Prussian blue / platinum composite nano-enzyme, preparation method thereof and application of Prussian blue / platinum composite nano-enzyme in antibacterial aspect
By preparing Prussian blue/platinum complex nanoenzymes, using their enzyme-like activities and photothermal properties, the killing problem of multidrug-resistant bacteria was solved, efficient inhibition of E. coli and Staphylococcus aureus was achieved, and alternative antibiotics were provided effective treatment options.
Patent Information
- Application Number
- CN202411026138.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
Existing antibiotics are ineffective against multidrug-resistant bacteria such as E. coli and Staphylococcus aureus, and there is an urgent need to develop alternative therapeutic drugs.
Prepare a Prussian blue/platinum composite nanoenzyme, combine with potassium chloroplatinate through silicon-based Prussian blue nanomaterial, add ascorbic acid to form a composite nanoenzyme powder, and use its enzyme-like activity to generate hydroxyl radicals and near-infrared lasers to cause Cell membrane proteins denaturate to kill bacteria.
It has achieved efficient killing of multidrug-resistant bacteria, has good peroxidase-like activity and photothermal performance, is stable, is suitable for biomedical applications, replaces traditional antibiotics, reduces drug dosage and avoids systemic side effects.
Smart Images

Figure CN118948889A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nanomaterials, and specifically relates to a Prussian blue / platinum composite nanoenzyme and a preparation method thereof and an application thereof in antibacterial aspects. Background Art
[0002] Serious infectious diseases caused by pathogenic bacteria, including pneumonia, endocarditis, sepsis, etc., have become one of the most difficult healthcare problems threatening public health. Several bacterial genera, the most common of which are Escherichia coli and Staphylococcus aureus, have developed multidrug resistance. Escherichia coli, a Gram-negative bacterium, is a representative indicator of antimicrobial resistance (AMR) of Gram-negative bacteria. Escherichia coli can cause gastrointestinal tract and urinary tract infections and other local tissue and organ infections. Staphylococcus aureus is a representative of Gram-positive bacteria. Under appropriate conditions, Staphylococcus aureus can produce enterotoxins and cause food poisoning. In order to combat pathogenic bacterial infections, in recent decades, people have invested a lot of energy in the research and development of various antibiotic-based drugs. However, the resistance of microorganisms to antibiotic treatment is becoming more and more serious, and there is an urgent need to develop alternative therapeutic drugs that are resistant to antibiotics.
[0003] The antimicrobial activity of metal particles has been well established, while nanotechnology has facilitated the successful synthesis of metal nanoparticles, making them potential antimicrobial agents. D-block metals called transition metals have unique electronic structures that make them multifunctional by changing the properties of specific molecules. These transition metals include platinum group metals (PGMs). They are a group of six transition d-block metallic elements that are clustered together in the periodic table. These PGMs are iridium, osmium, palladium, platinum, rhodium, and ruthenium. They are also known as platinum group, platinum compounds, platinum group, platinum group, platinum group, platinum group elements, or platinum group elements (PGE). Nowadays, metal nanoparticles made of metal ions such as gold, silver, platinum, and tantalum are widely used in catalysis and biomedical applications. Among them, platinum nanoparticles (PtNPs) have been intensively explored as efficient nanozymes due to their biocompatibility and excellent catalytic activity, which makes them potential candidates for antimicrobial agents.
[0004] Prussian blue (PB) is a common hexacyanoferrate, also known as ferric ferrocyanide, with a molecular formula of Fe4[Fe(CN)6]3. Its synthesis method is simple and has high biosafety. It has been approved by the US Food and Drug Administration as a clinical drug for the treatment of thallium poisoning. In addition, due to its mixed valence state of Fe atoms similar to Fe3O4, it has high peroxidase-like catalytic activity, which has aroused widespread research interest. In addition, PB has obvious absorption in the near-infrared light segment and has good photothermal conversion efficiency. Therefore, PB is also a good photothermal material based on its good photothermal properties.
