Carbon dioxide adsorbent, preparation method thereof and related device

By functionalizing the bimetal oxide with amine and coating and forming treatment, an efficient and stable carbon dioxide adsorbent was prepared, which solved the problem of CO2 adsorption in the closed space, and achieved efficient air purification and good stability.

CN118949912APending Publication Date: 2024-11-15CHINA CONSTR THIRD ENG BUREAU GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411173286.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

It is difficult to develop an efficient, stable and suitable carbon dioxide adsorbent in closed spaces for indoor air purification, especially in the case of low CO2 concentrations.

Method used

Coated molded amine functionalized bimetal oxide is prepared by providing bimetal oxide with a pore structure and amine functionalized treatment to form amine functionalized bimetal oxides, which are then coated on a support, and coated with a molded amine functionalized bimetal oxides, are prepared by providing bimetal oxides with pore structures and amine functionalized treatments, forming amine functionalized bimetal oxides, which are then coated onto a support. Adsorbent retains its high specific surface area and abundant pore structure.

Benefits of technology

It has achieved the ability to efficiently adsorb carbon dioxide at lower CO2 concentrations, has broad application prospects and market potential, can effectively reduce the CO2 concentration in the enclosed space, improve indoor air quality, and has good stability and renewability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949912A_ABST
    Figure CN118949912A_ABST
Patent Text Reader

Abstract

The invention relates to a carbon dioxide adsorbent, a preparation method thereof and a direct air trapping device for carbon dioxide. The preparation method comprises the following steps: providing a bimetallic oxide with a pore structure; carrying out amine functionalization treatment on the bimetallic oxide to obtain an amine-functionalized bimetallic oxide; the amine functionalized bimetallic oxide is coated on a carrier to obtain the carbon dioxide adsorbent, and the carbon dioxide adsorbent is the coating molded amine functionalized bimetallic oxide adsorbent. The coating forming amine functionalized bimetallic oxide adsorbent is formed through a coating forming process, so that the coating forming amine functionalized bimetallic oxide adsorbent can retain the morphological characteristics of high specific surface area, rich pore structure and the like of the amine functionalized bimetallic oxide; therefore, the efficient and stable formed carbon dioxide adsorbent capable of being used for purifying air in a closed space can be prepared, has wide application prospects and market potential, and is expected to bring innovative development to the field of indoor air purification.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of carbon capture technology, and in particular to a carbon dioxide adsorbent and a preparation method thereof, and related devices. Background Art

[0003] At present, direct air capture (DAC) is an emerging negative carbon technology that can separate and enrich CO2 in the atmosphere by adsorption or absorption. The capture efficiency and energy consumption of CO2 are directly related to the concentration of CO2 in the gas. Compared with the extremely dilute concentration of 400ppm CO2 in the atmosphere, the concentration of CO2 in buildings can range from 2000 to 10000ppm. Therefore, the driving force for capturing CO2 from buildings is higher and the energy consumption is lower. A study shows that the CO2 content in the ventilation system of buildings in Germany in 2020 accounted for 4% of its total annual carbon emissions. If this part of the carbon source is effectively utilized, the building can show huge negative carbon potential. At the same time, applying direct air capture technology to indoor CO2 removal can greatly reduce the required amount of fresh air and reduce the load on the air-conditioning system. According to the "Technical Standards for Residential Fresh Air Systems", the fresh air volume of the fresh air system is usually determined by the indoor CO2 content (produced by the human body). By applying a direct air capture device, the CO2 concentration can be reduced through capture by the device. At this time, the required fresh air volume is only a very small amount to supplement the oxygen and other components in the indoor air, thereby greatly reducing the additional air-conditioning energy consumption brought by the fresh air.

[0004] Therefore, it is necessary to develop a shaped CO2 adsorbent that is efficient, stable, and can be used for air purification in closed spaces. Summary of the invention

[0005] The purpose of this application is to provide a carbon dioxide adsorbent and a preparation method thereof, as well as a carbon dioxide direct air capture device, so as to prepare a shaped carbon dioxide adsorbent that is efficient, stable, and can be used for air purification in closed spaces. It has broad application prospects and market potential, and is expected to bring innovative development to the field of indoor air purification.

[0006] An embodiment of the present application provides a method for preparing a carbon dioxide adsorbent, which comprises: providing a bimetallic oxide, wherein the bimetallic oxide has a porous structure; performing amine functionalization treatment on the bimetallic oxide to obtain an amine functionalized bimetallic oxide; coating the amine functionalized bimetallic oxide on a carrier to obtain a carbon dioxide adsorbent, wherein the carbon dioxide adsorbent is a coated amine functionalized bimetallic oxide adsorbent.

[0007] Among them, the bimetallic oxide is subjected to amine functionalization treatment to obtain amine functionalized bimetallic oxide, including: adding bimetallic oxide, branched polyethyleneimine, and styrene-butadiene-styrene block copolymer into an organic solvent in a weight ratio and stirring and mixing them evenly to obtain a fourth solution including amine functionalized bimetallic oxide.

[0008] The amine-functionalized bimetallic oxide is coated on a carrier to obtain a carbon dioxide adsorbent, including: immersing the carrier in a fourth solution to coat it evenly, and then curing it to obtain a coated carrier; and drying the coated carrier until the organic solvent carried by the coated carrier is completely volatilized to obtain a carbon dioxide adsorbent.

