench, and the softener solution is evenly sprayed on the surface of the fiber web using a spraying device. The spraying amount is controlled at 1.5g / m² so that the softener evenly covers the entire fiber web. The treated fiber web is gently flattened using a roller to allow the softener to penetrate evenly, and the flattened fiber web is sent to the drying device again for drying.
[0032] In step S6, an antibacterial agent is added during the impregnation of the wet tissue, and phenoxyethanol is selected as the antibacterial agent. The amount of the antibacterial agent added is 0.3% of the total weight of the fiber.
[0033] After step S6, the treated wet tissue substrate is cut into a desired size and shape, and the cut wet tissues are packaged in single or multiple pieces using biodegradable packaging materials.
[0034] Cut into rectangles of 15cmx20cm in size, and choose polylactic acid, polyhydroxyalkanoate or starch-based plastic as biodegradable packaging material.
[0035] Embodiment three: Please see attached Figure 1 The present invention provides a process for preparing a hydrolyzable and flushable wet tissue, comprising the following steps: S1: Material preparation: wood pulp fiber is selected from coniferous trees or broad-leaved trees, cotton fiber is selected from natural cotton fiber, regenerated cellulose fiber is selected from viscose fiber, water-soluble adhesive is selected from polyvinyl alcohol, wet strength enhancing agent is selected from cationic polymer-cationic starch, wetting agent is selected from glycerin or propylene glycol, and moisturizing agent is selected from aloe extract or urea; S2: Fiber pulp preparation: wood pulp fiber, cotton fiber and regenerated cellulose fiber are mixed in a certain proportion and added into water to make fiber pulp. The fiber pulp is beaten into an appropriate concentration using a pulping machine to ensure that the fibers are evenly dispersed. During the pulping, the fiber length should be controlled to make the fibers have an appropriate length. S3: Fiber web forming, spraying the fiber slurry evenly onto the mesh of the web forming machine, removing excess water by vacuum absorption or mechanical pressing to form a uniform fiber web; S4: Adhesive coating: preparing a water-soluble adhesive into a solution of appropriate concentration, uniformly coating the solution on the fiber web by spraying or dipping, and then pressing the solution after coating to allow the adhesive to fully penetrate into the fiber web; S5: Drying, sending the fiber web coated with the adhesive into a drying device for drying, using hot air drying, infrared drying or microwave drying to quickly evaporate the water in the fiber web to form a dry wet tissue substrate; S6: impregnation treatment, mixing the wetting agent, moisturizing agent and antibacterial agent in proportion to prepare an impregnation solution, impregnating the dried fiber web into the impregnation solution to allow it to fully absorb the effective ingredients in the impregnation solution, taking the fiber web out of the impregnation solution, and removing excess liquid by squeezing.
[0036] In step S1, wood pulp fiber accounts for 70%, cotton fiber accounts for 20%, and regenerated cellulose fiber accounts for 10%.
[0037] In step S1, 3% of water-soluble binder, 1.5% of wet strength enhancer, 1.5% of wetting agent and 1.5% of moisturizer were added.
[0038] In step S2, the fiber pulp concentration is 2.5%, the beating time is 40 minutes, the fiber length is controlled to be 2.5 mm, the web thickness in step S3 is 0.4 mm, the vacuum dehydration pressure is set to 0.3 MPa, the binder solution concentration in step S4 is 6%, the coating amount is 2 g / m², the drying temperature in step S5 is 65°C, the drying time is 18 minutes, and in step S6, the wetting agent is added at 1.5%, the moisturizing agent is added at 1.5%, the antibacterial agent is added at 0.1, the impregnation time is 2 minutes, and the pressing pressure is 0.18 MPa.
[0039] In step S5, after the drying step, a softening process is added. The softener is selected from silicone oil emulsion or cationic softener. The softener addition amount is 2% of the total weight of the fiber. The softener is added to the water in proportion and stirred evenly to ensure that the softener is completely dissolved. The dried fiber web is spread flat on the workbench, and the softener solution is evenly sprayed on the surface of the fiber web using a spraying device. The spraying amount is controlled at 2g / m² so that the softener evenly covers the entire fiber web. The treated fiber web is gently flattened using a roller to allow the softener to penetrate evenly, and the flattened fiber web is sent to the drying device again for drying.
[0040] In step S6, an antibacterial agent is added during the impregnation of the wet tissue, and phenoxyethanol is selected as the antibacterial agent. The amount of the antibacterial agent added is 0.1% of the total weight of the fiber.
[0041] After step S6, the treated wet tissue substrate is cut into a desired size and shape, and the cut wet tissues are packaged in single or multiple pieces using biodegradable packaging materials.
[0042] Cut into rectangles of 15cmx20cm in size, and choose polylactic acid, polyhydroxyalkanoate or starch-based plastic as biodegradable packaging material.