[0005] Metal nanoparticles show significant bactericidal efficacy, and their synergistic antibacterial effects with multimetallic complexes may be of great significance. However, the use of Prussian blue (PB) and platinum metal to prepare composite nanozymes for antibacterial applications has not been reported, especially in inhibiting the growth of Escherichia coli and Staphylococcus aureus. Summary of the invention
[0006] The purpose of the present invention is to provide a Prussian blue / platinum composite nanozyme and a preparation method thereof and an application thereof in antibacterial aspects.
[0007] The technical solution adopted by the present invention to solve the technical problem is as follows:
[0008] The present invention provides a method for preparing a Prussian blue / platinum composite nanozyme, comprising the following steps:
[0009] First, a silicon-based Prussian blue nanomaterial solution and a potassium chloroplatinite solution were prepared, and then the potassium chloroplatinite solution was added dropwise into the silicon-based Prussian blue nanomaterial solution. Finally, ascorbic acid was added, and after standing, centrifugation, washing, and vacuum drying, a Prussian blue / platinum composite nanozyme powder was obtained.
[0010] Preferably, the mass ratio of the silicon-based Prussian blue nanomaterial, potassium chloroplatinite and ascorbic acid is 1:1:2.
[0011] Preferably, the preparation method of the silicon-based Prussian blue nanomaterial is as follows:
[0012] (1) Preparation of silica spheres: adding hexadecyltrimethylammonium bromide to water to obtain a mixed system, then placing the system in a water bath, and sequentially adding anhydrous ethanol, a NaOH solution, and ethyl orthosilicate to react to obtain silica spheres;
[0013] (2) Preparation of mesoporous silica modified with 3-aminopropyltriethoxysilane: The silica spheres obtained in step (1) are ultrasonically dispersed in anhydrous ethanol again, and 3-aminopropyltriethoxysilane is added at the same time. The obtained mixed reaction system is stirred overnight, and the next day, it is centrifuged and washed. Then, the collected precipitate is dispersed in anhydrous ethanol solution, and ammonium nitrate is added to condense and reflux to react, thereby obtaining a mesoporous silica nanomaterial modified with 3-aminopropyltriethoxysilane;
[0014] (3) Preparation of silicon-based Prussian blue nanomaterials: citric acid, potassium ferrocyanide K4[Fe(CN)6] and FeCl3·6H2O are mixed to obtain liquid A, and then a water bath is adjusted to 60° C., water and the mesoporous silica nanomaterial modified with APTES in step (2) are added, stirred to dissolve, citric acid is added and stirred, and liquid A is then added dropwise and stirred. After stirring, the mixture is transferred to room temperature and stirred to obtain silicon-based Prussian blue nanomaterials.
[0015] The present invention provides a Prussian blue / platinum composite nanozyme prepared by the above-mentioned method for preparing a Prussian blue / platinum composite nanozyme.
[0016] The present invention also provides an application of the Prussian blue / platinum composite nanozyme in antibacterial aspects.
[0017] Among them, the enzyme-like activity of the Prussian blue / platinum composite nanozyme can first generate highly toxic hydroxyl radicals to cause protein denaturation of the cell membrane, and then the Prussian blue / platinum composite nanozyme can be irradiated with near-infrared laser to generate heat to kill bacteria.
[0018] Preferably, the bacteria are Escherichia coli and Staphylococcus aureus.
[0019] The invention provides a Prussian blue / platinum composite nanozyme for antibacterial application, which mainly comprises the following steps:
[0020] Pick up the colony and add it to LB culture medium, shake and amplify overnight, and add physiological saline for dilution; after the Prussian blue / platinum composite nanozyme powder is configured into a solution, the diluted bacterial solution is added for shaking culture at 28-32°C, 170-190r / min, and shaken for 2-3h; the obtained solution is irradiated with a laser at a wavelength of 808nm for 4-6min; after dilution, it is spread on a plate and cultured at 35-40°C for 12-18h, the number of colonies is counted, and the colony mortality rate is calculated.
[0021] Preferably, the Prussian blue / platinum composite nanozyme powder is prepared into a solution with a concentration of 2-4 mg / mL using ultrapure water.
[0022] Preferably, after the Prussian blue / platinum composite nanozyme powder is configured into a solution, the diluted bacterial solution is added for shaking culture, wherein the volume ratio of the Prussian blue / platinum composite nanozyme powder solution to the diluted bacterial solution is 1:9.