[0009] The weight proportion of the styrene-butadiene-styrene block copolymer is 10-30%, and the weight proportion of the branched polyethyleneimine to the weight proportion of the bimetallic oxide is 1:1 or 2:1.

[0010] Wherein, the organic solvent is toluene, dichloromethane or styrene.

[0011] Wherein, providing a bimetallic oxide includes: preparing a first solution, a second solution and a third solution, wherein the first solution includes magnesium ions and aluminum ions, the second solution is a weak alkaline solution including carbonate ions, and the third solution is a strong alkaline solution including hydroxide ions; adding a pH adjuster to the second solution to adjust the pH value to a preset value, the preset value being 9 to 11; adding the first solution to the second solution, and simultaneously adding the third solution to the second solution to adjust the pH value to a preset value to obtain a mixed solution; aging the mixed solution at room temperature and with stirring to obtain an aged mixed solution; separating the aged mixed solution into a solid-liquid phase, and washing, drying and calcining the separated solid to obtain a bimetallic oxide, wherein the bimetallic oxide is a magnesium-aluminum bimetallic oxide.

[0012] The method comprises: filtering the aged mixed solution and washing the filtered solid with deionized water until the pH value is equal to 7, keeping the solid in a moist state during the washing process, and obtaining a neutral solid; washing the neutral solid with an organic solvent, keeping the neutral solid in a moist state during the washing process, and obtaining an initial sample, which is a layered double metal hydroxide; dispersing the initial sample in an organic solvent, stirring for a certain period of time at room temperature, filtering, and washing the filtered solid with an organic solvent to obtain a washed sample; vacuum drying the washed sample to obtain a dried sample; and calcining the dried sample under a protective gas atmosphere to obtain a bimetallic oxide.

[0013] Wherein, the carrier is a metal honeycomb carrier.

[0014] The embodiment of the present application also provides a carbon dioxide adsorbent, which is prepared by any of the above-mentioned methods for preparing the carbon dioxide adsorbent.

[0015] An embodiment of the present application also provides a carbon dioxide direct air capture device, which includes any of the above-mentioned carbon dioxide adsorbents.

[0016] The carbon dioxide adsorbent and its preparation method, as well as the carbon dioxide direct air capture device provided in the present application, are obtained by providing a bimetallic oxide having a porous structure, and subjecting the bimetallic oxide to amine functionalization treatment to obtain an amine-functionalized bimetallic oxide, and then coating the amine-functionalized bimetallic oxide on a carrier to obtain a carbon dioxide adsorbent. The carbon dioxide adsorbent is a coated and formed amine-functionalized bimetallic oxide adsorbent, thereby forming a coated and formed amine-functionalized bimetallic oxide adsorbent through a coating and molding process, so that the coated and formed amine-functionalized bimetallic oxide adsorbent can retain the morphological characteristics of the amine-functionalized bimetallic oxide, such as high specific surface area and rich pore structure. Therefore, an efficient and stable carbon dioxide adsorbent that can be used for air purification in closed spaces can be prepared, which has broad application prospects and market potential, and is expected to bring innovative development to the field of indoor air purification. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The technical solution and other beneficial effects of the present application will be made apparent by describing in detail the specific implementation methods of the present application in conjunction with the accompanying drawings.

[0018] Figure 1 It is a schematic flow chart of a method for preparing a carbon dioxide adsorbent provided in an embodiment of the present application;

[0019] Figure 2 This is a morphology diagram of the aluminum honeycomb panel before coating provided in the embodiment of the present application;

[0020] Figure 3 This is a morphology diagram of the aluminum honeycomb panel after coating provided in the embodiment of the present application;

[0021] Figure 4 It is a graph showing the change of carbon dioxide adsorption amount over time of two carbon dioxide adsorbents provided in the examples of the present application and a comparative sample. DETAILED DESCRIPTION

[0022] The present application is further described in detail below in conjunction with the accompanying drawings and examples. It is particularly noted that the following examples are only used to illustrate the present application, but are not intended to limit the scope of the present application. Similarly, the following examples are only some embodiments of the present application rather than all embodiments, and all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of this application.

[0023] In the following description of the present application, reference is made to “some embodiments”, which describe a subset of all possible embodiments, but it can be understood that “some embodiments” may be the same subset or different subsets of all possible embodiments and may be combined with each other without conflict.

[0024] In the following description of the present application, the terms "first\second\third" involved are merely used to distinguish similar objects and do not represent a specific ordering of the objects. It can be understood that "first\second\third" can be interchanged with a specific order or sequence where permitted, so that the embodiments of the present application described here can be implemented in an order other than that illustrated or described here.

[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein are only for the purpose of describing the embodiments of this application and are not intended to limit this application.

[0026] The following is a detailed description with reference to specific embodiments. It should be noted that the serial numbers of the following embodiments are not intended to limit the preferred order of the embodiments.

[0027] See also Figure 1 , Figure 1 : is a schematic diagram of a process for preparing a carbon dioxide adsorbent provided in an embodiment of the present application. The specific process of the method for preparing the carbon dioxide adsorbent may be as follows:

[0028] Step S11. Providing a bimetallic oxide, wherein the bimetallic oxide has a porous structure.