[0043] Table 1: Hydrolyzable and flushable properties of wet wipes in different embodiments property Example 1 Example 2 Example 3 Hydrolysis time 5-10 minutes 7-12 minutes 10-15 minutes Degradation rate high medium Slow Biodegradation time 30-60 days 45-75 days 60-90 days Dispersion speed fast medium Slow Particle size Small and uniform medium Larger Softness Softness 5N Softness 4N Softness 3N Antimicrobial Antibacterial rate ≥99% Antibacterial rate ≥99% Antibacterial rate ≥99% Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A process for preparing a hydrolyzable and flushable wet tissue, characterized in that: The following steps are involved: S1: Material preparation: wood pulp fiber is selected from coniferous trees or broad-leaved trees, cotton fiber is selected from natural cotton fiber, regenerated cellulose fiber is selected from viscose fiber, water-soluble adhesive is selected from polyvinyl alcohol, wet strength enhancing agent is selected from cationic polymer-cationic starch, wetting agent is selected from glycerin or propylene glycol, and moisturizing agent is selected from aloe extract or urea; S2: Fiber pulp preparation: wood pulp fiber, cotton fiber and regenerated cellulose fiber are mixed in a certain proportion, added into water to make fiber pulp, and the fiber pulp is beaten into an appropriate concentration using a pulping machine. The fiber length should be controlled during the pulping process; S3: Fiber web forming, spraying the fiber slurry evenly onto the mesh of the web forming machine, and removing excess water by vacuum absorption or mechanical pressing; S4: adhesive coating, preparing a water-soluble adhesive into a solution of appropriate concentration, uniformly coating the solution on the fiber web by spraying or dipping, and then pressing the solution after coating; S5: Drying, sending the fiber web coated with the adhesive into a drying device for drying, using hot air drying, infrared drying or microwave drying; S6: impregnation treatment, mixing the wetting agent and the moisturizing agent in proportion to prepare an impregnation solution, impregnating the dried fiber web into the impregnation solution, taking the fiber web out of the impregnation solution, and removing excess liquid by squeezing.
2. The process for preparing a hydrolyzable and flushable wet tissue according to claim 1, characterized in that: In the S1 step, the wood pulp fiber accounts for 50%-70%, the cotton fiber accounts for 20%-30%, and the regenerated cellulose fiber accounts for 10%-20%.
3. The process for preparing a hydrolyzable and flushable wet tissue according to claim 1, characterized in that: In the step S1, 2% to 5% of the water-soluble adhesive is added, 0.5% to 1.5% of the wet strength enhancing agent is added, 1% to 3% of the wetting agent is added, and 0.5% to 2% of the moisturizing agent is added.
4. The process for preparing a hydrolyzable and flushable wet tissue according to claim 1, characterized in that: In the step S2, the fiber pulp concentration is 1%-3%, the beating time is 30-60 minutes, and the fiber length is controlled to be 1-3 mm. In the step S3, the web thickness is 0.2-0.5 mm, and the vacuum dehydration pressure is set to 0.1-0.3 MPa. In the step S4, the adhesive solution concentration is 5%-10%, and the coating amount is 2-5 g / m². In the step S5, the drying temperature is 60-80°C, and the drying time is 10-20 minutes. In the step S6, 2%-5% of the wetting agent is added, 1%-3% of the moisturizing agent is added, the impregnation time is 1-3 minutes, and the pressing pressure is 0.1-0.2 MPa.
5. The process for preparing a hydrolyzable and flushable wet tissue according to claim 1, characterized in that: In the step S5, after the drying step, a softening process is added, and the softener is selected from silicone oil emulsion or cationic softener, and the softener addition amount is 1%-2% of the total weight of the fiber. The softener is added to the water in proportion and stirred evenly, and the dried fiber web is spread on the workbench, and the softener solution is evenly sprayed on the surface of the fiber web using a spraying device, and the spraying amount is controlled at 1-2g / m². The treated fiber web is gently flattened using a roller, and the flattened fiber web is sent to the drying device again for drying.
6. The process for preparing a hydrolyzable and flushable wet tissue according to claim 1, characterized in that: In the step S6, an antibacterial agent is added during the impregnation of the wet tissue, and phenoxyethanol is selected as the antibacterial agent. The amount of the antibacterial agent added is 0.1%-0.3% of the total weight of the fiber.
7. The process for preparing a hydrolyzable and flushable wet tissue according to claim 1, characterized in that: After the step S6, the treated wet tissue substrate is cut into a desired size and shape, and the cut wet tissues are packaged in single or multiple pieces using biodegradable packaging materials.
8. The process for preparing a hydrolyzable and flushable wet tissue according to claim 7, characterized in that: The cutting size is a rectangle of 15 cm x 20 cm, and the biodegradable packaging material is selected from polylactic acid, polyhydroxyalkanoate or starch-based plastic.
Citation Information
Patent Citations
Preparing technology of hydrolysable and dispersable wet tissue
CN107476102A
Plant fiber dispersible material and preparation method thereof
CN112411246A
Preparation method of wet curtain paper with high wet strength and high water absorption
CN116145468A
Natural antibacterial dispersible wet toilet paper and preparation method thereof
CN118563596A