[0023] The beneficial effects of the present invention are:
[0024] The present invention designs and synthesizes a Prussian blue / platinum composite nanozyme, which is based on silicon dioxide as the core. Through the modification of APTES, the silane group in the APTES molecule undergoes a condensation reaction with the hydroxyl group on the surface of silicon dioxide to form a covalent bond connection. At the same time, an amino functional group is introduced to the surface of mSiO2, which can improve its surface activity and enhance the adsorption capacity of metal ions. Next, PB NPs terminated with citric acid are used. Since the citric acid carboxyl groups on the surface of PB NPs are easily ionized to produce hydrogen ions with negative charges, and the surface of the mesoporous silica spheres after APTES modification is easily ionized to produce hydroxide ions with positive charges, PB NPs can be successfully combined on the surface of the spheres through the mutual attraction of positive and negative charges. Next, ascorbic acid is used as a reducing agent and potassium chloroplatinite is used as a precursor to deposit and grow a Pt layer on the surface of PB NPs to form a final Prussian blue / platinum composite nanozyme material.
[0025] Compared with traditional PB or Pt nanozyme materials, the Prussian blue / platinum composite nanozyme material prepared by the present invention has the advantages of high yield, good stability, good dispersibility in water and good peroxidase-like activity. At the same time, the Prussian blue / platinum composite nanozyme material prepared by the present invention has good photothermal performance and photothermal stability. It can first produce highly toxic hydroxyl radicals (·OH) through the enzyme-like activity of the Prussian blue / platinum composite nanozyme, causing protein denaturation of the cell membrane, and then irradiate the Prussian blue / platinum composite nanozyme with near-infrared laser to generate heat to kill bacteria. The good peroxidase-like activity, photothermal performance and photothermal stability of the Prussian blue / platinum composite nanozyme material can successfully resist the growth of bacteria, opening up a new path for biomedical applications.
[0026] The invention provides a method for preparing a Prussian blue / platinum composite nanozyme, which has the advantages of simple preparation process, economy, environmental protection, high yield, and greater convenience for industrial development.
[0027] The present invention uses a prepared Prussian blue / platinum composite nanozyme to construct an antibacterial method for laser irradiation nanozyme to generate heat therapy, further improves the catalytic activity of the Prussian blue / platinum composite nanozyme, and has a rapid and effective effect of killing bacteria compared with the use of nanocatalytic treatment alone. Its treatment method can resist bacterial infection through nanozyme-photothermal therapy, overcome drug resistance, reduce drug dosage, and avoid potential systemic side effects, so it can effectively replace antibiotics to fight bacteria. During the treatment process, firstly, the highly toxic hydroxyl radical (·OH) is produced by the enzyme-like activity of the nanozyme, causing protein denaturation of the cell membrane; secondly, by introducing near-infrared laser (NIR), the nanozyme can quickly convert light energy into heat energy, further causing the death of damaged bacteria, and effectively kill microorganisms through the above two effects. In summary, according to the current research and development status of antibacterial drugs, it is urgent to design and synthesize a highly efficient antibacterial nanomaterial, which will have very important practical significance and application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for the description of the embodiments. The illustrative embodiments and their descriptions of the application are used to explain the present invention and do not constitute improper limitations of the present invention. The embodiments of the present invention will now be described in detail with reference to the drawings:
[0029] Figure 1 Transmission electron microscopy image of Prussian blue / platinum composite nanozyme.
[0030] Figure 2 This is the EDS element mapping spectrum of Prussian blue / platinum composite nanozyme.
[0031] Figure 3 The surface potential of each substance in the preparation process of a Prussian blue / platinum composite nanozyme of the present invention. In the figure, 1: silica, 2: APTES-modified silica spheres, 3: APTES-modified mesoporous silica spheres, 4: APTES-modified mesoporous silica spheres connected to PB materials, 5: Prussian blue / platinum composite nanozyme.
[0032] Figure 4 The UV-visible absorption spectra of various substances in the preparation process of a Prussian blue / platinum composite nanozyme of the present invention are shown in the figure. In the figure, 1: APTES-modified mesoporous silica spheres, 2: APTES-modified mesoporous silica spheres connected to PB materials, 3: Prussian blue / platinum composite nanozyme.