[0029] In this embodiment, the mixed metal oxide (MMO) includes at least two metals and can be a porous material, for example, a layered porous material, thereby ensuring that the bimetal oxide has a high specific surface area.

[0030] Specifically, the bimetallic oxide may include at least one divalent metal and at least one trivalent metal.

[0031] In some embodiments, the bimetallic oxide may specifically be a magnesium-aluminum bimetallic oxide, that is, a bimetallic oxide including divalent magnesium and trivalent aluminum.

[0032] Specifically, in the embodiment where the bimetallic oxide is a magnesium-aluminum bimetallic oxide, the step S11 may include:

[0033] Step S111. Prepare a first solution, a second solution and a third solution, wherein the first solution includes magnesium ions and aluminum ions, the second solution is a weak alkaline solution including carbonate ions, and the third solution is a strong alkaline solution including hydroxide ions.

[0034] The first solution may specifically contain aluminum ions (Al 3+ ) and magnesium ions (Mg 2+ ) aqueous solution. The second solution may have a pH value of 11 to 12 and contain carbonate ions (CO3 2- The third solution may be an aqueous solution having a pH value greater than 12 and containing hydroxide ions (OH - ) in an aqueous solution.

[0035] In some examples, the first solution may be specifically an aqueous solution of magnesium nitrate hexahydrate (Mg(NO3)2·6H2O) and aluminum nitrate nonahydrate (Al(NO3)3·9H2O), or may be specifically an aqueous solution of magnesium chloride hexahydrate (MgCl2·6H2O) and aluminum nitrate nonahydrate (Al(NO3)3·9H2O), and the concentration of magnesium nitrate hexahydrate or magnesium chloride hexahydrate in the first solution may be 0.55 mol / L, and the concentration of aluminum nitrate nonahydrate in the first solution may be 1 mol / L. The second solution may be specifically an aqueous solution of Na2CO3 with a concentration of 0.5 mol / L, and the volume of the second solution may be equal to the volume of the first solution. The third solution may be specifically an aqueous solution of sodium hydroxide with a concentration of 4 mol / L.

[0036] Step S112: Add a pH adjuster to the second solution to adjust the pH value to a preset value.

[0037] The preset value may be 9 to 11, for example, 9, 10 or 11. The pH adjuster may include at least one of ammonia water, sodium hydroxide, sodium bicarbonate, oxalic acid, phosphoric acid, nitric acid, hydrochloric acid and sulfuric acid, for example, dilute hydrochloric acid.

[0038] Specifically, the above step S112 may include: adding dilute hydrochloric acid to the second solution to adjust the pH value to 10. In this way, by adjusting the pH value of the second solution to a lower level, that is, weakening its alkalinity, the initial reaction rate of the subsequent precipitation reaction between the second solution and the first solution can be controlled to maintain it at a lower level, thereby facilitating the generation of a loose precipitate.

[0039] Step S113. Add the first solution to the second solution, and simultaneously add the third solution to the second solution to adjust the pH value to a preset value to obtain a mixed solution.

[0040] Specifically, the above step S113 may include: under normal temperature and stirring conditions, slowly adding the first solution to the second solution at a uniform speed, and simultaneously dropping the third solution into the second solution to adjust the pH value to a preset value, until the third solution is added, a mixed solution can be obtained. In this way, the pH value of the second solution and the first solution during the reaction process can be maintained at a preset value after the second solution is mixed with the first solution, that is, it is maintained weakly alkaline, thereby facilitating the second solution and the first solution to continue the precipitation reaction at a lower reaction rate.

[0041] Step S114: Aging the mixed solution at room temperature and with stirring to obtain an aged mixed solution.

[0042] Specifically, after obtaining the mixed solution, that is, after the third solution is added, the mixed solution can be stirred for a preset time at room temperature and under stirring conditions to achieve aging of the mixed solution, and an aged mixed solution can be obtained. Wherein, the preset time can be greater than or equal to 24h. In this way, by aging the mixed solution obtained by mixing the second solution with the first solution, it can be effectively ensured that the second solution can continue to react after mixing with the first solution, thereby extending the reaction time. This process is to ensure that under a specific environment where the pH value is a preset value (for example, 10), the double metal hydroxide crystals can grow slowly and orderly. In this way, the growth rate and conditions of the crystals can be effectively controlled to obtain an ideal crystal size to meet the specific needs of experiments or applications.

[0043] Step S115. Separate the aged mixed solution into solid-liquid form, and wash, dry and calcine the separated solid to obtain a bimetallic oxide, wherein the bimetallic oxide is a magnesium-aluminum bimetallic oxide.

[0044] Specifically, the above step S115 may include:

[0045] Step S1-1. Filter the aged mixed solution, and wash the filtered solid with deionized water until the pH value is equal to 7. Keep the solid in a wet state during the washing process to obtain a neutral solid.

[0046] Specifically, the solid obtained by filtration (ie, filter cake) can be washed with deionized water in a centrifuge until the filtrate is neutral, thereby obtaining a neutral solid.

[0047] Furthermore, it should be noted that the double hydroxide crystals (e.g., MgAl(OH)3CO3.H2O crystals) generated by the reaction of the second solution and the first solution will grow in an alkaline environment, and the deionized water washing used in this embodiment is to adjust the environment in which the double hydroxide crystals are located to a neutral pH, thereby stopping the growth of the double hydroxide crystals and obtaining the desired layered double hydroxide.

[0048] Step S1-2. Wash the neutral solid with an organic solvent, keep the neutral solid in a wet state during the washing process, and obtain an initial sample, which is a layered double metal hydroxide.

[0049] Specifically, the neutral solid can be washed with ethanol in a centrifuge, and the neutral solid is kept in a wet state during the washing process to obtain an initial sample.

[0050] Furthermore, it should be noted that the neutral solid is a layered double hydroxide, which has interlayer water at a microscopic scale, and the ethanol washing in this embodiment is to replace the interlayer water in the layered double hydroxide, so that a loose material with a high specific surface area and a high pore volume can be obtained after the ethanol finally evaporates. Moreover, the material is kept in a wet state during the washing process to avoid the problem that the interlayer water is converted into crystallization water after the material is dried, which leads to the problem that the water in the material cannot be replaced by washing with ethanol, which will cause the material to harden, which is not conducive to increasing the specific surface area and pore volume of the material.

[0051] In other embodiments, the ethanol used for washing the neutral solid can be replaced by other organic solvents, and the organic solvent can replace the interlayer water in the layered double metal hydroxide.

[0052] Step S1-3. The initial sample is dispersed in an organic solvent, stirred at room temperature for a certain period of time, filtered, and the filtered solid is washed with an organic solvent to obtain a washed sample.

[0053] Specifically, the initial sample can be dispersed in ethanol, stirred for a preset time at room temperature, filtered, and the filtered solid is washed with ethanol to obtain a washed sample. The preset time can be greater than or equal to 4 hours. In this way, by dispersing, filtering and washing the initial sample, other substances except the double metal hydroxide in the initial sample can be removed.

[0054] In other embodiments, the ethanol used to disperse the initial sample can be replaced by other organic solvents, as long as the organic solvent can effectively disperse the initial sample. In addition, the ethanol used to wash the filtered solid can also be replaced by other organic solvents, as long as the organic solvent can effectively wash the filtered solid.

[0055] Step S1-4. Vacuum-dry the washed sample to obtain a dried sample.

[0056] Specifically, the washed sample can be placed in a vacuum drying oven and vacuum dried at 60° C. for more than 12 hours to obtain a dried sample.

[0057] Step S1-5. Calcine the dried sample under a protective gas atmosphere to obtain a bimetallic oxide.

[0058] Specifically, the dried sample can be placed in a N2 protected atmosphere furnace and calcined at 400° C. for 5 h to obtain a magnesium aluminum bimetallic oxide.

[0059] Step S12: performing amine functionalization treatment on the bimetallic oxide to obtain an amine functionalized bimetallic oxide.

[0060] In this embodiment, the amine functionalization treatment of the bimetallic oxide may refer to: using a grafting agent to graft an organic amine into the pores of the bimetallic oxide. The amine functionalized bimetallic oxide is a bimetallic oxide grafted with an organic amine. The organic amine may be specifically a branched polyethyleneimine (Polyetherimide, PEI), and the grafting agent may be specifically a styrene-butadiene-styrene block copolymer (styrene-butadiene-styrene block copolymer, SBS).

[0061] It should be noted that organic amines have a strong adsorption capacity for carbon dioxide, and in this embodiment, by using a bimetallic oxide with a high specific surface area and pore volume as a carrier of the organic amine to achieve amine functionalization of the bimetallic oxide, the adsorption capacity for carbon dioxide can be further enhanced, thereby ensuring that the amine-functionalized bimetallic oxide has excellent CO2 adsorption performance and can achieve efficient adsorption at lower CO2 concentrations.

[0062] Specifically, the above step S12 may include: adding bimetallic oxide, branched polyethyleneimine, and styrene-butadiene-styrene block copolymer to an organic solvent in a weight ratio and stirring and mixing them evenly to obtain a fourth solution including amine-functionalized bimetallic oxide. Among them, styrene-butadiene-styrene block copolymer is used as a grafting agent to graft the branched polyethyleneimine into the pores of the bimetallic oxide to obtain the amine-functionalized bimetallic oxide.

[0063] Moreover, in a specific implementation, the bimetallic oxide, branched polyethyleneimine, and styrene-butadiene-styrene block copolymer can be added to an organic solvent in a weight ratio and stirred for 3 hours until a uniformly mixed solution is obtained. The uniformly mixed solution is the fourth solution including amine-functionalized bimetallic oxide.

[0064] The degree of polymerization of the branched polyethyleneimine may be 600. The organic solvent may be toluene, dichloromethane or styrene. In some examples, the organic solvent may be toluene, and the ratio of the mass of the organic solvent to the mass of the bimetallic oxide may be 6 to 8, for example, 6, 7 or 8.

[0065] In some examples, the weight ratio of the styrene-butadiene-styrene block copolymer is 10-30%, for example, 10%, 20% or 30%. In addition, the weight ratio of the branched polyethyleneimine to the weight ratio of the bimetallic oxide can be 1:1 or 2:1.

[0066] In some specific examples, the weight proportions of the styrene-butadiene-styrene block copolymer, the branched polyethyleneimine, and the bimetallic oxide may be 10%, 60%, and 30%, respectively, or may be 10%, 45%, or 45%, respectively.