[0033] Figure 5The UV-visible absorption spectra of the peroxidase activity of Prussian blue / platinum composite nanozymes at different concentrations. In the figure, 1: 2μg / mL, 2: 4μg / mL, 3: 6μg / mL, 4: 8μg / mL, 5: 10μg / mL, 6: 12μg / mL, 7: 14μg / mL, 8: 16μg / mL, 9: 20μg / mL.
[0034] Figure 6 To explore the effects of different pH and temperature on the peroxidase-like activity of Prussian blue / platinum composite nanozymes. In the figure, (a): pH, (b): temperature.
[0035] Figure 7 The Michaelis-Menten equation fitting curve (a) and the H2O2 enzyme activity double reciprocal curve (b) are shown when H2O2 is used as the substrate.
[0036] Figure 8 To explore the inhibitory effect of Prussian blue / platinum composite nanozymes on different bacteria under laser irradiation and the statistical graph of colonies. In the figure, (a): Escherichia coli, (b): Staphylococcus aureus, (c): Statistical graph of Escherichia coli colonies, (d): Statistical graph of Staphylococcus aureus colonies.
[0037] Fig. 9 To explore the heating curve of Prussian blue / platinum composite nanozyme under 808nm laser irradiation. DETAILED DESCRIPTION
[0038] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0039] Example 1 Preparation of Prussian blue / platinum composite nanozyme
[0040] This example synthesized a Prussian blue / platinum composite nanozyme, and the specific preparation method thereof is as follows:
[0041] (1) Preparation of silica spheres: 0.1 g of hexadecyltrimethylammonium bromide (CTAB) was weighed and added to a conical flask containing 20 ml of ultrapure water to obtain a mixed system, and the mixed system was ultrasonicated for 5 min until it was completely clear and transparent; then it was placed in a 70°C water bath for preheating for 15 min, and then 3 mL of anhydrous ethanol, 150 μL of NaOH solution (2 mol / L), and 200 μL of tetraethyl orthosilicate (TEOS) (added dropwise) were added in sequence, and then reacted at a constant speed of 850 rpm for 2 h; after the reaction was completed, it was cooled for 10 min; about 10 mL of anhydrous ethanol was added, and centrifuged at 9500 rpm for 15 min; 20 mL of anhydrous ethanol was added, vortexed, and centrifuged at 9500 rpm for 15 min, and the last centrifugation operation was repeated; finally, it was dispersed in 20 ml of ethanol to obtain silica spheres.
[0042] (2) Preparation of mesoporous silica spheres modified with 3-aminopropyltriethoxysilane (APTES): After centrifugation of the silica spheres obtained in step (1), the precipitate was collected and re-dispersed by ultrasonication into a conical flask containing 20 mL of anhydrous ethanol. At the same time, 200 μL of APTES was added to the conical flask. The obtained mixed reaction system was stirred overnight, i.e., the reaction time required ≥ 12 h. The next day, centrifugal washing was performed, referring to the operation in step (1). Next, the collected precipitate was dispersed into 50 mL of anhydrous ethanol solution, 0.3 g of ammonium nitrate was added, condensed and refluxed at 60 ° C for 10 h, and the centrifugal washing operation with ethanol was referred to the previous step (centrifugation twice). Finally, the supernatant was discarded after centrifugation, and resuspended in 10 mL of ultrapure water to obtain a mesoporous silica nanomaterial sample modified with APTES.