[0067] Step S13: coating the amine-functionalized bimetallic oxide on the carrier to obtain a carbon dioxide adsorbent, wherein the carbon dioxide adsorbent is a coated amine-functionalized bimetallic oxide adsorbent.

[0068] The carrier may be a metal honeycomb carrier, for example, an aluminum honeycomb panel (such as Figure 2 It should be noted that, due to its unique structure and excellent thermal conductivity, the metal honeycomb carrier can effectively improve the adsorption efficiency and adsorption capacity of carbon dioxide by uniformly coating the amine-functionalized bimetallic oxide on the surface of the metal honeycomb carrier in this embodiment, thereby achieving more efficient carbon dioxide capture and separation.

[0069] Specifically, the above step S13 may include:

[0070] Step S131: immerse the carrier in the fourth solution to coat it evenly, and then solidify it to obtain a coated carrier.

[0071] Step S132: Dry the coated carrier until the organic solvent carried by the coated carrier is completely volatilized to obtain a coated amine-functionalized bimetallic oxide adsorbent.

[0072] Specifically, after obtaining the fourth solution including the amine-functionalized bimetallic oxide, the support (eg Figure 2 The carrier (as shown) is immersed in the fourth solution and coated evenly, and then the carrier coated evenly with the fourth solution is placed in a drying oven for heating and curing. The heating temperature is 60° C. and the heating time is 15 minutes to obtain a coated carrier (as shown). Figure 3Then, the coated carrier can be placed in a vacuum drying oven and vacuum dried at 70-110° C. for more than 12 hours until the organic solvent carried by the coated carrier is completely volatilized and removed, thereby obtaining a coated amine-functionalized bimetallic oxide adsorbent.

[0073] In addition, it should be noted that, compared with the prior art, the coated and formed amine-functionalized bimetallic oxide adsorbent provided in this embodiment has the following advantages: First, the amine-functionalized bimetallic oxide has a high specific surface area and a rich pore structure, so it has excellent CO2 adsorption performance and can achieve efficient adsorption at a lower CO2 concentration; secondly, through the coating and molding process, the coated and formed amine-functionalized bimetallic oxide adsorbent retains the high specific surface area and pore structure inherent in the amine-functionalized bimetallic oxide, thereby ensuring that the coated and formed amine-functionalized bimetallic oxide adsorbent also has a high specific surface area and a rich pore structure, and thus has efficient CO2 adsorption capacity, can be used for air purification in enclosed spaces (such as buildings), can effectively reduce the CO2 concentration in the enclosed space, and improve the indoor air quality; thirdly, the coated and formed amine-functionalized bimetallic oxide adsorbent has good stability and renewability, can be used for a long time, and reduces maintenance costs.

[0074] In some embodiments, before the above step S13, the preparation method of the above carbon dioxide adsorbent may further include: cleaning the carrier. Specifically, the carrier (e.g., aluminum honeycomb panel) may be immersed in ethanol for ultrasonic cleaning for 10 minutes to remove impurities on the surface of the carrier. In this way, when the subsequent process steps are performed, that is, when the amine-functionalized bimetallic oxide is coated on the carrier, the coating effect can be significantly improved, ensuring uniform coating and strong adhesion, which helps to improve the performance and reliability of the final product.

[0075] It is understood that all raw materials used in the examples of the present application can be obtained commercially. In addition, in the process of preparing the carbon dioxide adsorbent, by optimizing the process parameters of synthesizing the bimetallic oxide and optimizing the process parameters of coating the amine-functionalized bimetallic oxide, the adsorption performance and service life of the prepared carbon dioxide adsorbent can be further improved.

[0076] Furthermore, for ease of understanding, the present application is further described in detail below through two specific examples (ie, Example 1 and Example 2), and Comparative Example 1 is used as a comparison.

[0077] Example 1

[0078] In Example 1, the specific process of the preparation method of the carbon dioxide adsorbent can be as follows:

[0079] Step S21. Provide a bimetallic oxide with a porous structure, including: preparing an aqueous solution of magnesium nitrate hexahydrate (Mg(NO3)2·6H2O) and aluminum nitrate nonahydrate (Al(NO3)3·9H2O) to obtain a first solution, and the concentration of magnesium nitrate hexahydrate in the first solution is 0.55 mol / L, and the concentration of aluminum nitrate nonahydrate in the first solution is 1 mol / L; preparing an aqueous solution of Na2CO3 with a concentration of 0.5 mol / L to obtain a second solution, and the volume of the second solution is equal to the volume of the first solution; preparing an aqueous solution of sodium hydroxide with a concentration of 4 mol / L to obtain a third solution; adding dilute hydrochloric acid to the second solution to adjust the pH value to 10; adding the first solution to the second solution at a uniform speed and slowly under normal temperature and stirring, and simultaneously adding the third solution to the second solution to adjust the pH value to 10; The pH value is adjusted to 10 to obtain a mixed solution; the mixed solution is aged for 24 hours at room temperature and with stirring to obtain an aged mixed solution; the aged mixed solution is filtered, and the filtered solid is washed with deionized water until the pH value is equal to 7, and the solid is kept in a moist state during the washing process to obtain a neutral solid; the neutral solid is washed with ethanol, and the neutral solid is kept in a moist state during the washing process to obtain an initial sample; the initial sample is dispersed in ethanol, stirred at room temperature for 4 hours, filtered, and the filtered solid is washed with ethanol to obtain a washed sample; the washed sample is placed in a vacuum drying oven, and vacuum dried at 60°C for more than 12 hours to obtain a dried sample; the dried sample is placed in a N2 protected atmosphere furnace, and calcined at 400°C for 5 hours to obtain a bimetallic oxide, which is a magnesium-aluminum bimetallic oxide.