[0043] (3) Preparation of silicon-based Prussian blue nanomaterials: First, prepare liquid A, add a certain mass of 98 mg of citric acid, 8.45 mg of K4[Fe(CN)6] and 5.4 mg of FeCl3·6H2O into a conical flask containing 20 mL of ultrapure water, and ultrasonicate for 5 min until the system is completely clear and transparent to obtain liquid A for standby use; then, adjust the water bath to 60°C, place the conical flask containing 10 mL of ultrapure water into the water bath, then add 5 mL of the sample in step (2), stir at 850 rpm until completely dissolved, and then add 98 mg of citric acid. After continuous stirring for 2 minutes, liquid A was added dropwise into the above system at a constant speed of 5 mL / min during stirring. At this time, the system was in an acidic state, and the pH was measured to be around 3 using a pH test paper; after continuing to stir at 60°C and 850 rpm for 5 minutes, the mixture was transferred to room temperature and stirred for 5 minutes, cooled to room temperature, and finally centrifuged and washed. An equal volume of anhydrous ethanol was added to the above sample; the mixture was centrifuged at 9500 rpm for 15 minutes, the supernatant was discarded, and the precipitation nanoparticles were redispersed in 20 mL of distilled water by ultrasonic treatment, and centrifuged again by adding 20 ml of anhydrous ethanol. The purification process was repeated 3 times.
[0044] (4) Preparation of Prussian blue / platinum composite nanozyme powder, i.e., platinum is connected to silicon-based Prussian blue nanomaterials: the silicon-based Prussian blue nanomaterial solution obtained in step (2) is ultrasonicated for 8-10 minutes, dried overnight, and then quantified. The next day, the quantified sample solution is pipetted into a conical flask containing 10 mL of ultrapure water, and placed on a stirring table for stirring, the mass of the sample is calculated, and then liquid B is prepared, a certain volume of potassium chloroplatinite is dissolved in 10 mL of water for standby use. The ratio of potassium chloroplatinite to sample is 1:1, and then liquid B is added dropwise to the conical flask containing the sample with a pipette; finally, ascorbic acid is added, and the ratio of potassium chloroplatinite to sample to ascorbic acid is 1:1:2; the above sample is allowed to stand for 24 hours, and then centrifuged and washed, and the resulting precipitate is dried overnight in a vacuum drying oven, and Prussian blue / platinum composite nanozyme powder is successfully obtained.
[0045] The Prussian blue / platinum composite nanozyme obtained in this example was subjected to transmission electron microscopy analysis and EDS element mapping analysis. Figure 1 As shown in Figure 2, transmission electron microscopy shows that PB has been successfully anchored and embedded in the mesoporous silica spheres. Figure 2 As shown, the presence of various elements such as Fe and Pt in PB can be seen. The Prussian blue / platinum composite nanozyme finally obtained is a nanoscale particle with a diameter of 100-110nm. This nanoscale particle is spherical with an irregular surface and the overall size is relatively uniform.
[0046] In order to further confirm the successful synthesis of Prussian blue / platinum composite nanozymes, the surface potentials of silica, APTES-modified silica spheres, APTES-modified mesoporous silica spheres, APTES-modified mesoporous silica spheres connected to PB materials, and Prussian blue / platinum composite nanozymes were measured, as well as the UV-visible absorption spectra of APTES-modified mesoporous silica spheres, APTES-modified mesoporous silica spheres connected to PB materials, and Prussian blue / platinum composite nanozymes.
[0047] The surface potential measurement results of each substance are as follows Figure 3 As shown, from Figure 3 It can be seen (1: silica, 2: APTES-modified silica spheres, 3: APTES-modified mesoporous silica spheres, 4: APTES-modified mesoporous silica spheres connected to PB materials, 5: Prussian blue / platinum composite nanozymes) that with the progress of each step in the preparation process, the surface potential of the materials at each stage has changed accordingly, which once again proves that PB and Pt have been successfully anchored and embedded in the mesoporous silica spheres.
[0048] The UV-visible absorption spectra of each substance are shown in Figure 4 As shown, from Figure 4 It can be seen (in the figure, 1: APTES-modified mesoporous silica spheres, 2: APTES-modified mesoporous silica spheres connected to PB materials, 3: Prussian blue / platinum composite nanozymes), Prussian blue / platinum composite nanozymes and APTES-modified mesoporous silica spheres connected to PB materials have the same absorption peak (600-810nm), while APTES-modified mesoporous silica spheres do not have this peak. Combined with the above transmission electron microscopy, energy spectrum and potential results, it further proves that PB has been successfully anchored and embedded in the mesoporous silica spheres. Based on the analysis of all the above results, it is proved that the Prussian blue / platinum composite nanozyme has been successfully prepared.
[0049] Example 2 Establishment of a model for simulating peroxidase activity of Prussian blue / platinum composite nanozyme
[0050] The specific establishment process includes the following steps:
[0051] (1) Preparing a Prussian blue / platinum composite nanozyme suspension: Grind the Prussian blue / platinum composite nanozyme powder obtained in Example 1 and dissolve it in ultrapure water to a concentration of 200 μg / mL, then ultrasonically treat the suspension for 20-30 min to uniformly disperse it in the aqueous solution to obtain a blue nanozyme suspension;
[0052] (1) Prepare 100 mmol / L H2O2 aqueous solution and 10 mmol / L TMB anhydrous ethanol solution, which will be used for dilution at different times in the following tests;
[0053] (2) When the Prussian blue / platinum composite nanozyme was used as the reaction variable, the final concentration of the reaction system was 0.5 mmol / L TMB, 10 mmol / L H2O2, the concentration of the Prussian blue / platinum composite nanozyme material was 2, 4, 6, 8, 10, 12, 14, 16, 20 μg / mL, and NaAc-HAc (pH = 4) buffer was used to provide an acidic environment. After incubation at 37°C for 15 min, the absorption spectrum at 500-750 nm was measured using an enzyme reader;
[0054] (3) When H2O2 was used as the substrate, the final concentration of the reaction system was 0.5 mmol / L TMB, 20 μg / mL Prussian blue / platinum composite nanozyme, and the H2O2 concentration was 0.2, 0.5, 1, 2, 3, 4, 5, 10, 15, and 20 mmol / L. NaAc-HAc (pH = 4) buffer was used to provide an acidic environment. After incubation at 37°C for 30 min, the absorbance at 652 nm was measured using an enzyme reader.
[0055] Results Analysis,In order to explore the optimal concentration of Prussian blue / platinum composite nanozyme, Figure 5 It can be seen that only 20 μg / mL of Prussian blue / platinum composite nanozyme material showed the highest characteristic absorption peak at 652 nm, which has a higher peroxidase activity. In order to further explore the optimal conditions for the activity of the Prussian blue / platinum composite nanozyme material, Figure 6 It can be seen that the Prussian blue / platinum composite nanozyme material has a Figure 6 (a)), 37℃( Figure 6 Based on the above results and test steps, the Michaelis-Menten fitting curve of H2O2 enzyme was obtained under the optimal conditions ( Figure 7 (a)) and the H2O2 enzyme activity double reciprocal curve ( Figure 7 In (b), it is calculated that the Km of H2O2 enzyme is 0.79mmol / L, showing a strong binding force to the enzyme substrate, which is much better than the natural enzyme, and indirectly proves the high catalytic activity of the Prussian blue / platinum composite nanozyme material. Based on the above enzyme kinetics analysis, the Prussian blue / platinum composite nanozyme material prepared by the present invention has excellent peroxidase-like catalytic activity.
[0056] Example 3 Application of Prussian blue / platinum composite nanozyme in antibacterial effect
[0057] In Example 2, a model simulating peroxidase activity was successfully constructed using Prussian blue / platinum composite nanozyme. Based on this, the peroxidase activity and photothermal properties of the nanozyme were used to inhibit bacteria.
[0058] Because the Prussian blue / platinum composite nanozyme has excellent peroxidase-like activity, under acidic conditions, H2O2 will be catalytically decomposed to produce hydroxyl free radicals. At the same time, its good photothermal properties can emit heat to kill bacteria.