[0080] Step S22. Performing amine functionalization treatment on the bimetallic oxide to obtain amine functionalized bimetallic oxide, comprising: adding the bimetallic oxide, a branched polyethyleneimine having a degree of polymerization of 600, and a styrene-butadiene-styrene block copolymer to toluene in a weight ratio of 10% (styrene-butadiene-styrene block copolymer): 60% (branched polyethyleneimine): 30% (bimetallic oxide), and stirring for 3 hours until a uniformly mixed solution is obtained, wherein the uniformly mixed solution is the fourth solution comprising the amine functionalized bimetallic oxide, wherein the ratio of the mass of toluene to the mass of the bimetallic oxide is 6 to 8.

[0081] Step S23. coating the amine-functionalized bimetallic oxide on a carrier to obtain a carbon dioxide adsorbent, comprising: immersing an aluminum honeycomb panel as a carrier in ethanol for ultrasonic cleaning for 10 minutes to remove impurities on the surface of the carrier; immersing the aluminum honeycomb panel in a fourth solution to coat it evenly, and then placing the evenly coated aluminum honeycomb panel in a drying oven for heating and curing, the heating temperature is 60°C, and the heating time is 15 minutes, to obtain a coated carrier; placing the coated carrier in a vacuum drying oven, vacuum drying at 70-110°C for more than 12 hours, until the organic solvent carried by the coated carrier is completely volatilized and removed, to obtain carbon dioxide adsorbent A1, which is a coated and formed amine-functionalized bimetallic oxide adsorbent.

[0082] Example 2

[0083] The preparation method of the carbon dioxide adsorbent provided in Example 2 is basically the same as the preparation method of the carbon dioxide adsorbent provided in Example 1. The difference between the two is that the weight ratio of the branched polyethyleneimine and the bimetallic oxide used in the amine functionalization process of the bimetallic oxide in Example 2 is 45%, instead of 60% and 30% respectively. Accordingly, in Example 2, the specific process of the preparation method of the carbon dioxide adsorbent can be as follows:

[0084] Step S31. Step S21. Provide a bimetallic oxide with a porous structure, including: preparing an aqueous solution of magnesium nitrate hexahydrate (Mg(NO3)2·6H2O) and aluminum nitrate nonahydrate (Al(NO3)3·9H2O) to obtain a first solution, and the concentration of magnesium nitrate hexahydrate in the first solution is 0.55 mol / L, and the concentration of aluminum nitrate nonahydrate in the first solution is 1 mol / L; preparing an aqueous solution of Na2CO3 with a concentration of 0.5 mol / L to obtain a second solution, and the volume of the second solution is equal to the volume of the first solution; preparing an aqueous solution of sodium hydroxide with a concentration of 4 mol / L to obtain a third solution; adding dilute hydrochloric acid to the second solution to adjust the pH value to 10; slowly adding the first solution to the second solution at a uniform speed under normal temperature and stirring, and simultaneously dropping the third solution into the second solution; The solution is adjusted to a pH value of 10 to obtain a mixed solution; the mixed solution is aged for 24 hours at room temperature and with stirring to obtain an aged mixed solution; the aged mixed solution is filtered, and the filtered solid is washed with deionized water until the pH value is equal to 7, and the solid is kept in a moist state during the washing process to obtain a neutral solid; the neutral solid is washed with ethanol, and the neutral solid is kept in a moist state during the washing process to obtain an initial sample; the initial sample is dispersed in ethanol, stirred at room temperature for 4 hours, filtered, and the filtered solid is washed with ethanol to obtain a washed sample; the washed sample is placed in a vacuum drying oven, and vacuum dried at 60°C for more than 12 hours to obtain a dried sample; the dried sample is placed in a N2 protected atmosphere furnace, and calcined at 400°C for 5 hours to obtain a bimetallic oxide, which is a magnesium-aluminum bimetallic oxide.

[0085] Step S32. Performing amine functionalization treatment on the bimetallic oxide to obtain amine functionalized bimetallic oxide, comprising: adding the bimetallic oxide, a branched polyethyleneimine having a degree of polymerization of 600, and a styrene-butadiene-styrene block copolymer to toluene in a weight ratio of 10% (styrene-butadiene-styrene block copolymer): 45% (branched polyethyleneimine): 45% (bimetallic oxide), and stirring for 3 hours until a uniformly mixed solution is obtained, wherein the uniformly mixed solution is the fourth solution comprising the amine functionalized bimetallic oxide, wherein the ratio of the mass of toluene to the mass of the bimetallic oxide is 6 to 8.