[0059] The antibacterial method of the Prussian blue / platinum composite nanozyme provided by the present invention is as follows:
[0060] 1. Shake the bacteria to amplify the bacterial solution density to 10 7 CFU / mL: Pick two colonies (Escherichia coli and Staphylococcus aureus), add 2mL LB medium respectively, and culture at 30℃ overnight. The OD value of the colony is about 1 on the second day. At this time, the colony density is 10 9 CFU / mL;
[0061] 2. Take 700 μL of the original bacterial solution in a 1 mL EP tube (operate in a clean bench), take 100 μL from the EP tube, add 900 μL of physiological saline (mass concentration of 0.9%, containing 1 g / L glucose), and dilute the bacterial solution to a density of 10 8 CFU / mL, take 4.5mL of the above saline and add 500μL of 10 8 CFU / mL bacterial solution was diluted to a density of 10 7 CFU / mL bacterial solution;
[0062] 3. Weigh the Prussian blue / platinum composite nanozyme powder prepared in Example 1 above, and prepare it into a 3 mg / mL solution with ultrapure water;
[0063] 4. Mixed incubation: The volume of the reaction system for antibacterial detection was 1 mL, in which the volume of the Prussian blue / platinum composite nanozyme sample solution added was 0 and 100 μL, and the volume of the physiological saline added was 100, 0, and 900 μL with a density of 10 7 CFU / mL of bacterial solution;
[0064] 5. Place in a shaker for incubation at 30°C, 180 r / min, and shake for 2 h;
[0065] 6. Then, take out the two EP tubes in 4 above, divide each 1 ml solution into two parts, one half is irradiated with 808 nm laser for 5 min (as the treatment group), and the other half is not treated (as the control group);
[0066] 7. Dilute the above 4 EP tubes with saline solution, dilute four gradients, and finally dilute 10 7 CFU / mL bacterial solution was diluted to a density of 10 3 CFU / mL, 100 μL was drawn from each EP tube for plating, and then the plate coated with E. coli was placed in a 37°C incubator for 12-15 h, while the plate coated with Staphylococcus aureus was placed in a 37°C incubator for 15-18 h.
[0067] 8. On the second day, observe the plate coated with colonies, count the number of colonies, and calculate the mortality rate (number of colonies in the treatment group / number of colonies in the control group).
[0068] Results analysis, such as Figure 8 As shown in (a), when the Prussian blue / platinum composite nanozyme was not added, the colony growth of Escherichia coli was almost unchanged under the conditions of no illumination (a)-1 and illumination (a)-2; while when the Prussian blue / platinum composite nanozyme was added, the colony growth of Escherichia coli was inhibited under the conditions of no illumination (a)-3 and illumination (a)-4, as shown in Figure 8As shown in (c)-2, the mortality rates were 70% and 2%, respectively. Figure 8 As shown in (b), when the Prussian blue / platinum composite nanozyme was not added, the colony growth of Staphylococcus aureus was almost unchanged under the conditions of no illumination (b)-1 and illumination (b)-2; while when the Prussian blue / platinum composite nanozyme was added, the colony growth of Staphylococcus aureus was inhibited under the conditions of no illumination (b)-3 and illumination (b)-4, as shown in Figure 8 As shown in (d)-2, the mortality rates are 31.26% and 5%, respectively. This shows that at a certain concentration, the Prussian blue / platinum composite nanozyme has a certain inhibitory effect, and the inhibitory effect is more obvious after laser irradiation.
[0069] In order to further verify the photothermal effect of Prussian blue / platinum composite nanozymes, different concentrations of Prussian blue / platinum composite nanozymes were used at 808 nm and a power density of 1.5 w / cm 2 The laser was irradiated for 5 minutes, and the temperature change was observed. The temperature change curve of the Prussian blue / platinum composite nanozyme solution with different concentrations was made. Fig. 9 As shown, with the increase of concentration and time, the temperature of the Prussian blue / platinum composite nanozyme solution continues to rise, and can reach a maximum of 54.1°C. This shows that the Prussian blue / platinum composite nanozyme has a good photothermal effect. Therefore, it can be applied to the actual detection of inhibiting bacterial growth, and has certain application value in related aspects of antibacterial.
[0070] The Prussian blue / platinum composite nanozyme successfully prepared by the present invention can be used for antibacterial detection. The Prussian blue / platinum composite nanozyme has good peroxidase-like activity. When H2O2 is used as a substrate, it can be seen from the Michaelis equation fitting curve that it conforms to the law of natural enzymes. The Prussian blue / platinum composite nanozyme also has a good photothermal effect. Under the irradiation of laser, it has a significant inhibitory effect on the growth of Escherichia coli and Staphylococcus aureus, which is dose-dependent.
[0071] The present invention discloses a Prussian blue / platinum composite nanozyme, a preparation method thereof, and an application thereof in antibacterial aspects. Those skilled in the art can refer to the contents of this article and appropriately improve the process parameters to achieve it. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all deemed to be included in the present invention. The products of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the products described herein without departing from the content, spirit and scope of the present invention to realize and apply the technology of the present invention.
Claims
1. A method for preparing a Prussian blue / platinum composite nanozyme, characterized in that: The following steps are involved: First, a silicon-based Prussian blue nanomaterial solution and a potassium chloroplatinite solution were prepared, and then the potassium chloroplatinite solution was added dropwise into the silicon-based Prussian blue nanomaterial solution. Finally, ascorbic acid was added, and after standing, centrifugation, washing, and vacuum drying, a Prussian blue / platinum composite nanozyme powder was obtained.
2. The method for preparing a Prussian blue / platinum composite nanozyme according to claim 1, characterized in that: The mass ratio of the silicon-based Prussian blue nanomaterial, potassium chloroplatinite and ascorbic acid is 1:1:
2.
3. The method for preparing a Prussian blue / platinum composite nanozyme according to claim 1, characterized in that: The preparation method of the silicon-based Prussian blue nanomaterial is as follows: (1) Preparation of silica spheres: adding hexadecyltrimethylammonium bromide to water to obtain a mixed system, then placing the system in a water bath, and sequentially adding anhydrous ethanol, a NaOH solution, and ethyl orthosilicate to react to obtain silica spheres; (2) Preparation of mesoporous silica modified with 3-aminopropyltriethoxysilane: The silica spheres obtained in step (1) are ultrasonically dispersed in anhydrous ethanol again, and 3-aminopropyltriethoxysilane is added at the same time. The obtained mixed reaction system is stirred overnight, and the next day, it is centrifuged and washed. Then, the collected precipitate is dispersed in anhydrous ethanol solution, and ammonium nitrate is added to condense and reflux to react, thereby obtaining a mesoporous silica nanomaterial modified with 3-aminopropyltriethoxysilane; (3) Preparation of silicon-based Prussian blue nanomaterials: citric acid, potassium ferrocyanide K4[Fe(CN)6] and FeCl3·6H2O are mixed to obtain liquid A, and then a water bath is adjusted to 60° C., water and the mesoporous silica nanomaterial modified with APTES in step (2) are added, stirred to dissolve, citric acid is added and stirred, and liquid A is then added dropwise and stirred. After stirring, the mixture is transferred to room temperature and stirred to obtain silicon-based Prussian blue nanomaterials.
4. A Prussian blue / platinum composite nanozyme prepared by the preparation method as described in any one of claims 1 to 3.
5. Use of a Prussian blue / platinum composite nanozyme as claimed in claim 4 in antibacterial aspects.
6. The use according to claim 5, characterized in that: First, the enzyme-like activity of the Prussian blue / platinum composite nanozyme generates highly toxic hydroxyl radicals to cause protein denaturation of the cell membrane, and then the Prussian blue / platinum composite nanozyme is irradiated with a near-infrared laser to generate heat to kill the bacteria.
7. The use according to claim 5, characterized in that: The bacteria are Escherichia coli and Staphylococcus aureus.
8. The use according to claim 5, characterized in that: The following steps are involved: Pick up the colony and add it to LB culture medium, shake and amplify overnight, and add physiological saline for dilution; after the Prussian blue / platinum composite nanozyme powder is configured into a solution, the diluted bacterial solution is added for shaking culture at 28-32°C, 170-190r / min, and shaken for 2-3h; the obtained solution is irradiated with a laser at a wavelength of 808nm for 4-6min; after dilution, it is spread on a plate and cultured at 35-40°C for 12-18h, the number of colonies is counted, and the colony mortality rate is calculated.
9. The use according to claim 8, characterized in that: The Prussian blue / platinum composite nanozyme powder was prepared into a solution with a concentration of 2-4 mg / mL using ultrapure water.
10. The use according to claim 8, characterized in that: After the Prussian blue / platinum composite nanozyme powder was prepared into a solution, the diluted bacterial solution was added for shaking culture, wherein the volume ratio of the Prussian blue / platinum composite nanozyme powder solution to the diluted bacterial solution was 1:9.