[0086] Step S33. coating the amine-functionalized bimetallic oxide on the carrier to obtain a carbon dioxide adsorbent, comprising: immersing the aluminum honeycomb panel as the carrier in ethanol for ultrasonic cleaning for 10 minutes to remove impurities on the surface of the carrier; immersing the aluminum honeycomb panel in a fourth solution to coat it evenly, and then placing the evenly coated aluminum honeycomb panel in a drying oven for heating and curing, the heating temperature is 60°C, and the heating time is 15 minutes, so as to obtain a coated carrier; placing the coated carrier in a vacuum drying oven, vacuum drying at 70-110°C for more than 12 hours, until the organic solvent carried by the coated carrier is completely volatilized and removed, so as to obtain the carbon dioxide adsorbent A2, which is a coated and formed amine-functionalized bimetallic oxide adsorbent.

[0087] Comparative Example 1

[0088] In Comparative Example 1, the specific process of the preparation method of the carbon dioxide adsorbent can be as follows:

[0089] Step S41. Provide aluminum oxide (Al2O3), wherein the aluminum oxide is commercial gamma phase aluminum oxide.

[0090] Step S42. Performing amine functionalization treatment on alumina to obtain amine functionalized alumina, comprising: adding alumina, branched polyethyleneimine with a degree of polymerization of 600, and styrene-butadiene-styrene block copolymer to toluene in a weight ratio of 10% (styrene-butadiene-styrene block copolymer): 45% (branched polyethyleneimine): 45% (alumina), and stirring for 3 hours until a uniformly mixed solution is obtained, the uniformly mixed solution is the fourth solution including amine functionalized alumina, wherein the ratio of the mass of toluene to the mass of alumina is 6 to 8.

[0091] Step S43. coating the amine-functionalized alumina on a carrier to obtain a carbon dioxide adsorbent as a comparison sample, comprising: immersing the aluminum honeycomb panel as a carrier in ethanol for ultrasonic cleaning for 10 minutes to remove impurities on the surface of the carrier; immersing the aluminum honeycomb panel in a fourth solution to coat it evenly, and then placing the evenly coated aluminum honeycomb panel in a drying oven for heating and curing, the heating temperature is 60°C, and the heating time is 15 minutes, to obtain a coated carrier; placing the coated carrier in a vacuum drying oven, vacuum drying at 70-110°C for more than 12 hours, until the organic solvent carried by the coated carrier is completely volatilized and removed, to obtain a carbon dioxide adsorbent (i.e., a comparison sample), and the comparison sample is a coated and formed amine-functionalized alumina adsorbent.

[0092] Specifically, the carbon dioxide adsorbent A1 / A2 and the comparative sample obtained in the above-mentioned Example 1, Example 2 and Comparative Example 1 were subjected to dynamic adsorption test at 25°C and 400ppm CO2 concentration, and the performance parameter results of the carbon dioxide adsorbent A1 / A2 and the comparative sample were obtained as follows: Figure 4 As shown in Table 1 below.

[0093] Table 1

[0094]

[0095] Reference Figure 4 As shown in Table 1, by comparing the carbon dioxide adsorbents A1 / A2 obtained in Examples 1 and 2 with the control sample, it can be seen that the carbon dioxide adsorbents A1 / A2 obtained in Examples 1 and 2 have significant adsorption capacity and kinetic advantages over the control sample.

[0096] As can be seen from the above, the preparation method of the carbon dioxide adsorbent provided in this embodiment provides a bimetallic oxide, the bimetallic oxide has a porous structure, and performs amine functionalization treatment on the bimetallic oxide to obtain an amine functionalized bimetallic oxide, and then coats the amine functionalized bimetallic oxide on a carrier to obtain a carbon dioxide adsorbent. The carbon dioxide adsorbent is a coated and formed amine functionalized bimetallic oxide adsorbent, thereby forming a coated and formed amine functionalized bimetallic oxide adsorbent through a coating and molding process, so that the coated and formed amine functionalized bimetallic oxide adsorbent can retain the morphological characteristics of the amine functionalized bimetallic oxide, such as high specific surface area and rich pore structure, thereby preparing an efficient and stable carbon dioxide adsorbent that can be used for air purification in closed spaces, which has broad application prospects and market potential, and is expected to bring innovative development to the field of indoor air purification.

[0097] In order to better implement the preparation method of the carbon dioxide adsorbent provided in the embodiment of the present application, the embodiment of the present application further provides a carbon dioxide adsorbent, which is prepared by the preparation method of the carbon dioxide adsorbent provided in any of the above embodiments.

[0098] Specifically, the carbon dioxide adsorbent is a coated shaped amine-functionalized bimetallic oxide adsorbent, and specifically includes a carrier and an amine-functionalized bimetallic oxide coated on the carrier.

[0099] Compared with the prior art, the coated and formed amine-functionalized bimetallic oxide adsorbent provided in this embodiment has the following advantages: first, the amine-functionalized bimetallic oxide has a high specific surface area and a rich pore structure, so it has excellent CO2 adsorption performance and can achieve efficient adsorption at a lower CO2 concentration; second, through the coating and molding process, the coated and formed amine-functionalized bimetallic oxide adsorbent retains the high specific surface area and pore structure inherent in the amine-functionalized bimetallic oxide, thereby ensuring that the coated and formed amine-functionalized bimetallic oxide adsorbent also has a high specific surface area and a rich pore structure, and thus has efficient CO2 adsorption capacity, can be used for air purification in closed spaces (such as buildings), can effectively reduce the CO2 concentration in the closed space, and improve the indoor air quality; thirdly, the coated and formed amine-functionalized bimetallic oxide adsorbent has good stability and renewability, can be used for a long time, and reduces maintenance costs.

[0100] Furthermore, it should be noted that the carbon dioxide adsorbent in the embodiment of the present application is prepared by adopting the preparation method of the carbon dioxide adsorbent provided by any of the above embodiments, and therefore has all the same beneficial effects, which will not be described in detail in this embodiment.

[0101] An embodiment of the present application also provides a carbon dioxide direct air capture device, which includes the carbon dioxide adsorbent of any of the above embodiments.

[0102] The carbon dioxide adsorbent is a coated and formed amine-functionalized bimetallic oxide adsorbent, and specifically includes a carrier and an amine-functionalized bimetallic oxide coated on the carrier.

[0103] Specifically, the carbon dioxide direct air capture device can be applied to air purification in a closed space (e.g., a building). In addition, during specific implementation, the carbon dioxide adsorbent can adsorb CO2 in the air, and after the carbon dioxide adsorbent adsorbs CO2, the carbon dioxide adsorbent can be heated to a preset temperature (e.g., 50-100° C.) to release the adsorbed CO2, thereby achieving regeneration and reuse of the carbon dioxide adsorbent.

[0104] In some embodiments, the above-mentioned carbon dioxide direct air capture device can be an air purifier, and the carbon dioxide adsorbent contained therein can be used as a filter element in the air purifier.

[0105] It should be noted that the carbon dioxide direct air capture device provided in the embodiment of the present application, since it is equipped with the carbon dioxide adsorbent provided in the embodiment of the present application, can achieve the beneficial effects that can be achieved by any carbon dioxide adsorbent provided in the embodiment of the present application. Please see the previous embodiments for details, which will not be repeated here.

[0106] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0107] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a carbon dioxide adsorbent, characterized in that: include: Providing a bimetallic oxide, wherein the bimetallic oxide has a porous structure; Performing amine functionalization treatment on the bimetallic oxide to obtain an amine functionalized bimetallic oxide; The amine-functionalized bimetallic oxide is coated on a carrier to obtain a carbon dioxide adsorbent, wherein the carbon dioxide adsorbent is a coated and formed amine-functionalized bimetallic oxide adsorbent.

2. The preparation method according to claim 1, characterized in that: The step of subjecting the bimetallic oxide to amine functionalization to obtain an amine functionalized bimetallic oxide comprises: The bimetallic oxide, branched polyethyleneimine and styrene-butadiene-styrene block copolymer are added to an organic solvent in a weight ratio and stirred and mixed evenly to obtain a fourth solution including amine-functionalized bimetallic oxide.

3. The preparation method according to claim 2, characterized in that: The amine-functionalized bimetallic oxide is coated on a carrier to obtain a carbon dioxide adsorbent, comprising: Immersing the carrier in the fourth solution to coat it evenly, and then curing it to obtain a coated carrier; The coated carrier is dried until the organic solvent carried by the coated carrier is completely volatilized to obtain a carbon dioxide adsorbent.

4. The preparation method according to claim 2, characterized in that: The weight proportion of the styrene-butadiene-styrene block copolymer is 10-30%, and the weight proportion of the branched polyethyleneimine to the weight proportion of the bimetallic oxide is 1:1 or 2:

1.

5. The preparation method according to claim 2, characterized in that: The organic solvent is toluene, dichloromethane or styrene.

6. The preparation method according to claim 1, characterized in that: The bimetallic oxide provided comprises: Prepare a first solution, a second solution and a third solution, wherein the first solution includes magnesium ions and aluminum ions, the second solution is a weak alkaline solution including carbonate ions, and the third solution is a strong alkaline solution including hydroxide ions; Adding a pH adjuster to the second solution to adjust the pH value to a preset value, wherein the preset value is 9 to 11; adding the first solution to the second solution, and simultaneously adding the third solution to the second solution to adjust the pH value to the preset value, to obtain a mixed solution; Aging the mixed solution at room temperature and with stirring to obtain an aged mixed solution; The aged mixed solution is separated into solid and liquid, and the separated solid is washed, dried and calcined to obtain a bimetallic oxide, which is a magnesium-aluminum bimetallic oxide.

7. The preparation method according to claim 6, characterized in that: The aged mixed solution is separated into solid and liquid, and the separated solid is washed, dried and calcined to obtain a bimetallic oxide, comprising: Filtering the aged mixed solution, and washing the filtered solid with deionized water until the pH value is equal to 7, keeping the solid in a wet state during the washing process, to obtain a neutral solid; Washing the neutral solid with an organic solvent, keeping the neutral solid in a wet state during the washing process, to obtain an initial sample, wherein the initial sample is a layered double metal hydroxide; Dispersing the initial sample in an organic solvent, stirring for a certain period of time at room temperature, filtering, and washing the filtered solid with an organic solvent to obtain a washed sample; vacuum drying the washed sample to obtain a dried sample; The dried sample is calcined under a protective gas atmosphere to obtain a bimetallic oxide.

8. The preparation method according to claim 1, characterized in that: The carrier is a metal honeycomb carrier.

9. A carbon dioxide adsorbent, characterized in that: The method is prepared by the method according to any one of claims 1 to 8.

10. A carbon dioxide direct air capture device, characterized in that: Comprising the carbon dioxide adsorbent according to claim 9.